Device and method for repairing blade film holes by laser-assisted electric field driven spray deposition

Through laser-assisted electric field-driven jet deposition technology, the micro-melting pool is formed by using electric field-driven jet deposition printing equipment and lasers, which can accurately repair the air film holes of the turbine blades, and solve the problems of poor repair results and cumbersome processes in the existing technology. , achieving efficient and accurate repair results.

CN114850503BActive Publication Date: 2024-11-12QINGDAO UNIV OF TECH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210402765.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-18
Publication Date
2024-11-12
Estimated Expiration
2042-04-18

AI Technical Summary

Technical Problem

The prior art is difficult to effectively repair the air membrane hole of the turbine blade, especially the repair effect around the orifice is poor and the process is cumbersome, so the real repair effect cannot be achieved.

Method used

The laser-assisted electric field-driven jet deposition technology is used to print the slurry into a wire through the electric field-driven jet deposition printing equipment, and a micro-melting pool is formed at the air membrane hole of the blade, combining the remelted wire with the substances in the melt pool. Achieve accurate repair of worn parts.

Benefits of technology

It realizes efficient repair of corroded and damaged air membrane pores. The powder can be captured by micron-level micro-melting pools, with good forming quality and high forming efficiency, achieving ideal repair results, and solving the problem that traditional technology is difficult to achieve micro-scale repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114850503B_ABST
    Figure CN114850503B_ABST
Patent Text Reader

Abstract

The present invention provides an apparatus and method for repairing blade film holes by using laser-assisted electric field driven jet deposition, comprising: an electric field driven jet deposition printing device, comprising a flat electrode for placing an engine and a printing nozzle, wherein the printing nozzle is used to print slurry into a wire; a laser, which is used to remelt the wire and simultaneously form a molten pool at the position of the blade film hole to be repaired; in the present invention, the wire required for repair is produced by using an electric field driven jet deposition printing device, and then, under the action of the laser, the wire is remelted and simultaneously a micro molten pool is formed at the position of the blade film hole to be repaired, thereby realizing the combination of the wire and the material in the molten pool; the operation is simple, and the corroded and damaged air film holes can be repaired, and the remelted powder can be captured by the micron-level molten pool, with good forming quality and high forming efficiency, and accurate repair of worn parts can be realized to achieve an ideal effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of blade film hole repair, and in particular relates to a device and method for repairing blade film holes by laser-assisted electric field driven jet deposition. Background Art

[0002] As a strategic high-tech industry, the development level of the aviation manufacturing industry is a symbol of a country's comprehensive national strength, and it is also one of the important guarantees for national security and great power status. As the "heart" of an aircraft, the reliability of an aircraft engine is crucial to the normal operation of the aircraft. Among them, the surface accuracy and surface integrity of the turbine blade determine the service performance and service life of the aircraft, and it is listed as one of the core components in the manufacturing of aircraft engines. Due to the long-term exposure to harsh environments such as centrifugal loads, thermal stresses and corrosion, the microstructures of the film holes on the blades, such as the edges and tips of the blades, will suffer from cracks, wear, fracture damage and corrosion due to erosion corrosion and oxidation corrosion. If the height of the deposits near the outlet surface of the film hole increases, the cooling efficiency of the pore film downstream of the hole will be greatly reduced, thereby reducing the service life of the turbine blade. The cost of repairing the film holes of the blades is only about 10% of the manufacturing of the entire blade. Therefore, the research on the repair technology of the film holes of aircraft engine turbine blades is conducive to extending the service life of the blades, reducing manufacturing costs, and has huge economic benefits.

[0003] The inventor found that in order to solve the problem of repairing the air film holes of the blades, the Chinese patent with publication number CN113249728A discloses a method and device for repairing the hole wall defects of the air film holes. The invention mainly places a metal magnetic microneedle of a certain length in the air film hole and adds polishing liquid, and uses an electric motor to provide power to drive the rotating disk to drive the cylindrical container to rotate to remove the blocked impurities or remove the hole wall defects. However, the invention can only repair the inner side of the hole wall and cannot repair the periphery of the air film hole, and the repair effect is not good; Publication number CN2017112989 Chinese Patent No. 60 discloses a method for repairing air film holes after repair of damaged turbine blades. The invention uses ultrafast laser to repair the air film holes to be repaired, adopts rotary cutting and layer-by-layer scanning hole making method, performs circular rotary cutting to repair holes, removes excess coating, and then processes the air film holes to be repaired into air film holes that meet the requirements. However, large errors will occur during the operation of the invention, and the process requires layer-by-layer removal, the process is cumbersome, and the repair effect on the air film holes is not obvious. It only removes the coating that blocks the air film holes when repairing the blades, and does not achieve the purpose of truly repairing the air film holes. Summary of the invention

[0004] In order to solve the above problems, the present invention proposes a device and method for repairing blade air film holes by laser-assisted electric field driven jet deposition. The present invention is simple to operate, can repair the corroded and damaged air film holes, the powder can be captured by the micron-level molten pool, the forming quality is good, the forming efficiency is high, and the worn parts can be accurately repaired to achieve the ideal effect.

[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0006] In a first aspect, the present invention provides a device for repairing blade film holes by laser-assisted electric field driven spray deposition, comprising:

[0007] An electric field driven jet deposition printing device, comprising a flat plate electrode for placing an engine and a printing nozzle, wherein the printing nozzle is used to print a slurry into a filament;

[0008] The laser is used to remelt the wire and form a molten pool at the position of the blade film hole to be repaired; the remelted wire is combined with the material in the molten pool to repair the blade film hole.

[0009] Furthermore, the flat plate electrode is provided with a high voltage power supply.

[0010] Furthermore, the printing nozzle is communicated with the discharge port at the lowermost end of the printing nozzle and is located directly above the flat electrode, and the printing nozzle is perpendicular to the flat electrode.

[0011] Furthermore, the printing nozzle is connected to the XYZ three-axis motion platform via a connecting frame.

[0012] In a second aspect, the present invention further provides a method for repairing blade film holes by laser-assisted electric field driven spray deposition, which uses the device for repairing blade film holes by laser-assisted electric field driven spray deposition as described in the first aspect, comprising:

[0013] Using electric field driven jet deposition technology to print the slurry into filaments;

[0014] Under the irradiation of the laser beam, the wire is remelted, and a molten pool is formed at the position of the air film hole to be repaired on the blade;

[0015] The remelted wire is combined with the material in the molten pool to repair the air film holes on the blade.

[0016] Furthermore, when printing the slurry into a filament, a high voltage is applied to form an induced charge on the surface of the slurry droplet through self-induction. The repulsive force between the charges induces the formation of a cone jet to obtain a filament.

[0017] Furthermore, the high voltage is DC high voltage, pulse high voltage or AC high voltage; the DC high voltage range is 0KV~5KV; the pulse high voltage range is 0KV~±4KV, and the pulse frequency range is 0Hz~3000Hz; the AC high voltage range is 0KV~±4KV; and the nozzle movement speed is 0~20μm / s.

[0018] Furthermore, the laser parameters for emitting the laser beam are power: 0-1500W, spot diameter: 10-20μm, and scanning speed 10-30μm / s.

[0019] Furthermore, the slurry includes nickel-based high-temperature alloy metal powder and a binder.

[0020] Furthermore, the slurry includes nickel-based high-temperature alloy metal powder, nano-ceramic powder and a binder.

[0021] Furthermore, the high energy density of the laser beam vaporizes the binder in the wire and melts the metal powder; at the same time, the high energy density of the laser beam discharges the micropores inside the wire.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. In the present invention, the wire material required for repair is produced by an electric field-driven jet deposition printing device, and then, under the action of a laser, the wire material is remelted, and a micro-melting pool is formed at the position of the air film hole to be repaired in the blade, so that the wire material and the material in the micro-melting pool can be combined; the operation is simple, and the corroded and damaged air film hole can be repaired. The remelted powder can be captured by the micron-level micro-melting pool, and the forming quality is good and the forming efficiency is high, and the wear part can be accurately repaired to achieve the ideal effect;

[0024] 2. At present, the only laser additive manufacturing technology that can achieve repair is the laser stereo forming technology based on the technical characteristics of powder feeding. However, due to the influence of the powder convergence accuracy during the synchronous powder feeding process, the powder is difficult to be captured by the micron-level micro-melting pool, resulting in poor forming quality and low forming efficiency. In this embodiment, the powder is prepared into a slurry, and the electric field-driven jet deposition micro-nano 3D printing technology is used to prepare the "micro-filament", which is then repaired under the action of a laser beam to achieve precise repair of the worn parts. This method is simple to operate and can repair the corroded and damaged air film holes. The powder can be captured by the micron-level micro-melting pool, with good forming quality and high forming efficiency. It can also achieve precise repair of the worn parts to achieve the ideal effect, solving the problem that traditional laser repair is difficult to achieve microscale repair. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings in the specification that constitute a part of this embodiment are used to provide a further understanding of this embodiment. The schematic embodiments of this embodiment and their descriptions are used to explain this embodiment and do not constitute improper limitations on this embodiment.

[0026] Figure 1 This is a schematic diagram of the structure of Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0028] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0029] Terminology explanation:

[0030] Electric field driven jet deposition: a 3D printing technology based on self-excited electrostatic induction electric field driven micro-jet forming.

[0031] Air film holes on aircraft engine blades: These are circular holes with a certain arrangement pattern on the surface of aircraft engine turbine blades, which can form a layer of cooling air film on the surface of the turbine blades to cool the turbine blades.

[0032] Microfilament: It is a microstructure printed by electric field driven jet deposition, and its shape is filamentous.

[0033] Embodiment 1:

[0034] Film holes are circular holes with a certain arrangement pattern on the surface of turbine blades (with a diameter of 20μm-800μm). Their function is to extract cold air from the compressor to take away part of the heat inside the blades through enhanced convective heat exchange, and then flow out from the film holes on the blade body or end wall of the turbine blade. Due to the flow, the cold air will adhere to the wall surface to form a lower temperature cold air layer, thereby playing a good high-temperature isolation role and preventing the blades from being burned by high-temperature combustion gas, thereby achieving the effect of cooling the turbine blades. The cooling design of the film holes of turbine blades can reduce the thickness of the blade wall to reduce weight, use existing materials to reduce costs, increase the temperature before the turbine, thereby improving the thrust-to-weight ratio and extending the life of components.

[0035] In order to solve the problem of repairing film holes in aircraft engine blades, in this embodiment, a laser-assisted electric field driven jet deposition device for repairing film holes in blades is proposed, including an electric field driven jet deposition printing device and a laser;

[0036] The electric field driven jet deposition printing device comprises a flat plate electrode for placing an engine and a printing nozzle, wherein the printing nozzle is used to print the slurry into a filament;

[0037] The laser is used to remelt the wire and simultaneously form a micro-melting pool at the position where the air film hole of the blade is to be repaired; the remelted wire is combined with the material in the micro-melting pool to repair the air film hole of the blade.

[0038] The function of the electric field driven jet deposition printing device is to realize the forming of micron-scale "micro filaments" by using electric field driven jet deposition micro-nano 3D printing technology. The electric field driven jet deposition micro-nano 3D printing technology applies a high voltage between the nozzle and the substrate (or only applies a high voltage at the substrate, that is, a single potential), and forms an induced charge on the surface of the slurry droplet at the nozzle outlet through self-induction. The repulsive force between the charges induces the formation of a conical jet, thereby printing out "micro filaments" with a width of 10μm or even thinner. It should be noted that, in the present embodiment, the slurry may include nickel-based high-temperature alloy metal powder and a binder; the slurry is prepared by mixing metal powder and a binder according to a certain ratio, specifically, the ratio of nickel-based high-temperature alloy metal powder and the binder may be: nickel-based high-temperature alloy metal powder 65-80wt%, binder 8-25wt%, solvent 5-15wt%, and the nickel-based high-temperature alloy metal powder may be obtained in existing products; in other embodiments, the slurry may include nickel-based high-temperature alloy metal powder, nano-ceramic powder and a binder, and the ratio of nickel-based high-temperature alloy metal powder, nano-ceramic powder and binder may be: nickel-based high-temperature alloy metal powder 60-70wt%, ceramic powder 5-10%, binder 8-25wt%, and solvent 5-15wt%.

[0039] The role of the laser is to remelt the "micro-wire" formed by the electric field-driven jet deposition micro-nano 3D printing based on the laser stereo forming technology fed by the "micro-wire" under the irradiation of the laser beam; on the one hand, the high energy density of the laser will vaporize the binder in the micro-wire and melt the metal at the same time, and under the action of Marangoni convection, the micropores inside the micro-wire will be discharged to form a dense organization. On the other hand, the high energy density of the laser beam will form a micro-molten pool on the substrate, so that the "micro-wire" and the substrate are metallurgically bonded to meet the bonding strength requirements.

[0040] The main contents of this embodiment are as follows:

[0041] The electric field driven jet deposition printing device adopts a single flat electrode electric field driven multi-nozzle jet deposition micro-nano 3D printing device, including a print nozzle module, a print nozzle module of any material, a print substrate of any material, a flat electrode, a printing platform, a signal generator, a high voltage power supply, a feeding module, a precision back pressure control module, an XYZ three-axis precision motion platform, a positive pressure gas path system, an observation and positioning module, a UV curing module, a laser rangefinder, a base, a connecting frame, a first adjustable bracket, a second adjustable bracket and a third adjustable bracket, etc.;

[0042] The printing platform is fixed on the base, the flat electrode is located on the printing platform, the output end of the signal generator is connected to the high-voltage power supply, one end of the high-voltage power supply is connected to the flat electrode, and the other end is grounded; the printing substrate is located on the flat electrode, each printing nozzle in the printing nozzle module is connected to the discharge port at the bottom end of the corresponding printing nozzle in the printing nozzle module, and is located directly above the flat electrode, and each printing nozzle in the printing nozzle module is perpendicular to the flat electrode; each feeding module in the feeding module is connected to the lower half of the corresponding printing nozzle of the printing nozzle module The back pressure control module in the precision back pressure control module is connected to the top of the corresponding print head in the print head module, and the positive pressure air path system is connected to each back pressure control module in the precision back pressure control module; the print head module is connected to the XYZ three-axis precision motion platform through the connecting frame, the observation and positioning module is connected to the first adjustable bracket, and the first adjustable bracket is fixedly connected to the connecting frame; the laser rangefinder is connected to the second adjustable bracket, and the second adjustable bracket is fixedly connected to the connecting frame; the UV curing module is connected to the third adjustable bracket, and the third adjustable bracket is fixedly connected to the connecting frame.

[0043] The signal generator is used to output a variety of waveforms, with an output frequency of 0MHz to 1MHz, and can adjust the output peak voltage, bias voltage, frequency and duty cycle to achieve point or line printing as needed. Here, the high-voltage power supply is set to amplifier mode, and the signal generator is set to a frequency of 800Hz, a peak value of 7V, a bias voltage of 0V, and a duty cycle of 50%;

[0044] The observation and positioning module is used to observe and locate the position of the print head relative to the air film hole in the vertical direction, and an industrial camera or a high-resolution CCD camera can be used here;

[0045] The UV curing module is used to quickly cure the printed microfilaments, and an LED or a high-pressure mercury lamp can be used here;

[0046] The laser rangefinder is used to achieve accurate measurement of the printed micro-filaments and air film holes;

[0047] In this embodiment, the process parameter range of electric field driven jet deposition printing can be set as: the inner diameter size range of the printing nozzle is 0.1μm~300μm, the thickness range of the flat electrode is 0.5mm~30mm, the high voltage power supply can output DC high voltage, AC high voltage or pulse high voltage, the DC high voltage range is 0KV~5KV, the output pulse DC voltage range is 0KV~±4KV and is continuously adjustable, the output pulse frequency range is 0Hz~3000Hz and is continuously adjustable, the AC high voltage range is 0KV~±4KV, and the nozzle movement speed is 0~20μm / s.

[0048] Adjust the position of the turbine engine blades so that the nozzle is placed directly above the damaged and corroded air film holes on the turbine blades, and print "micro filaments" around the air film holes.

[0049] Using a solid-state laser, the cladding process parameter range can be set to: power: 0 ~ 1500W, spot diameter: 10-20μm, scanning speed 10 ~ 30μm / s.

[0050] Adjust the position of the laser, and the "micro-wire" formed by electric field-driven jet deposition micro-nano 3D printing will be remelted under the irradiation of the laser beam; the high energy density of the laser will vaporize the binder in the micro-wire and melt the metal at the same time, and under the action of Marangoni convection, the micropores inside the micro-wire will be discharged to form a dense tissue; in addition, the high energy density of the laser beam will form a micro-molten pool on the substrate, so that the "micro-wire" and the substrate are metallurgically bonded to meet the bonding strength requirements, thereby achieving a repair effect.

[0051] Embodiment 2:

[0052] This embodiment provides a method for repairing blade film holes by laser-assisted electric field driven spray deposition, which uses the device for repairing blade film holes by laser-assisted electric field driven spray deposition described in Embodiment 1, and includes:

[0053] Using electric field driven jet deposition technology to print the slurry into filaments;

[0054] Under the irradiation of the laser beam, the wire is remelted, and a micro-melting pool is formed at the position of the air film hole to be repaired on the blade;

[0055] The remelted wire is combined with the material in the micro-melting pool to repair the air film holes on the blade.

[0056] In this embodiment, when printing the slurry into a filament, a high voltage is applied to form an induced charge on the surface of the slurry droplet through self-induction, and the repulsive force between the charges induces the formation of a cone jet to obtain a filament.

[0057] In this embodiment, the high voltage is DC high voltage, pulse high voltage or AC high voltage; the DC high voltage range is 0KV~5KV; the pulse high voltage range is 0KV~±4KV, and the pulse frequency range is 0Hz~3000Hz; the AC high voltage range is 0KV~±4KV; the nozzle movement speed is 0~20μm / s.

[0058] In this embodiment, the laser parameters for emitting the laser beam are power: 0-1500W, spot diameter: 10-20 μm, and scanning speed: 10-30 μm / s.

[0059] In this embodiment, the slurry includes nickel-based high-temperature alloy metal powder and a binder.

[0060] In this embodiment, the slurry includes the nickel-based high-temperature alloy metal powder, nano-ceramic powder and a binder.

[0061] In this embodiment, the high energy density of the laser beam vaporizes the binder in the wire and melts the metal powder; at the same time, the high energy density of the laser beam discharges the micropores inside the wire.

[0062] Embodiment 3:

[0063] Different from Example 2, in this embodiment, the process parameters of electric field driven jet deposition 3D printing are selected: the inner diameter of the printing nozzle is 100μm, the nozzle moving speed is 20μm / s, and the DC high voltage is 2KV. After that, the position of the turbine engine blade is adjusted so that the nozzle is placed directly above the damaged and corroded air film hole of the turbine blade, and the "micro-wire" is printed around the air film hole. Then, a laser that outputs continuous laser is used, and the process parameters are: power 300W, spot diameter 2μm, and scanning speed 10μm / s. Adjust the position of the laser, and the "micro-wire" formed by electric field driven jet deposition micro-nano 3D printing will be remelted under the irradiation of the laser beam. The high energy density of the laser beam will form a micro-molten pool on the substrate, so that the "micro-wire" and the substrate are metallurgically bonded to meet the bonding strength requirements. Thereby achieving a repair effect.

[0064] Embodiment 4:

[0065] Different from Example 2 and Example 3, in this embodiment, the process parameters of electric field driven jet deposition 3D printing are selected: the inner diameter of the printing nozzle is 100μm, the nozzle moving speed is 20μm / s, and the DC high voltage is 2KV. After that, the position of the turbine engine blade is adjusted so that the nozzle is placed directly above the damaged and corroded air film hole of the turbine blade, and the "micro-wire" is printed around the air film hole. Then, a laser that outputs continuous laser is used, and the process parameters are: power 500W, spot diameter 2μm, and scanning speed 15μm / s. Adjust the position of the laser, and the "micro-wire" formed by electric field driven jet deposition micro-nano 3D printing will be remelted under the irradiation of the laser beam. The high energy density of the laser beam will form a micro-molten pool on the substrate, so that the "micro-wire" and the substrate are metallurgically bonded to meet the bonding strength requirements. Thereby achieving a repair effect.

[0066] The above description is only a preferred embodiment of the present embodiment and is not intended to limit the present embodiment. For those skilled in the art, the present embodiment may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present embodiment shall be included in the protection scope of the present embodiment.

Claims

1. A method for repairing blade air film holes by laser-assisted electric field driven jet deposition, a device for repairing blade air film holes by laser-assisted electric field driven jet deposition, the device include: An electric field driven jet deposition printing device, comprising a flat plate electrode for placing an engine and a printing nozzle, wherein the printing nozzle is used to print a slurry into a filament; A laser is used to remelt the wire and form a molten pool at the position of the blade film hole to be repaired; The remelted wire combines with the material in the molten pool to repair the air film holes on the blades; Characterized in that the method comprises: Using electric field driven jet deposition technology to print the slurry into filaments; Under the irradiation of the laser beam, the wire is remelted, and a molten pool is formed at the position of the air film hole to be repaired on the blade; The remelted wire combines with the material in the molten pool to repair the air film holes on the blades; The slurry includes nickel-based high-temperature alloy metal powder and a binder; Or, the slurry includes nickel-based high-temperature alloy metal powder, nano-ceramic powder and a binder; The powder is mixed into a slurry, and the micro-wire is prepared through electric field driven jet deposition micro-nano 3D printing technology, which is then repaired by laser under the action of a laser beam to achieve precise repair of worn parts; the width of the micro-wire is 10μm or less.

2. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 1, It is characterized in that The flat plate electrode is connected to a high voltage power supply.

3. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 1, It is characterized in that The printing nozzle is communicated with the discharge port at the lowermost end of the printing nozzle and is located directly above the flat electrode. The printing nozzle is perpendicular to the flat electrode.

4. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 1, It is characterized in that The printing nozzle is connected to the XYZ three-axis motion platform through a connecting frame.

5. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 1, It is characterized in that When printing the slurry into filaments, a high voltage is applied to form induced charges on the surface of the slurry droplets through self-induction. The repulsive force between the charges induces the formation of a cone jet to obtain the filament.

6. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 5, It is characterized in that The high voltage is DC high voltage, pulse high voltage or AC high voltage; the DC high voltage range is 0KV~5KV; the pulse high voltage range is 0KV~±4KV, and the pulse frequency range is 0Hz~3000Hz; the AC high voltage range is 0KV~±4KV; the nozzle movement speed is 0~20μm / s.

7. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 1, It is characterized in that The laser parameters for emitting the laser beam are power: 0-1500W, spot diameter: 10-20μm, and scanning speed 10-30μm / s.

8. The method for repairing blade film holes by laser-assisted electric field driven spray deposition as claimed in claim 1, It is characterized in that The high energy density of the laser beam vaporizes the binder in the wire and melts the metal powder; at the same time, the micropores inside the wire are discharged under the high energy density of the laser beam.