Application of perovskite LSCM materials in solid oxide electrolysis cells
By using the perovskite LaxSr1-xCr0.5Mn0.5O3-δ material as the fuel electrode in the solid oxide electrolytic cell, the problems of agglomeration and carbon deposition that are easily caused by traditional fuel electrodes under high temperature, high humidity and carbon dioxide are solved, and the realization of It improves the structural stability and carbon deposition resistance of the material, and significantly improves the long-term stability and electrolysis performance of the battery.
Patent Information
- Application Number
- CN202210549862.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-05-20
AI Technical Summary
Existing solid oxide electrolytic cell fuel electrode materials are prone to agglomeration, coarsening and carbon deposition of traditional cermet particles in the presence of high temperature, high humidity and carbon dioxide, affecting battery stability and efficiency.
The perovskite LaxSr1-xCr0.5Mn0.5O3-δ material is used as the co-electrolysis fuel electrode material of the solid oxide electrolytic cell, prepared by the sol-gel method or combustion method, and applied in the electrolytic cell through the screen printing method , ensuring that the material maintains structural stability and anti-carbon deposition properties in a redox atmosphere.
The perovskite LaxSr1-xCr0.5Mn0.5O3-δ material maintains a stable chemical composition in high temperature and high humidity environments, has good resistance to carbon deposition and catalytic activity, and significantly improves the long-term stability and stability of solid oxide electrolytic cells. The electrolysis performance is excellent especially under the mixed gas of carbon dioxide and water vapor.
Smart Images

Figure CN114855203B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid oxide electrolytic cells and relates to a perovskite-type La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ Application of (LSCM) materials in solid oxide electrolysis cells. Background Art
[0002] Solid oxide electrolysis cells (SOEC) have attracted widespread attention worldwide as a device that converts electrical energy into chemical energy continuously, efficiently and without capacity restrictions. Operating at high temperatures (700°C to 900°C), the efficiency of hydrogen production by electrolysis can be close to 100%, which is much higher than the more mature and gradually commercialized alkaline water electrolysis (AEC) and proton exchange membrane electrolysis cells (PEMEC). Among them, the co-electrolysis technology of the solid oxide electrolysis cell (SOEC) can not only achieve energy storage without capacity restrictions, but also convert water and carbon dioxide into fuel. The electrode material of the fuel electrode of the solid oxide electrolysis cell is the bottleneck of the co-electrolysis technology. The water vapor content in the fuel electrode (hydrogen electrode) of SOEC is significantly increased. At this time, the high temperature and high humidity environment of the fuel electrode easily causes the agglomeration and coarsening of the traditional metal ceramic fuel electrode particles, resulting in an increase in the polarization of the fuel electrode [Pihlatie, M; Kaiser, A.; Mogensen, M., et al. Electrical conductivity of Ni-YSZ composites; Degradation due to Ni particle growth [J]. Solid State lonics, 2011, 189 (1): 89-90]. Due to the presence of CO2, carbon deposition is very likely to occur in the fuel after electrolysis [Tao, Y,; Ebbesen, SD; Mogensen, MB Degradation of solid oxide cells during co-electrolysis of steam and carbon dioxide at high current densities [J]. Journal of Power Sources, 2016, 328: 452-462.]. In the process of searching for suitable SOEC co-electrolysis fuel electrode materials, perovskite oxides have attracted attention due to their good catalytic activity and anti-carbon deposition performance. Their general formula is ABO3.
[0003] Chinese patent CN 105130426 B uses a strontium titanate-based fuel electrode material with high-temperature chemical stability to replace the Ni-based metal ceramic fuel electrode material, but only improves the structural stability of the material itself at high temperature, and does not improve the ability of the fuel electrode material to prevent carbon deposition. Chinese patent CN 102731090 A discloses a La and Cr co-doped strontium titanate fuel electrode material, which has high ionic conductivity and can be directly used in hydrocarbon solid oxide fuel cells, but when strontium titanate is used as a matrix as a solid oxide electrolyzer fuel electrode material, the catalytic ability for carbon dioxide is relatively poor, and the polarization resistance is about 50Ω [Ma Zheng. Preparation and co-electrolysis performance of a new ceramic fuel electrode for solid oxide electrolyzer [D]. Nanjing: Nanjing University of Science and Technology, 2021: 63-64], which affects the long-term stability of the battery. Therefore, it is necessary to find a fuel electrode material with good stability in a reducing atmosphere and excellent anti-sulfur and anti-carbon deposition capabilities. Summary of the invention
[0004] The object of the present invention is to provide a perovskite type La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ Application of (LSCM) materials in solid oxide electrolysis cells.
[0005] Specifically, the perovskite La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The material is used as a co-electrolysis fuel electrode material in a solid oxide electrolysis cell.
[0006] The perovskite La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ Material, wherein 0.5≤x<1, and δ is the stoichiometric ratio of oxygen vacancies determined by the doping element and the atmosphere in which the material is located.
[0007] Preferably, x=0.75, the perovskite La 0.75 Sr 0.25 Cr 0.5 Mn 0.5 O 3-δ The material has the best stability and electrical performance when used as a fuel electrode material for co-electrolysis in a solid oxide electrolysis cell.
[0008] The perovskite La x Sr 1-x Cr 0.5Mn 0.5 O 3-δ The material is prepared by existing methods, such as any one or two of a solid phase method, a sol-gel method, and a combustion method.
[0009] The perovskite La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The specific application method of the material as a solid oxide electrolytic cell co-electrolysis fuel electrode material is: by screen printing, the perovskite type La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The material is printed on the electrolyte side of the oxygen electrode / electrolyte semi-electrolyzer, dried and calcined to form an electrolyzer.
[0010] The oxygen electrode of the present invention adopts oxygen electrode materials commonly used in the technical field, such as lanthanum strontium manganate.
[0011] Preferably, the coating thickness of the fuel electrode is 10 to 70 μm.
[0012] Compared with the prior art, the present invention has the following advantages:
[0013] (1) This invention is the first to convert the perovskite La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ As a fuel electrode of a solid oxide electrolytic cell, the material has a stable chemical composition in a redox atmosphere because it is an oxide. It can maintain structural stability in an oxidized or reduced state and in an electrolysis atmosphere of water vapor or carbon dioxide for a long time, and can perform co-electrolysis stably and efficiently for a long time.
[0014] (2) Perovskite-type La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The material has good catalytic activity for carbon dioxide, and the solid oxide fuel electrolyzer constructed shows obvious performance advantages and anti-carbon deposition characteristics when electrolyzing carbon dioxide or a mixed gas of carbon dioxide and water vapor. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 XRD patterns of LSCM powders prepared by different preparation methods;
[0016] Figure 2This is the SEM image of the interface between the fuel electrode and the electrolyte of the LSCM full cell;
[0017] Figure 3 The XRD patterns of LSCM powders after being treated in O2 and H2 at 800℃ for 10h respectively;
[0018] Figure 4 The curve of the conductivity of LSCM sample changing with temperature in air atmosphere;
[0019] Figure 5 The curves of conductivity variation with temperature of LSCM samples prepared by different preparation methods in air atmosphere;
[0020] Figure 6 The EIS curves of the LSCM electrolytic cell when different voltages were loaded in an atmosphere of 60% water vapor and 40% carbon dioxide;
[0021] Figure 7 Schematic diagram of the electrolysis process of carbon dioxide and water vapor on LSCM. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0023] The LSCM fuel electrode material described in the present invention is prepared by an existing method, such as one or two of a solid phase method, a sol-gel method, and a combustion method. Reference can be made to the existing literature [Sun Kening. Solid Oxide Fuel Cell [M]. Beijing: Science Press, 2019: pages 108-109], or Chinese patent application CN 113258086 A, or Chinese patent application CN113178587 A, or Chinese patent application CN 113782798 A.
[0024] Example 1
[0025] (1) Perovskite-type La 0.75 Sr 0.25 Cr 0.5 Mn0.5O 3-δ The material was prepared by the sol-gel method, and the specific steps are as follows:
[0026] Weigh the drugs according to the molar ratio of strontium: lanthanum: chromium: manganese = 1:3:2:2. First, add La(NO3)3·6H2O, Sr(NO3)2, Cr(NO3)3·H2O and Mn(NO3)2·4H2O to an aqueous solution of citric acid monohydrate (the molar ratio with metal ions is 1:1.5), stir in an oil bath at 80°C, adjust the solution pH to 6 with ammonia water during stirring, and stir continuously until the solution is clear. Continue stirring under the oil bath condition. The liquid will first become turbid, then slowly turn into a light yellow solution, and finally slowly stir in a water bath to become a sol, and then age to a gel with increasingly poor fluidity. At this time, take out the beaker and place it in a drying oven for drying at 150°C. The gel finally becomes a solid mixed with organic matter, and then is placed in a muffle furnace for calcination at 1000°C for 6h to remove the organic matter, and obtain LSCM powder.
[0027] Figure 1 is the XRD diagram of the prepared LSCM powder, indicating that the prepared LSCM powder corresponds to the standard peak of perovskite, and the XRD diagrams of LSCM powders prepared by solid phase method and combustion method are consistent with those of LSCM powders prepared by sol-gel method. Figure 2 This is the SEM image of the interface between the fuel electrode and the electrolyte of the LSCM full cell. It can be seen that the prepared LSCM powder material particles are small and uniform.
[0028] A small amount of LSCM powder was taken and treated in oxygen atmosphere and hydrogen atmosphere for 10 hours at 800℃, which simulates the operating temperature of the electrolytic cell. XRD analysis of the treated LSCM powder showed that the phase structure of the powder did not change significantly and no impurity phase was generated, proving that LSCM can maintain structural stability in the oxidation or reduction state for a long time and is a stable electrode material. Figure 3 shown.
[0029] (2) Take a small amount of the prepared LSCM powder sample and mix it with 2wt.% PVB binder, add an appropriate amount of anhydrous ethanol for granulation, grind the granulated powder in a mortar, take about 2g of powder and press it into a long strip test sample with a length, width and height of 20mm, 5mm and 2mm respectively, and place the sample in a box-type high-temperature sintering furnace for heat treatment at 1400℃ for 6h. The conductivity test needs to ensure the density of the sample. The density of the sample after sintering should be above 90%, so during the pressing process, it is necessary to ensure that there is no cracking and peeling on the surface of the strip sample. Then, the conductive silver paste and silver wire are bonded to the sintered body and placed in a tubular high-temperature sintering furnace for temperature rise test. The required test atmosphere is selected, the temperature is controlled by the tubular furnace, and the voltage and current at the corresponding temperature are measured by an electrochemical workstation. The temperature is kept at 50℃ for 15min, and the test temperature range of the sample is 300~800℃. Figure 4This is the curve of the conductivity of the LSCM sample in air atmosphere versus temperature. It can be seen from the figure that the conductivity of LSCM increases continuously with increasing temperature, and the conductivity is 16S / cm at 800℃. Figure 5 The curves of the conductivity of LSCM samples prepared by different preparation methods in air atmosphere vary with temperature. It can be seen that the conductivity of LSCM samples prepared by different preparation methods is slightly different, especially above 700°C; for the oxide fuel electrode, it has sufficient conductivity.
[0030] (3) Using LSCM as the fuel electrode material of SOEC, La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ (LSCF) is the oxygen electrode material, YSZ is used as the electrolyte, and the electrode material is brushed on both sides of the electrolyte by screen printing to assemble a single cell, and the thickness of the electrode layer is 30μm. A mixture of H2O and CO2 is continuously introduced into the fuel electrode at a flow rate of 30ml / min, and the fuel electrode is in a static air atmosphere. The ohmic resistance and interfacial polarization resistance of the electrolytic cell at different voltages can be obtained from the intercepts of the low-frequency and high-frequency bands on the real axis of the impedance spectrum with the x-axis. At a lower voltage, the gas encounters great resistance when it is transmitted to the three-phase interface of electrode-electrolyte-gas. At this time, most of the energy of the electric work is not converted into chemical energy, which is manifested as an increase in polarization resistance. At this time, a large amount of Joule heat is generated in the process of the current flowing through the electrolyte and the electrode to generate a voltage drop on the resistor, and the difficulty in converting the electric work into chemical energy makes the ohmic resistance higher than that in the open circuit case. As the voltage increases to about 1.5V and 2V, the polarization resistance decreases significantly. At this time, the electrolysis process occurs rapidly, the electrical work is quickly converted into chemical energy, and the gas reacts and digests quickly inside the battery. During the voltage rise process, the electrolytic cell continues to release heat, causing the temperature to rise, which promotes the step-by-step reduction of the ohmic resistance. In the atmosphere of 60% H2O + 40% CO2, the current density of the electrolytic cell reaches 0.21A·cm when the voltage is loaded at 2V. 2 , polarization resistance is about 1.80Ω·cm 2 ,like Figure 6 As shown in the figure, compared with the metal ceramic fuel electrode of the electrolyte-supported SOEC, it has better initial performance and stability. And for the co-electrolysis process, the high-frequency polarization resistance is not greatly affected at different ratios, while the increase in the overall polarization resistance of the electrolytic cell is due to the increase in the low-frequency polarization resistance as the water vapor concentration increases. The high-concentration water vapor atmosphere will affect the material transfer process of the electrolytic cell. On the LSCM fuel electrode, the electrode process of the co-electrolysis of carbon dioxide and water vapor is shown in the figure. Figure 7 As shown. Under the actual electrolysis voltage, the performance of the electrolysis reaction is very small when the ratio of carbon dioxide to water vapor is different. x Sr1-x Cr 0.5 Mn 0.5 O 3-δ The material exhibits excellent resistance to carbon deposition.
Claims
1. Perovskite La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The application of the material in a solid oxide electrolytic cell is characterized in that: Step 1: Preparation of perovskite La by sol-gel method x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ Material: Weigh the drugs according to the molar ratio of strontium: lanthanum: chromium: manganese = 1:3:2:
2. First, add La(NO3)3·6H2O, Sr(NO3)2, Cr(NO3)3·H2O and Mn(NO3)2·4H2O to the aqueous solution of citric acid monohydrate. The molar ratio of citric acid monohydrate to metal ions is 1:1.
5. Stir in an oil bath at 80°C. Adjust the solution pH to 6 with ammonia water during stirring. Stir continuously until the solution is clear. Continue stirring under oil bath conditions. The liquid is turbid at first, then slowly turns into a light yellow solution. Finally, slowly stir in a water bath to turn into a sol, and then age to a gel with increasingly poor fluidity. At this time, take out the beaker and place it in a drying oven for drying at 150°C. The gel finally turns into a solid mixed with organic matter, which is then placed in a muffle furnace for calcination at 1000°C for 6h to remove the organic matter to obtain perovskite-type La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ Material, where x = 0.75, δ is the stoichiometric ratio of oxygen vacancies determined by the doping element and the atmosphere in which the material is located; Step 2: The perovskite La prepared in step 1 x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The material is used as a co-electrolysis fuel electrode material in a solid oxide electrolysis cell, and the electrolysis atmosphere is a mixed gas of carbon dioxide and water vapor.
2. The use according to claim 1, characterized in that: The specific application method is: by screen printing, the perovskite type La x Sr 1-x Cr 0.5 Mn 0.5 O 3-δ The material is printed on the electrolyte side of the oxygen electrode / electrolyte semi-electrolyzer, dried and calcined to form an electrolyzer.
3. The use according to claim 2, characterized in that: The oxygen electrode material is lanthanum strontium manganate.
4. The use according to claim 2, characterized in that: The coating thickness of the fuel electrode is 10~70μm.
Citation Information
Patent Citations
Anode material of direct-hydrocarbon solid oxide fuel cell and preparation method thereof
CN102731090A
A kind of high temperature chemically stable SOFC perovskite anode material and preparation method thereof
CN105130426B
Solid oxide fuel cell anode material and preparation method and application thereof
CN113178587A
Three-phase conductor-proton-conductor composite cathode material and preparation method thereof
CN113258086A
Solid oxide electrolytic cell cathode material, and preparation method and application thereof
CN113782798A