A high-adhesion tinplate and preparation method thereof
By optimizing the flattening, reflowing and passivation processes of tin-plated plates, the problem of poor adhesion of tin-plated plates with tin content in high-protein food cans has been solved, and the adhesion and sulfur resistance properties of tin-plated plates have been improved, making it suitable for high-protein food cans. Application of canned protein foods.
Patent Information
- Application Number
- CN202210414413.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-15
AI Technical Summary
The existing tin-plated plate with a tin content of 5.6g/m2 is prone to poor adhesion of the paint film when used in food cans with high protein content, and the oxidation of the tin layer leads to a decrease in adhesion.
By controlling the roughness and surface morphology of the textured roller and grinding roller in the smoothing stage, optimizing the reflow temperature and passivation process, and adopting a two-stage passivation process of chemical passivation and electrochemical passivation, the quality of the passivation film is controlled. content and structure, reduce the adverse effect of Cr(OH)3 on adhesion, and prepare high adhesion tin plate.
It is possible to improve the adhesion of the tin-plated plate on the basis of the nominal tin content, ensure the adhesion and sulfur resistance of the paint film in high-protein food cans, and extend the service life of the tin-plated plate.
Smart Images

Figure CN114855230B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of steel preparation, and in particular to a high-adhesion tinplate and a preparation method thereof. Background Art
[0002] Nominal tin content 5.6g / m 2 Tinplate is generally used for products such as milk powder cans, electronic components and aerosol valves. During use, it is not painted or coated with a layer of paint film. The thickness of the paint film is generally 6g / m 2 When used to package high-protein braised pork or luncheon meat cans, two layers of paint are applied to the inner wall of the can with a thickness of 10-15g / m 2 ; The thicker the paint film, the higher the adhesion requirement for the tinplate, and the tin content is 5.6g / m 2 The roughness of the tin-plated sheet with tin layer will decrease with the oxidation of the tin layer, resulting in a significant deterioration in the adhesion of the tin-plated sheet with low tin content. Therefore, when it is used in canned meat, it is very easy to have poor paint film adhesion problems. Since canned meat is high in protein, the paint film of the tin-plated sheet has a high chromium content to prevent the paint film from being oxidized. The high surface chromium content is beneficial to the anti-sulfur performance of the tin-plated sheet but is not conducive to the paint film adhesion.
[0003] Therefore, how to obtain high-adhesion tin-plated sheets based on the nominal tin content is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application provides a high-adhesion tinplate and a preparation method thereof, so as to solve the technical problem in the prior art that it is difficult to obtain a high-adhesion tinplate based on the nominal tin content.
[0005] In a first aspect, the present application provides a method for preparing a high-adhesion tinplate, the method comprising:
[0006] obtaining a steel strip;
[0007] The steel strip is leveled, alkali washed, straightened, pickled, electrotinned, reflowed and passivated to obtain a tin-plated sheet;
[0008] The roughness Ra of the flat textured roller is 1.2 μm to 2.0 μm, and the Pc value of the flat textured roller is 120 to 150 pieces / cm.
[0009] The roughness Ra of the flat grinding roller is 0.2 μm to 0.6 μm;
[0010] The passivation is carried out in at least two stages, including a first stage and a second stage. The passivation method in the first stage includes chemical passivation, and the passivation method in the second stage includes electrochemical passivation.
[0011] The reflow temperature is 250°C to 280°C.
[0012] Optionally, the total flattening elongation is the sum of the flattening elongation of the texturing roller and the flattening elongation of the grinding roller, and the ratio of the flattening elongation of the texturing roller to the flattening elongation of the grinding roller is 1% to 1.2%: 0.8% to 1%.
[0013] Optionally, the total flattening elongation of the flattening is 1.8% to 2.2%.
[0014] Optionally, the reflow includes pure induction reflow, the height of the induction coil of the pure induction reflow from the liquid surface is 4.5m to 5.5m, and the quenching water temperature of the pure induction reflow is 80°C to 95°C.
[0015] Optionally, the chemical passivation and electrochemical passivation are performed in two passivation tanks respectively.
[0016] Optionally, the concentration of the passivation solution is 20 g / L to 25 g / L, the temperature of the passivation solution is 42° C. to 45° C., and the pH of the passivation solution is 3.8 to 4.0.
[0017] Optionally, the charge density of the electrochemical passivation is 0.3 As / dm 2 ~0.5As / dm 2 .
[0018] In a second aspect, the present application provides a high-adhesion tinplate, the tinplate being prepared by the method described in the first aspect, the tinplate comprising a steel substrate and a coating, the coating covering at least one surface of the steel substrate;
[0019] The tin coating amount of the coating is 5.2 g / m 2 ~5.6g / m 2 The coating includes Sn-Fe alloy and surface Cr, and the Sn-Fe alloy content of the coating is 0.6g / m 2 ~0.9g / m 2 The surface Cr content of the coating is 3 mg / m 2 ~5 mg / m 2 .
[0020] Optionally, the surface Cr includes:
[0021] [Cr(OH)3] / [Cr2O3]≤0.5,
[0022] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0023] Optionally, the roughness Ra of the tin-plated plate is 0.4 μm to 0.8 μm, the skewness Ssk>0, and the surface peak density Sds≥3200 / mm 2 .
[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0025] A method for preparing a high-adhesion tinplate is provided in an embodiment of the present application. The roughness and surface morphology of the roughening roller and the grinding roller in the leveling stage are controlled to control the roughness and peak density of the steel substrate, thereby improving the physical bonding ability of the coating and the paint film. The temperature of the soft melt is controlled to achieve both surface leveling to leak out the peaks and control the oxidation process of tin in the surface coating, thereby improving the surface adhesion of the tinplate. Finally, through the first stage of chemical passivation and the second stage of electrochemical passivation, the content and structure of the passivation film are controlled to reduce the adverse effect of Cr(OH)3 in the passivation solution coating on the adhesion, thereby achieving the purpose of obtaining a high-adhesion tinplate based on the nominal tin content. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A schematic diagram of the preparation method provided in the examples of the present application. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0030] The creative idea of this application is: According to domestic and foreign data and the production experience of various tinplate manufacturers, the research on the adhesion of tinplate at home and abroad mainly focuses on 5.6g / m 2The following low-tin tin-plated sheets, the research on the influence of low-tin tin-plated sheets on adhesion mainly focuses on roughness and passivation film. The research on roughness mainly focuses on the influence of roughness Ra on adhesion, while the research on the influence of other parameters of surface profile on adhesion is less. The research on passivation film mainly focuses on the influence of passivation film content and structure on adhesion, while the research on the influencing factors and control process of passivation film structure is less. At the same time, the soft melting process has no obvious effect on the adhesion of low-tin tin-plated sheets, but it has an obvious effect on 5.6g / m 2 Tinplate with tin plating amount or above plays a very important role.
[0031] However, there are three main deficiencies in the existing technology:
[0032] 1) Ra has a significant effect on adhesion in low-tin tinplate, but at 5.6g / m 2 For coatings above 1000 mm, due to the leveling effect of the surface tin, the Ra of the tin-plated sheet has little effect on the adhesion, and other surface profile parameters need to be used to characterize it.
[0033] 2) Improving adhesion only by reducing the surface passivation film content of tinplate is not comprehensive. The passivation film structure has a greater impact on adhesion, and process optimization is needed to control the passivation film structure;
[0034] 3) The soft melting process has no obvious effect on the adhesion of low-tin tin-plated plates, but it has a significant effect on 5.6g / m 2 Tinplates with a thickness of 100 mm and above play a very important role, and a reasonable reflow process range needs to be set to improve the adhesion of the tinplate.
[0035] In one embodiment of the present application, Figure 1 As shown, a method for preparing a high-adhesion tinplate is provided, the method comprising:
[0036] S1. Obtaining strip steel;
[0037] S2. The strip is successively leveled, alkali washed, straightened, pickled, electroplated, soft melted and passivated to obtain a tin plate;
[0038] The leveling includes dual-frame wet leveling, and the dual-frame wet leveling includes a first frame and a second frame;
[0039] The roughness Ra of the flat textured roller is 1.2 μm to 2.0 μm, and the Pc value of the flat textured roller is 120 to 150 pieces / cm.
[0040] The roughness Ra of the flat grinding roller is 0.2 μm to 0.6 μm;
[0041] The passivation is carried out in at least two stages, including a first stage and a second stage. The passivation method in the first stage includes chemical passivation, and the passivation method in the second stage includes electrochemical passivation.
[0042] The reflow temperature is 250°C to 280°C.
[0043] In the present application, the positive effect of the roughness Ra of the texturing roller being 1.2μm to 2.0μm is that within the range of the roughness Ra, it can not only eliminate some defects on the surface of the incoming annealed sheet, but also ensure that the surface roughness of the tinplate is between 0.4μm and 0.8μm; when the value of the roughness Ra exceeds the maximum value of the range, the adverse effect will be that the roughness is too high, which will make the surface roughness of the tinplate too large, which is not conducive to the uniformity and corrosion resistance of the tin layer of the tinplate; when the value of the roughness Ra is lower than the minimum value of the range, the adverse effect will be that the roughness is too low, which will make the tinplate unable to obtain a roughness ≥0.4μm.
[0044] The positive effect of the texturing roller Pc value of 120 to 150 pieces / cm is that within this value range, the surface peak density sds of the tinplate can be ≥ 3200 pieces / mm 2 , thereby improving the mechanical bonding with the paint film to obtain good adhesion performance; when the peak density Pc value exceeds the maximum value of this range, the adverse effect will be caused by the fact that the roughness is inversely proportional to the Pc value. When the PC value exceeds 150 pieces / cm, it cannot be guaranteed that its roughness is greater than 1.2μm. When the peak density Pc value is lower than the minimum value of this range, the adverse effect will be that the Pc value is too low, resulting in a peak density of less than 3200 pieces / mm on the surface of the tinplate. 2 , which is not conducive to the adhesion performance of the tinplate surface.
[0045] The positive effect of the grinding roller roughness Ra of 0.2μm~0.6μm is that within the roughness range, the surface roughness of the tinplate can be guaranteed to be in the range of 0.4μm~0.8μm; when the roughness Ra value exceeds the maximum value of this range, the adverse effect will be that the roughness Ra is too high, which will offset the profile formed by the frame texturing roller in the double-frame leveling machine, resulting in the roughness of the tinplate being too low, which is not conducive to the adhesion performance of the tinplate; when the roughness Ra value is lower than the minimum value of this range, the adverse effect will be that the roughness Ra is too low, resulting in the tinplate surface roughness being too large, which is not conducive to ensuring the uniformity and corrosion resistance of the tin layer of the tinplate.
[0046] The positive effect of the soft melting temperature being 250℃~280℃ is that within this temperature range, an alloy tin layer of appropriate thickness can be obtained to ensure the corrosion resistance of the tinplate, and the amount of SnO generated can be reduced to ensure the adhesion performance of the tinplate; when the temperature value exceeds the maximum value of this range, the adverse effect will be that the temperature is too high, resulting in poor adhesion performance of the tinplate; when the temperature value is lower than the minimum value of this range, the adverse effect will be that the temperature is too low, the content of the tin-iron alloy layer is too low, and the corrosion resistance of the tinplate is poor.
[0047] As an optional embodiment, the total flattening elongation is the sum of the flattening elongation of the texturing roller and the flattening elongation of the grinding roller, and the ratio of the flattening elongation of the texturing roller to the flattening elongation of the grinding roller is 1% to 1.2%: 0.8% to 1%.
[0048] As an optional implementation, the total flattening elongation of the flattening is 1.8% to 2.2%.
[0049] In the present application, the positive effect of the total flattening elongation of 1.8% to 2.2% is that within the range of the flattening elongation, a tinplate with the required roughness and surface peak density can be obtained; when the total flattening elongation exceeds the maximum value of the range, the adverse effect will be that the total flattening elongation is too large, which will cause the tinplate roughness to be too large, and at the same time, the surface peak density of the tinplate is too low, and the adhesion performance is reduced; when the total flattening elongation is lower than the minimum value of the range, the adverse effect will be that the total flattening elongation is too low, which will cause the tinplate roughness to be too low and the adhesion performance is reduced.
[0050] As an optional implementation, the reflow includes pure induction reflow, the induction coil of the pure induction reflow is at a height of 4.5m to 5.5m from the liquid surface, and the quenching water temperature of the pure induction reflow is 80°C to 95°C.
[0051] In the present application, the positive effect of the height of the induction coil from the liquid surface being 4.5m to 5.5m is that within this height range, both an alloy layer of appropriate thickness can be obtained, thereby ensuring the corrosion resistance of the tinplate, and the formation of an oxide film can be controlled, thereby ensuring the adhesion performance of the tinplate; when the height of the induction coil from the liquid surface exceeds the maximum value of the range, the adverse effect will be that the height is too high, which will cause the oxide film to thicken and the adhesion will decrease; when the height of the induction coil from the liquid surface is lower than the minimum value of the range, the adverse effect will be that the thickness of the alloy layer is too low, resulting in a decrease in corrosion resistance.
[0052] The positive effect of the quenching water temperature of pure induction softening being 80℃~95℃ is that under this temperature condition, the formation of quenching spots can be suppressed to ensure the surface quality of the tinplate; when the quenching water temperature exceeds the maximum value of this range, the adverse effect will be that the temperature is too high and high-temperature quenching spots will be formed; when the quenching water temperature is lower than the minimum value of this range, the adverse effect will be that the temperature is too low and low-temperature quenching spots will be formed on the surface of the tinplate.
[0053] As an optional implementation, the chemical passivation and electrochemical passivation are performed in two passivation tanks respectively.
[0054] As an optional implementation, the concentration of the passivation solution is 20 g / L to 25 g / L, the temperature of the passivation solution is 42° C. to 45° C., and the pH of the passivation solution is 3.8 to 4.0.
[0055] In the present application, the positive effect of the passivation solution concentration of 20g / L to 25g / L is that within this concentration range, the desired passivation film thickness can be obtained and the Cr(OH)3 / Cr2O3 ratio in the passivation film can be controlled to ensure the adhesion performance of the tinplate; when the concentration value exceeds the maximum value of the range, the adverse effect will be that the passivation solution concentration is too high, which will cause the Cr(OH)3 / Cr2O3 ratio in the passivation film to gradually increase, and the adhesion performance of the tinplate will decrease. When the concentration value is lower than the minimum value of the range, the adverse effect will be that the passivation solution concentration is too low, which will reduce the passivation current efficiency, which will cause the passivation film to become thinner and the corrosion resistance of the tinplate to decrease.
[0056] The positive effect of the passivation solution temperature of 42℃~45℃ is that within this concentration range, the required passivation film thickness can be obtained and the Cr(OH)3 / Cr2O3 ratio in the passivation film can be controlled to ensure the adhesion performance of the tinplate; when the temperature value exceeds the maximum value of this range, the adverse effect will be that the temperature is too high, which will cause the Cr(OH)3 / Cr2O3 ratio in the passivation film to gradually increase, and the adhesion performance of the passivation film will decrease. When the temperature value is lower than the minimum value of this range, the adverse effect will be that the temperature is too low, which will reduce the passivation current efficiency, which will cause the passivation film to become thinner and the corrosion resistance of the tinplate to decrease.
[0057] The positive effect of the passivation solution pH being 3.8-4.0 is that within the pH range, the desired passivation film thickness can be obtained and the Cr(OH)3 / Cr2O3 ratio in the passivation film can be controlled to ensure the adhesion performance of the tinplate; when the pH value exceeds the maximum value of the range, the adverse effect will be that the pH is too high, which will cause the Cr(OH)3 / Cr2O3 ratio in the passivation film to gradually increase, and the adhesion performance of the tinplate will decrease; when the pH value is lower than the minimum value of the range, the adverse effect will be that the pH is too low, which will intensify the hydrogen evolution reaction, and at the same time the surface passivation film of the tinplate will be thinned, resulting in a decrease in the corrosion resistance of the tinplate.
[0058] As an optional embodiment, the charge density of the electrochemical passivation is 0.3 As / dm 2 ~0.5As / dm 2 .
[0059] In this application, the charge density of electrochemical passivation is 0.3As / dm 2 ~0.5As / dm 2 The positive effect is that within the range of charge density, the required passivation film thickness can be obtained and the Cr(OH)3 / Cr2O3 ratio in the passivation film can be controlled to ensure the adhesion performance of the tinplate; when the charge density value exceeds the maximum value of this range, the adverse effect will be that the charge density is too large, which will cause the Cr(OH)3 / Cr2O3 ratio in the passivation film to gradually increase, and the adhesion performance of the tinplate will decrease. When the charge density value is lower than the minimum value of this range, the adverse effect will be that the charge density is too low, which will cause the passivation film to become thinner and the corrosion resistance of the tinplate will decrease.
[0060] In one embodiment of the present application, a high-adhesion tinplate is provided, the tinplate is prepared by the method, the tinplate comprises a steel substrate and a coating, the coating covers at least one surface of the steel substrate;
[0061] The tin coating amount of the coating is 5.2 g / m 2 ~5.6g / m 2 The coating includes Sn-Fe alloy and surface Cr, and the Sn-Fe alloy content of the coating is 0.6g / m 2 ~0.9g / m 2 The surface Cr content of the coating is 3 mg / m 2 ~5 mg / m 2 .
[0062] In this application, the Sn-Fe alloy content of the coating is 0.6 g / m 2 ~0.9g / m 2The positive effect is that within this content range, the corrosion resistance and adhesion performance of the tinplate can be guaranteed at the same time; when the alloy content exceeds the maximum value of this range, the adverse effect will be that the Sn-Fe alloy content is too high, which will lead to a decrease in the adhesion performance of the tinplate; when the alloy content is lower than the minimum value of this range, the adverse effect will be that the Sn-Fe alloy content is too low and the corrosion resistance of the tinplate is insufficient.
[0063] As an optional embodiment, the surface Cr includes:
[0064] [Cr(OH)3] / [Cr2O3]≤0.5,
[0065] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0066] In the present application, the positive effect of [Cr(OH)3] / [Cr2O3]≤0.5 is that under this condition, it can prevent the dehydration of Cr(OH)3 in the passivation film during coating and baking, which causes the adhesion performance of the tinplate to decrease; when the ratio exceeds the maximum value of this range, the adverse effect will be that there is too much Cr(OH)3 in the passivation film, which will dehydrate and cause the adhesion performance of the tinplate to decrease.
[0067] As an optional embodiment, the roughness Ra of the tinplate is 0.4 μm to 0.8 μm, the skewness Ssk>0, and the surface peak density Sds≥3200 / mm 2 .
[0068] Example 1
[0069] A method for preparing a high-adhesion tinplate, comprising:
[0070] S1. A cold-rolled and annealed steel plate T-4CA having a thickness of 0.21 mm and a width of 934 mm, the steel plate is annealed to obtain a strip;
[0071] S2. The strip is successively leveled, alkali washed, straightened, pickled, electroplated, soft melted and passivated to obtain a tin plate;
[0072] The roughness Ra of the flat texture roller is 1.6μm, and the Pc value of the flat texture roller is 130 pieces / cm.
[0073] The roughness Ra of the flat grinding roller is 0.4 μm;
[0074] The passivation includes a first stage and a second stage, the first stage includes chemical passivation, and the second stage includes electrochemical passivation;
[0075] The reflow temperature is 250°C.
[0076] The total flattening elongation of flattening includes the flattening elongation of the textured roller and the flattening elongation of the grinding roller, and the ratio of the flattening elongation of the textured roller to the flattening elongation of the grinding roller is 1.1%:0.9%.
[0077] The total flat elongation after flattening is 2.0%.
[0078] Soft melting includes pure induction soft melting. The height of the induction coil of pure induction soft melting from the liquid surface is 5.0m, and the quenching water temperature of pure induction soft melting is 90℃.
[0079] Chemical passivation and electrochemical passivation are carried out in two passivation tanks respectively, the circuits of the No. 1 and No. 2 plates in the first passivation tank are closed, and the circuits of the No. 3 and No. 4 plates in the second passivation tank are opened;
[0080] The concentration of the passivation solution is 20 g / L, the temperature of the passivation solution is 42° C., and the pH of the passivation solution is 4.0.
[0081] The charge density of electrochemical passivation is 0.4As / dm 2 .
[0082] A high-adhesion tinplate, prepared by the above method, comprises a steel substrate and a coating, wherein the coating covers at least one surface of the steel substrate;
[0083] The tin coating weight is 5.2g / m 2 ; The coating includes Sn-Fe alloy and surface Cr, and the content of Sn-Fe alloy in the coating is 0.8g / m 2 The surface Cr content of the coating is 4.0 mg / m 2 .
[0084] Surface Cr includes:
[0085] [Cr(OH)3] / [Cr2O3]=0.2,
[0086] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0087] The roughness Ra of the tinplate is 0.45μm, the skewness Ssk>0, and the surface peak density Sds=3500 pieces / mm 2 .
[0088] Example 2
[0089] Comparing Example 2 with Example 1, the difference between Example 2 and Example 1 is:
[0090] A method for preparing a high-adhesion tinplate, comprising:
[0091] S1. A cold-rolled and annealed steel plate T-3CA having a thickness of 0.19 mm and a width of 911 mm, the steel plate is annealed to obtain a strip;
[0092] S2. The strip is leveled, sprayed with alkali solution, electrolytically washed, straightened, pickled, electroplated with tin, soft melted and passivated in sequence to obtain a tin plate;
[0093] The roughness Ra of the flat texture roller is 2.0μm, and the Pc value of the flat texture roller is 150 pieces / cm.
[0094] The roughness Ra of the flat grinding roller is 0.6 μm;
[0095] The reflow temperature is 280°C.
[0096] The total flattening elongation is the sum of the flattening elongation of the textured roller and the flattening elongation of the grinding roller, and the ratio of the flattening elongation of the textured roller to the flattening elongation of the grinding roller is 1.2%:0.8%.
[0097] The total flattened elongation is 2.2%.
[0098] The height of the induction coil of pure induction melting is 5.5m from the liquid surface, and the quenching water temperature of pure induction melting is 95℃.
[0099] The concentration of the passivation solution is 25 g / L, the temperature of the passivation solution is 45° C., and the pH of the passivation solution is 4.0.
[0100] The charge density of electrochemical passivation is 0.5As / dm 2 .
[0101] A high-adhesion tinplate, prepared by the above method, comprises a steel substrate and a coating, wherein the coating covers at least one surface of the steel substrate;
[0102] The tin coating weight is 5.2g / m 2 ; The coating includes Sn-Fe alloy and surface Cr, and the Sn-Fe alloy content of the coating is 0.9g / m 2 The surface Cr content of the coating is 5.0 mg / m 2 .
[0103] Surface Cr includes:
[0104] [Cr(OH)3] / [Cr2O3]=0.2,
[0105] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0106] The roughness Ra of the tinplate is 0.7μm, the skewness Ssk>0, and the surface peak density Sds=3800 pieces / mm 2 .
[0107] Example 3
[0108] Comparing Example 3 with Example 1, the difference between Example 3 and Example 1 is:
[0109] A method for preparing a high-adhesion tinplate, comprising:
[0110] S1. A cold-rolled and annealed steel plate T-4CA having a thickness of 0.21 mm and a width of 934 mm, the steel plate is annealed to obtain a strip;
[0111] S2. The strip is successively leveled, alkali washed, straightened, pickled, electroplated, soft melted and passivated to obtain a tin plate;
[0112] The roughness Ra of the flat texture roller is 1.2μm, and the Pc value of the flat texture roller is 120 pieces / cm.
[0113] The roughness Ra of the flat grinding roller is 0.2μm;
[0114] The passivation includes a first stage including chemical passivation and a second stage including electrochemical passivation;
[0115] The reflow temperature is 250°C.
[0116] The total flattening elongation of the flattening includes the flattening elongation of the textured roller and the flattening elongation of the grinding roller, and the ratio of the flattening elongation of the textured roller to the flattening elongation of the grinding roller is 1%:1%.
[0117] The total flattened elongation is 1.8%.
[0118] Soft melting includes pure induction soft melting. The height of the induction coil of pure induction soft melting from the liquid surface is 4.5m, and the quenching water temperature of pure induction soft melting is 80℃.
[0119] The concentration of the passivation solution is 22 g / L, the temperature of the passivation solution is 42° C., and the pH of the passivation solution is 3.9.
[0120] The charge density of electrochemical passivation is 0.3As / dm 2 .
[0121] A high-adhesion tinplate, prepared by the above method, comprises a steel substrate and a coating, wherein the coating covers at least one surface of the steel substrate;
[0122] The tin coating weight is 5.4g / m 2; The coating includes Sn-Fe alloy and surface Cr, and the content of Sn-Fe alloy in the coating is 0.6g / m 2 The surface Cr content of the coating is 3 mg / m 2 .
[0123] Surface Cr includes:
[0124] [Cr(OH)3] / [Cr2O3]=0.4,
[0125] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0126] The roughness Ra of the tinplate is 0.4μm, the skewness Ssk>0, and the surface peak density Sds=3200 pieces / mm 2 .
[0127] Comparative Example 1
[0128] Comparing Comparative Example 1 with Example 1, the difference between Comparative Example 1 and Example 1 is:
[0129] A method for preparing a high-adhesion tinplate, comprising:
[0130] S1. A cold-rolled and annealed steel plate T-3CA having a thickness of 0.21 mm and a width of 934 mm, the steel plate is annealed to obtain a strip;
[0131] S2. The strip is successively leveled, alkali washed, straightened, pickled, electroplated, soft melted and passivated to obtain a tin plate;
[0132] The roughness Ra of the flat texture roller is 1.6μm, and the Pc value of the flat texture roller is 130 pieces / cm.
[0133] The roughness Ra of the flat grinding roller is 0.4 μm;
[0134] The reflow temperature is 290°C.
[0135] The total flattening elongation of the flattening includes the flattening elongation of the textured roller and the flattening elongation of the grinding roller, and the ratio of the flattening elongation of the textured roller to the flattening elongation of the grinding roller is 1.1%:0.9%.
[0136] The total flat elongation after flattening is 2.0%.
[0137] Soft melting includes pure induction soft melting. The height of the induction coil of pure induction soft melting from the liquid surface is 5.5m, and the quenching water temperature of pure induction soft melting is 90℃.
[0138] The concentration of the passivation solution is 20 g / L, the temperature of the passivation solution is 42° C., and the pH of the passivation solution is 4.0.
[0139] The charge density of electrochemical passivation is 0.0.4As / dm 2 .
[0140] A high-adhesion tinplate, prepared by the above method, comprises a steel substrate and a coating, wherein the coating covers at least one surface of the steel substrate;
[0141] The tin coating weight is 5.2g / m 2 ; The coating includes Sn-Fe alloy and surface Cr, and the content of Sn-Fe alloy in the coating is 1.4g / m 2 The surface Cr content of the coating is 4.0 mg / m 2 .
[0142] Surface Cr includes:
[0143] [Cr(OH)3] / [Cr2O3]=0.2,
[0144] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0145] The roughness Ra of the tinplate is 0.45μm, the skewness Ssk>0, and the surface peak density Sds=3500 pieces / mm 2 .
[0146] Comparative Example 2
[0147] Comparing Comparative Example 2 with Example 1, the difference between Comparative Example 2 and Example 1 is:
[0148] A method for preparing a high-adhesion tinplate, comprising:
[0149] S1. A cold-rolled and annealed steel plate T-4CA having a thickness of 0.19 mm and a width of 911 mm, the steel plate is annealed to obtain a strip;
[0150] S2. The strip is successively leveled, alkali washed, straightened, pickled, electroplated, soft melted and passivated to obtain a tin plate;
[0151] The roughness Ra of the flat texture roller is 1.1μm, and the Pc value of the flat texture roller is 100 pieces / cm.
[0152] The roughness Ra of the flat grinding roller is 0.1 μm;
[0153] The reflow temperature is 240℃
[0154] The ratio of the flat elongation of the texturing roller to the flat elongation of the grinding roller is 1%:2%.
[0155] The total flattened elongation is 1.4%.
[0156] Soft melting includes pure induction soft melting. The height of the induction coil of pure induction soft melting from the liquid surface is 4m, and the quenching water temperature of pure induction soft melting is 100℃.
[0157] The passivation solution concentration is 15 g / L, and the passivation solution temperature is 40°C.
[0158] The charge density of electrochemical passivation is 0.2As / dm 2 .
[0159] The tin coating weight is 5.0g / m 2 ; The coating includes Sn-Fe alloy and surface Cr, and the content of Sn-Fe alloy in the coating is 0.5g / m 2 The surface Cr content of the coating is 2 mg / m 2 .
[0160] A high-adhesion tinplate, prepared by the above method, comprises a steel substrate and a coating, wherein the coating covers at least one surface of the steel substrate;
[0161] Surface Cr includes:
[0162] [Cr(OH)3] / [Cr2O3]=1.2,
[0163] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0164] The roughness Ra of the tinplate is 0.5μm, the skewness Ssk>0, and the surface peak density Sds=3200 pieces / mm 2 .
[0165] Comparative Example 3
[0166] Comparing Comparative Example 3 with Example 1, the difference between Comparative Example 3 and Example 1 is:
[0167] A method for preparing a high-adhesion tinplate, comprising:
[0168] S1. A cold-rolled and annealed steel plate T-4CA having a thickness of 0.19 mm and a width of 911 mm, the steel plate is annealed to obtain a strip;
[0169] S2. The strip is successively leveled, alkali washed, straightened, pickled, electroplated, soft melted and passivated to obtain a tin plate;
[0170] The roughness Ra of the flat texture roller is 2.1μm, and the Pc value of the flat texture roller is 160 pieces / cm.
[0171] The roughness Ra of the flat grinding roller is 0.8 μm;
[0172] The reflow temperature is 300°C.
[0173] The ratio of the flat elongation of the texturing roller to the flat elongation of the grinding roller is 1.3%:1.1%.
[0174] The total flattened elongation is 2.4%.
[0175] Soft melting includes pure induction soft melting. The height of the induction coil of pure induction soft melting from the liquid surface is 6.0m, and the quenching water temperature of pure induction soft melting is 100℃.
[0176] The concentration of the passivation solution is 30 g / L, and the temperature of the passivation solution is 50°C.
[0177] The charge density of electrochemical passivation is 1.0 As / dm 2 .
[0178] The tin coating weight is 5.6g / m 2 ; The coating includes Sn-Fe alloy and surface Cr, and the content of Sn-Fe alloy in the coating is 1.2g / m 2 The surface Cr content of the coating is 6.5 mg / m 2 .
[0179] Surface Cr includes:
[0180] [Cr(OH)3] / [Cr2O3]=1.4,
[0181] Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, and [Cr2O3] is the mass fraction of Cr2O3.
[0182] The roughness Ra of the tinplate is 1.2μm, the skewness Ssk<0, and the surface peak density Sds=3000 pieces / mm 2 .
[0183] Related experiments:
[0184] The tin-plated sheets obtained in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the results are shown in Table 1.
[0185] Test methods for related experiments:
[0186] Paint film adhesion grade: Tested in accordance with QB / T2763 "Coated tin (or chromium) thin steel sheet".
[0187] Anti-sulfur performance of tinplate: tested in accordance with QB / T2763 "Coated tin (or chromium) thin steel plate".
[0188] Table 1
[0189]
[0190]
[0191] In Table 1,
[0192] The paint film adhesion grade refers to the ability of the paint film to bond with the surface of the coated object or between coatings. The lower the paint film adhesion grade, the stronger the adhesion of the tinplate.
[0193] Anti-sulfur performance refers to the material's resistance to sulfur. The lower the level of anti-sulfur performance, the higher the paint film's resistance to sulfur and the stronger its protection against food.
[0194] From the data of Examples 1-4, it can be seen that:
[0195] According to different strip steel specifications, the process parameters of leveling, soft melting and passivation are adjusted, so that different specifications of strip steel can be controlled to obtain tinplate with grade 1 paint film adhesion and grade 1 sulfur resistance.
[0196] From the data of Comparative Examples 1-3, it can be seen that:
[0197] If the process parameters used are not within the scope of this application, the paint film adhesion level and sulfur resistance level of the strip will be reduced.
[0198] One or more technical solutions in the embodiments of the present application also have at least the following technical effects:
[0199] (1) The preparation method provided in the embodiment of the present application proposes that Ra has no obvious effect on the adhesion of the paint film of high-tin tin-plated plates, while the surface profile parameter skewness Ssk and surface peak density can better represent the influence of surface morphology on adhesion, and determines the roller matching and process parameters of the leveling process.
[0200] (2) The preparation method provided in the embodiment of the present application optimizes the soft melting process to achieve the surface leveling effect to leak out the peak and control the oxidation of the surface tin to improve the adhesion of the paint film.
[0201] (3) The preparation method provided in the embodiment of the present application innovatively adopts a first stage including chemical passivation and a second stage including electrochemical passivation to comprehensively control the value of Cr(OH)3 / Cr2O3, thereby controlling the Cr(OH)3 content to improve adhesion.
[0202] (4) The tin-plated sheet provided in the embodiment of the present application has a roughness Ra of 0.4 μm to 0.8 μm, a skewness Ssk>0, and a surface peak density Sds≥3200 pieces / mm 2 .
[0203] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0204] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a high-adhesion tinplate, characterized in that: The method comprises: Obtaining strip steel; The strip steel is leveled, alkali washed, straightened, pickled, electrotinned, soft melted and passivated to obtain a tin plate, wherein the roughness Ra of the tin plate is 0.4 μm to 0.8 μm, the skewness Ssk>0, and the surface peak density Sds≥3200 pieces / mm 2 The tin coating weight is 5.2g / m 2 ~5.6g / m 2 The coating includes Sn-Fe alloy and surface Cr, and the Sn-Fe alloy content of the coating is 0.6g / m 2 ~0.9g / m 2 The surface Cr content of the coating is 3 mg / m 2 ~5 mg / m 2 , the surface Cr comprises: [Cr(OH)3] / [Cr2O3]≤0.5, Wherein, [Cr(OH)3] is the mass fraction of Cr(OH)3, [Cr2O3] is the mass fraction of Cr2O3; The roughness Ra of the flat textured roller is 1.2 μm to 2.0 μm, and the Pc value of the flat textured roller is 120 to 150 pieces / cm. The roughness Ra of the flat grinding roller is 0.4 μm to 0.6 μm; The passivation is carried out in at least two stages, including a first stage and a second stage. The passivation method of the first stage includes chemical passivation, and the passivation method of the second stage includes electrochemical passivation. The charge density of the electrochemical passivation is 0.3 As / dm 2 ~0.5As / dm 2 ; The temperature of the soft melting is 250°C to 280°C, the total flattening elongation of the flattening is the sum of the flattening elongation of the textured roller and the flattening elongation of the grinding roller, the ratio of the flattening elongation of the textured roller to the flattening elongation of the grinding roller is 1% to 1.2%: 0.8% to 1%, and the total flattening elongation of the flattening is 1.8% to 2.2%; The reflowing includes pure induction reflowing, the induction coil of the pure induction reflowing is at a height of 4.5m to 5.5m from the liquid surface, and the quenching water temperature of the pure induction reflowing is 80°C to 95°C.
2. The method according to claim 1, characterized in that The chemical passivation and electrochemical passivation are carried out in two passivation tanks.
3. The method according to claim 1, characterized in that: The concentration of the passivation solution is 20 g / L to 25 g / L, the temperature of the passivation solution is 42° C. to 45° C., and the pH of the passivation solution is 3.8 to 4.
0.
4. A high adhesion tinplate, characterized in that: The tinplate is prepared by the method according to any one of claims 1 to 3, and comprises a steel substrate and a coating, wherein the coating covers at least one surface of the steel substrate.
Citation Information
Patent Citations
Cold rolled tin-plated steel plate for multiple printing and painting and manufacturing method thereof
CN104711474A
Preparation method of tinned steel plate with ultralow tin content and application of preparation method
CN109023445A