Terminals

A terminal with a Cu, Sn, and Sn-Cu alloy plating layer and intermetallic Ni crystals addresses durability issues in high-temperature environments by enhancing mechanical properties.

JP7579476B1Active Publication Date: 2024-11-07NAPRA

Patent Information

Application Number
JP2024024522
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-11-07
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

Terminals made of precious metals or single metals face durability issues when operating in high-temperature environments.

Method used

A terminal with a plating layer containing Cu, Sn, and a Sn-Cu alloy, and dispersed intermetallic compound crystals of Ni, featuring a concentration gradient of base metal and Sn, is developed to enhance durability.

Benefits of technology

The terminal exhibits excellent durability, impact resistance, and abrasion resistance in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579476000001_ABST
    Figure 0007579476000001_ABST
Patent Text Reader

Abstract

Because of their high electrical conductivity, plating films made of precious metals or single metals such as silver plating or tin plating are widely used in contacts and terminal parts of electronic devices such as connectors, switches, relays, etc. However, terminals made of such precious metals or single metals have issues with durability when operating in high-temperature environments. [Solution] The above problem is solved by providing a terminal having a plating layer formed on the surface of a substrate, the plating layer having a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing Sn and a Sn-Cu alloy, and the plating layer has a concentration gradient in which the concentrations of Cu and Sn change from the substrate toward the terminal surface.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a terminal suitable for use as a connecting portion for electronic components, a joining terminal, or the like. [Background technology]

[0002] Because of their high electrical conductivity, plating films made of precious metals or single metals, such as silver plating or tin plating, are widely used for contacts and terminals in electronic device connectors, switches, relays, etc. However, terminals made of such precious metals or single metals have issues with durability when operating in high-temperature environments.

[0003] The following Patent Document 1 discloses a tin contact terminal having a tin-copper intermetallic compound dispersed therein, which is characterized in that a tin plating layer having a tin-copper intermetallic compound dispersed therein is formed on the surface of a substrate made of copper or a copper alloy. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-82499 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a terminal that is excellent in durability when operating in a high-temperature environment. [Means for solving the problem]

[0006] The present invention provides a terminal having a plating layer formed on the surface of a substrate, the plating layer containing Cu and having a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing Sn and a Sn-Cu alloy, and the plating layer has a concentration gradient in which the concentrations of the substrate metal and Sn change from the substrate toward the terminal surface. Effect of the Invention

[0007] According to the present invention, it is possible to provide a terminal that is excellent in durability when operating in a high-temperature environment. The terminal of the present invention is also excellent in impact resistance and abrasion resistance. [Brief description of the drawings]

[0008] [Figure 1] 1 is an optical image of a cross section of the electrolytic plating electrode of the present invention obtained in Example 1, thinly cut with a FIB (focused ion beam). [Diagram 2] 2 is a cross-sectional SEM image of the obtained electrolytic plating electrode of Example 1. [Figure 3A] FIG. 2 is a cross-sectional view of a plating layer illustrating measurement points in an element mapping analysis by EDS of the contact terminal obtained in Example 1. [Figure 3B] FIG. 3B is a diagram showing the results of element mapping analysis by EDS of region 001 in FIG. 3A. [Figure 3C] FIG. 3B is a diagram showing the results of elemental mapping analysis by EDS of region 002 in FIG. 3A. [Figure 3D] FIG. 3B is a diagram showing the results of elemental mapping analysis by EDS of region 003 in FIG. 3A. [Figure 3E] FIG. 3B is a diagram showing the results of elemental mapping analysis by EDS of region 004 in FIG. 3A. [Figure 3F] FIG. 3B is a diagram showing the results of elemental mapping analysis by EDS of region 005 in FIG. 3A. [Figure 3G] FIG. 3B is a diagram showing the results of elemental mapping analysis by EDS of region 006 in FIG. 3A. [Figure 4] FIG. 2 is a diagram for explaining an example of a manufacturing apparatus suitable for manufacturing the metal particles of the present invention. [Diagram 5] 4 is a micrograph showing the results of a 180-degree bending test of the contact terminal of Example 1. [Figure 6] 4 is a micrograph showing the results of a surface crack test on the contact terminal of Example 1. [Figure 7]4 is a micrograph showing the heat resistance test results of Example 1. [Figure 8] 11 is a photomicrograph showing the results of a 180-degree bending test of the contact terminal of Comparative Example 1. [Figure 9] 1 is a photomicrograph showing the results of a surface crack test for Comparative Example 1. [Figure 10] 1 is a micrograph showing the results of a heat resistance test of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present invention will be described in further detail. First, the terminology used in this specification is as follows unless otherwise specified. (1) When referring to metals, it can include not only single metallic elements but also alloys containing multiple metallic elements and intermetallic compound crystals. (2) When referring to a single metallic element, it does not mean only a substance that is completely and purely made of that metallic element, but also includes cases where it contains trace amounts of other substances. In other words, it does not mean to exclude substances that contain trace amounts of impurities that have almost no effect on the properties of the metallic element, and for example, when referring to a parent phase, it does not mean to exclude a substance in which some of the atoms in a Sn crystal are replaced by other elements (e.g., Cu). For example, the other substances or other elements may be: Under conditions that have little effect on the properties of the metal element, The following terminals may contain 0 to 0.1% by mass. (3) Endotaxial bonding means that intermetallic compound crystals are precipitated in a substance that will become a metal or alloy (the parent phase in this invention), and during this precipitation, the Sn-Cu alloy and the intermetallic compound crystals are bonded at the crystal lattice level to form crystal grains and crystal layers. The term endotaxial is well known and is described, for example, in Nature Chemistry 3(2): 160-6, 2011, page 160, left column, last paragraph.

[0010] The terminal of the present invention is a terminal having a plating layer formed on the surface of a base material, the plating layer containing Cu and having a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing Sn and a Sn-Cu alloy.

[0011] The following electrolytic plating electrode is applied to the plating bath for providing the plating layer. Hereinafter, the electrolytic plating electrode may be referred to as the "electrolytic plating electrode of the present invention."

[0012] The electrolytic plating electrode of the present invention has a structure having an intermetallic compound crystal containing Sn, Cu, Cr and Ni in a matrix containing Sn and a Sn-Cu alloy, and the composition of the structure is preferably Cu 5~85% by mass, Cr 0.001~1% by mass, Ni 0.01~5% by mass, The balance is Sn (however, it may contain unavoidable impurities of 0.1% by mass or less), The intermetallic compound crystals are present in a state of being contained in the matrix. The composition of the matrix phase is preferably 5 mass % or less of Cu, 1 mass % or less of Ni, 1 mass % or less of Cr, and the balance being Sn (however, unavoidable impurities may be contained at 0.1 mass % or less).

[0013] FIG. 1 is an optical image of a cross section of an electrolytic plating electrode of the present invention obtained in Example 1 below, which was thinly cut with a FIB (focused ion beam).

[0014] The electrolytic plating electrode of the present invention may be a soluble electrode and may be produced by the following method. First, metal particles described below (hereinafter sometimes referred to as metal particles of the present invention) are produced. Next, the obtained metal particles of the present invention are melted by high-frequency induction heating under vacuum, cast into a mold in a nitrogen gas atmosphere under atmospheric pressure, cooled and solidified, and formed into a rolled sheet, and multiple sheets of this are stacked as necessary (hereinafter sometimes referred to as bulk) to obtain an electrode for electrolytic plating.

[0015] The metal particles of the present invention can be produced from a raw material having a composition of, for example, 8% by mass of Cu, 1% by mass of Cr, 1% by mass of Ni, and the balance being Sn, by melting the raw material, feeding it onto a dish-shaped disk rotating at high speed in a nitrogen gas atmosphere, scattering the molten metal as small droplets by centrifugal force, and cooling and solidifying it under reduced pressure.

[0016] An example of a manufacturing apparatus suitable for manufacturing the metal particles of the present invention will be described with reference to FIG. 4. The granulation chamber 1 has a cylindrical upper part and a cone-shaped lower part, and has a lid 2 on the upper part. A nozzle 3 is inserted vertically into the center of the lid 2, and a dish-shaped rotating disk 4 is provided directly below the nozzle 3. Reference numeral 5 denotes a mechanism for supporting the dish-shaped rotating disk 4 so that it can move up and down. An exhaust pipe 6 for the generated particles is connected to the lower end of the cone part of the granulation chamber 1. The upper part of the nozzle 3 is connected to a melting furnace 7 for melting the metal to be granulated. Ambient gas adjusted to a predetermined composition in a mixed gas tank 8 is supplied to the inside of the granulation chamber 1 and the upper part of the electric furnace 7 through pipes 9 and 10, respectively. The pressure in the granulation chamber 1 is controlled by a valve 11 and an exhaust device 12, and the pressure in the electric furnace 7 is controlled by a valve 13 and an exhaust device 14, respectively. The molten metal supplied from the nozzle 3 onto the dish-shaped rotating disk 4 is dispersed in the form of fine droplets by the centrifugal force of the dish-shaped rotating disk 4, and is cooled under reduced pressure to become solid particles. The solid particles thus produced are fed from the discharge pipe 6 to an automatic filter 15 where they are separated. Reference numeral 16 denotes a fine particle collector.

[0017] The process of cooling and solidifying the molten metal from a high temperature melt is important for forming the metal particles of the present invention. For example, the following conditions may be mentioned: The melting temperature of the metal in the melting furnace 7 is set to 800° C. to 1000° C., and while maintaining this temperature, the molten metal is supplied from the nozzle 3 onto the dish-shaped rotating disk 4 . The dish-shaped rotating disk 4 used is a dish-shaped disk having an inner diameter of 35 mm and a rotor thickness of 5 mm, and is rotated at 80,000 to 100,000 revolutions per minute. Granulation chamber 1: 9 x 10 -2After reducing the pressure in the granulation chamber 1 using a vacuum chamber capable of reducing the pressure to about 1×10 Pa, nitrogen gas at 15 to 50° C. was supplied while simultaneously evacuating the gas. -1 Pa or less.

[0018] The metal particles of the present invention are obtained in the manner described above. The particle diameter of the metal particles of the present invention is approximately 5 μm, and preferably ranges from 1 μm to 50 μm, for example.

[0019] Next, the obtained metal particles of the present invention are melted by high-frequency induction heating under vacuum, cast into a mold in a nitrogen gas atmosphere under atmospheric pressure, cooled and solidified, and formed into a rolled sheet, and multiple sheets of this are stacked as necessary to obtain a bulk. The high-frequency induction heating and cooling / solidifying conditions are important for forming the electrolytic plating electrode of the present invention. For example, the following conditions may be mentioned: High frequency induction heating: 9×10 -2 A crucible for high-frequency melting is placed in a vacuum chamber capable of reducing the pressure to about Pa, and the metal particles of the present invention are introduced into the crucible. While the pressure is reduced to about the aforementioned reduced pressure level, high-frequency induction heating is performed on the metal particles of the present invention, the heating temperature is increased to 800°C to 1000°C to melt the metal particles of the present invention, and the temperature is maintained for 5 to 15 minutes. Cooling and solidification: Next, while flowing nitrogen gas at 15 to 50°C into the tank, the heating temperature is set to about 400°C or higher under atmospheric pressure, casting is performed, and the mixture is cooled and solidified at 30°C or lower.

[0020] The electrolytic plating electrode of the present invention preferably has a composition, for example, Cu 5~85% by mass, Cr 0.001~1% by mass, Ni 0.01~5% by mass, The balance is Sn (however, it may contain unavoidable impurities of 0.1 mass % or less). The composition is the same as that of the metal particles of the present invention.

[0021] The composition of the parent phase in the electrolytic plating electrode can be 5 mass % or less (e.g., 0.1 to 5 mass %) of Cu, 1 mass % or less (e.g., 0.01 to 1 mass %) of Ni, 1 mass % or less (e.g., 0.01 to 1 mass %) of Cr, and the balance being Sn. The composition of the parent phase is the same as that of the metal particles of the present invention.

[0022] The composition of the intermetallic compound crystal in the electrolytic plating electrode of the present invention is as follows: Sn 50~70% by mass, Cu 30~50% by mass, Cr 0.001~3% by mass, Ni 0.01~6.5% by mass It is preferable that: The proportion of the intermetallic compound crystals in the electrolytic plating electrode of the present invention is, for example, 20 to 60 mass %, and preferably 30 to 40 mass %, based on the entire electrolytic plating electrode. The intermetallic compound crystals are present in a state of being included in the matrix.

[0023] The composition and ratio of the parent phase and intermetallic compound crystals in the electrolytic plating electrode of the present invention can be satisfied by following the manufacturing conditions of the electrolytic plating electrode. The inventors have confirmed that the structure of the electrolytic plating electrode of the present invention is maintained even when the electrode is rolled into a sheet or bulked.

[0024] In the electrolytic plating electrode of the present invention, it is preferable that at least a part of the parent phase and the intermetallic compound crystal is endotaxy bonded. As described above, endotaxy bond is a bonding in which an intermetallic compound crystal is precipitated in a substance (parent phase in the present invention) that becomes a metal or alloy, and during this precipitation, the Sn-Cu alloy and the intermetallic compound crystal are bonded at the crystal lattice level to form a crystal grain. The formation of endotaxy bond can solve the problem of the brittleness of the intermetallic compound crystal, and can also suppress the decrease in mechanical strength caused by the change in the crystal structure of Sn, thereby providing a contact terminal with excellent durability. The endotaxial bond of the electrolytic plating electrode of the present invention can be formed according to the manufacturing conditions of the electrolytic plating electrode described above.

[0025] In addition, the endotaxy bonding is preferably 30% or more, and more preferably 60% or more, when the entire bonding surface between the Sn-Cu alloy and the intermetallic compound crystal in the parent phase is taken as 100%. The proportion of the endotaxy bonding can be calculated, for example, as follows. The cross section of the electrode for electrolytic plating is photographed using an electron microscope, and 50 joint surfaces between the Sn-Cu alloy and the intermetallic compound crystal are randomly sampled. The joint surfaces are then image-analyzed to determine the extent to which endotaxial joints, as shown in the following examples, exist on the sampled joint surfaces.

[0026] The electrolytic plating electrode of the present invention is also useful as an electrolytic plating electrode (anode) for forming the plating layer. In the electrolytic plating electrode of the present invention, the intermetallic compound crystals contained in the electrolytic plating electrode are dispersed in a plating bath at nano-sized sizes (1 μm or less), and are plated on the substrate surface together with the parent phase with an electric charge to form a plating layer. The formed plating layer preferably has a structure in which intermetallic compound crystals containing Sn, Cu, Cr, and Ni are dispersed in a parent phase made of an Sn-Cu alloy, and at least a part of the parent phase and the intermetallic compound crystals are endotaxy-bonded. Also, it is preferable that the electrode is epitaxially bonded to the substrate.

[0027] The plating bath for providing the plating layer may contain the electrolytic plating electrode of the present invention and may have, for example, the following composition. Copper sulfate 180~250g / L Stannous sulfate 30~50g / L Sulfuric acid 80~120g / L Additives, etc. (adhesion inhibitors, interface complexing agents, film forming agents, electrodiffusion wear forming agents)

[0028] In addition to the above-mentioned exemplary components of the plating bath, known dispersants, brighteners, antioxidants, etc. may be appropriately added as necessary. Examples of such agents include dispersants such as polyoxyethylene cumyl phenyl ether and polyoxyethylene lauryl ether, brighteners such as cresol sulfonic acid, acetaldehyde, and acetylacetone, and antioxidants such as formalin, catechol, and hydroquinone.

[0029] The plating temperature is, for example, 30°C or lower, and is preferably 15 to 20°C.

[0030] The current density is, for example, 1 to 10 A / dm 2 The range is adjusted appropriately.

[0031] The composition of the plating layer and the composition of the intermetallic compound crystals contained in the plating layer are the same as those of the electrode for electrolytic plating of the present invention. The composition of the plating layer is Cu 5~85% by mass, Cr 0.001~1% by mass, Ni 0.01~5% by mass, The balance is Sn (however, it may contain unavoidable impurities of 0.1 mass % or less). The composition of the intermetallic compound crystal is as follows: Sn 50~70% by mass, Cu 30~50% by mass, Cr 0.001~3% by mass, Ni 0.01~6.5% by mass It is. The amount of intermetallic compound crystals contained in the plating layer is, for example, 20 to 60 mass%. The composition of the parent phase is also the same as that of the electrolytic plating electrode of the present invention. That is, the composition of the parent phase is 5 mass% or less of Cu, 1 mass% or less of Ni, 1 mass% or less of Cr, and the balance is Sn (however, inevitable impurities may be contained in an amount of 0.1 mass% or less). The above-mentioned composition and structure of the entire plating layer, the parent phase and the intermetallic compound can be formed under the above-mentioned plating conditions using the electrolytic plating electrode of the present invention.

[0032] The plated substrate is then heat-treated. The heat treatment conditions are, for example, a temperature of 200°C to 220°C in an inert gas atmosphere and a heating time of, for example, about 60 to 120 minutes. In particular, these heat treatment conditions cause the plating layer to have a concentration gradient in which the concentrations of Cu and Sn change from the substrate toward the terminal surface.

[0033] By the above operation, the metal contained in the base material (base material metal) diffuses into the plating layer, and Sn contained in the parent phase migrates, resulting in a concentration gradient in which the concentrations of the base material metal and Sn change from the base material toward the terminal surface. The plating layer has a thickness of, for example, 2 μm to 10 μm. Also, a Sn diffusion layer is formed in a range of 0.1 μm to 10 μm from the contact point between the base material and the plating layer toward the inside of the base material. The following description will be given taking the case where the base material metal is Cu as an example. Specifically, the plating layer preferably has at least a first region having a high Cu concentration and a low Sn concentration, and a second region having a lower Cu concentration and a higher Sn concentration than the first region, arranged in this order from the substrate surface toward the terminal surface (composition condition 1). The Sn diffusion layer preferably has a concentration gradient in which the Sn concentration decreases from the contact point between the substrate and plating layer toward the inside of the substrate. By having such a concentration gradient in the Sn concentration, the substrate is less likely to split vertically, and the Sn exhibits peeling, heat resistance, pressure resistance, chemical resistance, and pressure resistance. More specifically, it is preferable that a concentration gradient of Cu and Sn is formed in the plating layer from the substrate surface to the terminal surface, as shown in the following table. Note that the ranges other than the first and second regions in the table below can take any value so long as the above composition condition 1 is satisfied.

[0034] [Table 1]

[0035] The substrate may be aluminum, an aluminum alloy, copper, a copper alloy, or stainless steel, and may be selected from known materials without particular limitation. For example, copper alloys include brass and phosphor bronze. When the present invention is used as a microbump, it is preferable to use Si, Sic or GaN as the semiconductor substrate and to apply Ti / Cu plating as the underlayer. The present invention also provides a bump as another embodiment. The bump of the present invention has the same composition as the terminal of the present invention. That is, the bump of the present invention is formed by forming a plating layer on the surface of a base material, and the plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing Sn and a Sn-Cu alloy, and the plating layer has a concentration gradient in which the concentrations of Cu and Sn change from the base material toward the bump surface. The details of the plating layer of the bump of the present invention are the same as those of the plating layer of the terminal of the present invention, and the method of forming the plating layer on the bump surface is also the same as those of the terminal of the present invention, so detailed explanations will be omitted.

[0036] In the terminal and bump of the present invention, by adjusting the concentration gradient of the plating layer as described above, particularly by diffusing Cu into the terminal surface side of the plating layer, the Vickers hardness of the plating layer surface can be set to a range of 10 (Hv) to 500 (Hv). By having such hardness, there is an advantage that impact durability, abrasion durability, etc. can be improved. The range of the hardness is more preferably 150 to 400 Hv. The Vickers hardness is measured in accordance with JIS Z 2244-1:2020.

[0037] In addition, a titanium, nickel or nickel alloy layer can be formed on the undercoat of the plating layer to further improve heat resistance. Nickel alloys that contain one or two of iron, tin, zinc, copper, cobalt, phosphorus, silver, boron, etc. can be used. The thickness of this undercoat layer is preferably about 0.1 μm to 1.5 μm, for example. EXAMPLES

[0038] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. Example 1 The raw material had a composition of 8 mass % Cu, 1 mass % Cr, 1 mass % Ni, and the balance Sn, and was used to produce metal particles 1 having a diameter of about 3 to 50 μm by the production apparatus shown in FIG. In this case, the following conditions were adopted: A melting crucible was placed in a melting furnace 7, the above-mentioned raw materials were placed therein, and melted at 900° C. While maintaining that temperature, the molten metal was supplied from the nozzle 3 onto the dish-shaped rotating disk 4. The dish-shaped rotating disk 4 used was a dish-shaped disk having a diameter of 35 mm and a rotating disk thickness of 3 to 5 mm, and was rotated at 80,000 to 100,000 revolutions per minute. Granulation chamber 1: 9 x 10 -2 After reducing the pressure in the granulation chamber 1 using a vacuum chamber capable of reducing the pressure to about 1×10 Pa, nitrogen gas at 15 to 50° C. was supplied while simultaneously evacuating the gas. -1 Pa or less. The obtained metal powder 1 was used to prepare an electrode for electrolytic plating of the present invention. In this case, the following conditions were adopted: High frequency induction heating: 9×10 -2 A crucible for high-frequency melting was placed in a vacuum chamber capable of reducing the pressure to about Pa, and the metal particles 1 of the present invention were introduced into the crucible. While the pressure was reduced to about the above-mentioned reduced pressure level, high-frequency induction heating was performed on the metal particles 1 of the present invention, the heating temperature was raised to 900°C to melt the metal particles 1 of the present invention, and the temperature was maintained for 5 minutes. Cooling and solidification: Next, while nitrogen gas at 15 to 50°C was flowed into the tank for 10 minutes, the heating temperature of the raw material was set to about 400°C under atmospheric pressure, the mixture was poured into a mold, and then cooled and solidified at room temperature. The obtained material was rolled into a sheet, which was then fed into a cutter heated to 150° C. and cut into 1 cm to 3 cm squares to obtain the electrolytic plating electrode of Example 1, which was then placed in the following plating bath.

[0039] The obtained electrolytic plating electrode of Example 1 had a cross section as shown in Fig. 1. Fig. 2 is a cross-sectional SEM image of the obtained electrolytic plating electrode of Example 1, which confirmed that intermetallic compound crystals (dark color) containing Sn, Cu, Cr and Ni were present in a matrix phase (light color) containing Sn and a Sn-Cu alloy. Furthermore, elemental mapping analysis by EDS of a cross section of the electrolytic plating electrode revealed that the composition was 8 mass % Cu, 1 mass % Cr, 1 mass % Ni, and the balance Sn. It was also found that the electrolytic plating electrode of Example 1 had intermetallic compound crystals contained in the matrix, and at least a portion of the matrix and the intermetallic compound crystals were endotaxy bonded. The composition of the electrolytic plating electrode is as follows: Cu 5~85% by mass, Cr 0.001~1% by mass, Ni 0.01~5% by mass, The balance was Sn. In addition, the composition including the intermetallic compound crystal and the endotaxial joint portion is Sn 50~70% by mass, Cu 30~50% by mass, Cr 0.001~3% by mass, Ni 0.01~6.5% by mass It turned out to be. Moreover, the intermetallic compound crystals in the electrolytic plating electrode accounted for 30 to 35 mass %.

[0040] (Preparation of contact terminals) A phosphor bronze or brass plate (thickness: 0.30 mm) was used as the substrate (cathode). Electrolytic plating was carried out on the substrate under the following conditions using the electrolytic plating electrode of the present invention as the electrolytic plating electrode to obtain a plated sheet metal.

[0041] Plating bath composition (concentration per liter of water): Copper sulfate 180~250g / L Stannous sulfate 30~50g / L Sulfuric acid 80~120g / L In addition, a known reference electrode was used, and an appropriate amount of additive was added.

[0042] Plating temperature: 70℃ Current density: 3A / dm 2 Heat treatment temperature of the substrate after plating: 200℃ Heat treatment time of the substrate after plating: 300 seconds (in nitrogen atmosphere)

[0043] The composition of the resulting contact terminal was the same as that of the electrolytic plating electrode of the present invention.

[0044] The contact terminal thus obtained was heated under the following conditions. Heating temperature: 217℃ Cooking time: 60 minutes

[0045] In addition, the plating layer of the contact terminal was disassembled, and the concentrations of Cu and Sn in the direction from the substrate to the surface of the contact terminal were measured by EDS, with the results shown in Fig. 3 being obtained. Fig. 3A is a photograph of a cross section of the plating layer and substrate subjected to EDS analysis, with numbers 001-002 on the substrate side and numbers 003-006 from the substrate surface to the terminal side. Figs. 3B-G are diagrams showing the results of element mapping analysis by EDS of the contact terminal obtained in Example 1. The concentrations of Cu and Sn in each region, particularly the first region (region 003 in Fig. 3) and the second region (region 006 in Fig. 3), are as shown in Table 2 below.

[0046] [Table 2]

[0047] The Cu and Sn concentration measuring device is as follows. Measuring equipment name: JSM-IT300HR Manufacturer: JEOL Ltd. Measurement mode: ANALYTICAL SCANNING ELECTRON, MICROSCOPE

[0048] The durability of the contact terminal obtained in Example 1 was examined by the following experiment. <Durability test method> (180° bending test) A contact terminal using a brass plate as a base material was subjected to a 180-degree bending test, and the presence or absence of cracks in the plating layer was observed. The plating layer had a thickness of 5 μm. FIG. 5 is a micrograph showing the results of the 180-degree bending test of the contact terminal of Example 1 (a is a photograph of the entire contact terminal, and b is an enlarged photograph of the bent portion). As a result, no cracks were observed in the plating layer of the contact terminal of Example 1. (Surface crack test) The resulting contact terminal was punched from the back side and subjected to a surface crack test. Fig. 6 is a micrograph showing the results of the surface crack test of the contact terminal of Example 1. As a result, no surface cracks due to punching were confirmed in the plating layer of the contact terminal of Example 1. (Heat resistance test) The obtained contact terminal was left to stand at a temperature of 230°C for 500 hours, and the surface state of the plating layer was observed under a microscope. Fig. 7 is a micrograph showing the heat resistance test result of Example 1. No change was observed in the plating layer of the contact terminal of this Example 1 before and after the heat resistance test.

[0049] Comparative Example 1 Example 1 was repeated except that the electrolytic plating electrode in Example 1 was changed to tin metal, and the 180° C. bending test, surface crack test, and heat resistance test were carried out. 8 is a micrograph showing the results of a 180-degree bending test of the contact terminal of Comparative Example 1 (a is a photograph of the entire contact terminal, and b is a magnified photograph of the bent portion). As a result, in the 180-degree bending test, cracks occurred in the plating layer, and peeling occurred between the plating layer and the base material. 9 is a micrograph showing the results of the surface crack test of Comparative Example 1. As a result, surface cracks due to punching were confirmed in the plating layer of the contact terminal of Comparative Example 1. 10 is a micrograph showing the results of a heat resistance test of Comparative Example 1. As a result, it was confirmed that partial dissolution occurred in the plating layer of the contact terminal of Comparative Example 1 under heating conditions of being left standing at a temperature of 250°C for 500 hours.

[0050] Comparative Example 2 Example 1 was repeated except that the heating temperature for the obtained contact terminal was changed to 190° C., and the above-mentioned 180-degree bending test, surface crack test, and heat resistance test were carried out. As a result, in the 180-degree bending test, cracks occurred in the plating layer and peeling occurred between the plating layer and the base material. In the surface crack test, surface cracks due to punching were confirmed in the plating layer of the contact terminal. In the heat resistance test, it was confirmed that partial dissolution occurred in the plating layer of the contact terminal when it was left to stand at a temperature of 250°C for 500 hours. The plating layer did not have a concentration gradient in which the concentrations of the base metal and Sn changed from the base material toward the terminal surface.

[0051] Although the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited thereto, and it is obvious that a person skilled in the art can conceive of various modifications based on the basic technical ideas and teachings thereof. [Explanation of symbols]

[0052] 1 Granulation chamber 2 lid 3 Nozzles 4-plate rotating disc 5 Rotating disk support mechanism 6 Particle discharge pipe 7 Melting furnace 8 Mixed Gas Tank 9 Piping 10 Piping 11 Valve 12 Exhaust system 13 Valve 14 Exhaust system 15 Automatic Filter 16. Particle collection device

Claims

1. A terminal having a plating layer formed on a surface of a base material, the plating layer contains Cu and has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a matrix containing Sn and a Sn-Cu alloy; the plating layer has a concentration gradient in which the concentrations of the base metal and Sn change from the base material toward the terminal surface, The Vickers hardness of the surface of the plating layer is in the range of 10 (Hv) to 500 (Hv); Terminal.

2. 2. The terminal according to claim 1, wherein the base material has a Sn diffusion layer extending from a contact point between the base material and the plating layer toward the inside of the base material in a range of 0.1 μm to 10 μm.

3. The composition of the plating layer is Cu 5-85% by mass, Cr 0.001 to 1% by mass, Ni 0.01 to 5% by mass, The balance is Sn (however, inevitable impurities may be contained in an amount of 0.1% by mass or less). The terminal according to claim 1 .

4. The composition of the intermetallic compound crystal is Sn 50-70% by mass, Cu 30-50% by mass, Cr 0.001 to 3% by mass, Ni 0.01-6.5% by mass The terminal according to claim 1 ,

5. A bump having a plating layer formed on a surface of a base material, the plating layer contains Cu and has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a matrix containing Sn and a Sn-Cu alloy; the plating layer has a concentration gradient in which the concentrations of the base metal and Sn change from the base material toward the bump surface, The Vickers hardness of the surface of the plating layer is in the range of 10 (Hv) to 500 (Hv); bump.

6. 6. The bump according to claim 5, wherein the plating layer has a diffusion layer of the base metal in a range of 0.1 μm to 10 μm from the base material toward the bump surface.

Citation Information

Patent Citations

  • Sn plated copper alloy material for fitting connection terminal and fitting connection terminal

    JP2002298963A

  • Tin-copper intermetallic compound-dispersed tinned terminal

    JP2003082499A

  • Tin-plated copper terminal material with high insertability, and production method thereof

    JP2018115361A

  • Joint structure part

    JP2018144080A

  • Alloy Diffusion Barrier Layer

    JP2020534695A

Cited By

  • Metal substrate

    JP7883681B1