Conductive film and wound body thereof
By adjusting the difference in the surface free energy of the two surfaces of the conductive film substrate, the problem of the conductive film sticking to the wound body is solved, the yield and use stability are improved, and the conductivity and transparency are achieved.
Patent Information
- Application Number
- CN202080085135.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-10
- Filing Date
- 2020-12-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-12-09
AI Technical Summary
The conventional conductive film is prone to sticking problems in the winding body, especially when the conductive pattern is transferred to the back surface, resulting in poor adhesion of the conductive film and a decrease in yield.
By adjusting the difference in the free energy of the two surfaces of the substrate, we ensure that the conductive part has a high adhesion and mold release property with one side. Specific measures include adding a silicon compound layer as the outermost layer on one side and using melamine-based compounds on the other side. Materials such as alkyd compounds, fluorine compounds and silicone compounds are used as the outermost layer to control surface free energy and prevent conductive parts from adhering to the back surface.
It effectively suppresses the adhesion of the conductive film, improves the yield of the conductive film and the stability during use, and avoids the occurrence of defective products caused by the adhesion of the conductive portion on the back.
Smart Images

Figure CN114868209B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive film and a wound body thereof. Background Art
[0002] In the past, electronic devices such as electronic paper, touch panels, and flat panel displays used transparent conductive films using indium tin oxide (hereinafter referred to as "ITO"). In the future, in order to further increase the added value of electronic devices, it is important to increase the area, improve responsiveness, and make them flexible. Therefore, the conductive films used for this purpose are required to maintain high transmittance while improving conductivity and flexibility.
[0003] ITO has low inherent conductivity, so in order to show high conductivity, it needs to be thickened, which reduces transmittance. In addition, due to thickening, cracks are easily generated due to deformation such as bending, flexing, and bending. Therefore, when using a conductive film using ITO, it is difficult to show high transmittance, conductivity, and flexibility at the same time.
[0004] Therefore, research and development of conductive films that can replace ITO are vigorously conducted, and conductive films having metal fine wires patterned on a transparent substrate have attracted attention, and various studies have been conducted.
[0005] For example, Patent Document 1 discloses that the crystallite diameter of a metal fine particle sintered film measured by X-ray diffraction and the porosity of a cross section of the metal fine particle sintered film are specified in order to improve the adhesion and conductivity of the metal fine particle sintered film to a substrate.
[0006] In addition, Patent Document 2 discloses a method of providing a thickness adjustment pattern on a portion of a support body where no functional pattern is formed in order to suppress the concentration of pressure on the functional pattern during superposition. Furthermore, Patent Document 3 discloses a reverse offset printing apparatus for electronic materials.
[0007] In addition, Patent Document 4 discloses a conductive film having excellent adhesion between a conductive layer and a hard coating layer and excellent conductivity, and the surface free energy of the hard coating layer forming the conductive layer is specified in order to prevent sticking when the film is wound up and to improve the poor adhesion between the conductive layer and the hard coating layer.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2010-192841
[0011] Patent Document 2: Japanese Patent Application Publication No. 2016-51194
[0012] Patent Document 3: Japanese Patent Application No. 2015-523244
[0013] Patent Document 4: Japanese Patent Application Publication No. 2017-019273 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] However, the conductive film obtained as described above is wound up into a roll after manufacturing, and is stored and circulated. In addition, after the roll is unwound, various treatments such as stacking multiple sheets for storage are also considered. However, it is known that when the conductive part such as the metal fine wire formed on the surface of the conductive film like the roll contacts with other components, such as the back side of the conductive film, a part of the conductive part formed on the surface is transferred to the back side, and there is a problem of peeling.
[0016] This problem becomes particularly prominent when the conductive film is manufactured by a continuous process as in Patent Document 2, and an offset phenomenon easily occurs in which the conductive pattern is transferred to the back side of the film in contact with the conductive pattern in the wound body of the conductive film.
[0017] In addition, in Patent Document 4, in order to prevent the film from sticking when winding, the poor adhesion between the conductive layer and the hard coating layer is improved, but the conductive layer in Patent Document 4 refers to a layer containing a conductive material formed on the hard coating layer, which is a transparent conductive layer containing a resin binder and is a uniform layer. Therefore, it cannot be applied to a conductive layer composed of a fine line pattern, and there is a problem that a part of the fine line pattern formed on the surface is transferred to the back surface.
[0018] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a conductive film having a fine line pattern and capable of suppressing offset, and a wound body of the conductive film.
[0019] Solutions for solving problems
[0020] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by adjusting the surface free energy of both surfaces of a substrate, thereby completing the present invention.
[0021] That is, the present invention is as follows.
[0022] [1] A conductive film comprising a substrate and a conductive portion including at least a fine line pattern formed on a first surface of the substrate,
[0023] The surface free energy SFE1 of the first surface is larger than the surface free energy SFE2 of the second surface of the substrate which is opposite to the first surface.
[0024] [2] The conductive film according to [1], wherein the difference between the surface free energy SFE1 and the surface free energy SFE2 (SFE1-SFE2) is 1 mJ / m 2 above.
[0025] [3] The conductive film according to [1] or [2], wherein the surface free energy SFE1 is 40 to 50 mJ / m 2 .
[0026] [4] The conductive film according to any one of [1] to [3], wherein the substrate has a layer containing a silicon compound as an outermost layer on the first surface side.
[0027] [5] The conductive film according to any one of [1] to [4], wherein the surface free energy SFE2 is 11 to 42 mJ / m 2 .
[0028] [6] The conductive film according to any one of [1] to [5], wherein the substrate has a layer containing at least one selected from the group consisting of melamine compounds, alkyd compounds, fluorine compounds and siloxane compounds as the outermost layer on the second surface side.
[0029] [7] A wound body, which is the wound body of the conductive film according to any one of [1] to [6], wherein the wound body is wound so that the conductive portion is in contact with the second surface.
[0030] [8] The wound body according to [7], wherein the conductive film is a long film having a short side of 10 mm to 2000 mm and a long side of 1.0 m to 2000 m,
[0031] The wound body is formed by winding the conductive film in the longitudinal direction.
[0032] Effects of the Invention
[0033] According to the present invention, a conductive film having a fine line pattern and capable of suppressing offset, and a wound body of the conductive film can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic cross-sectional view showing one form of the conductive thin film according to the present embodiment.
[0035] Figure 2 It is a schematic perspective view showing one mode of the wound body of the conductive film according to the present embodiment.
[0036] Figure 3 It is a plan view showing one form of the conductive thin film according to the present embodiment.
[0037] Figure 4 for Figure 3 Partial cross-sectional view of the conductive film taken along line II'.
[0038] Figure 5 It is a partial plan view showing the relationship between the aperture ratio and the pitch of the conductive film.
[0039] Figure 6 It is a schematic diagram showing the method for producing the conductive thin film according to the present embodiment.
[0040] Figure 7 The photographs show the offset results of the conductive film of the example.
[0041] Figure 8 The photographs show the offset results of the conductive film of the comparative example. DETAILED DESCRIPTION
[0042] An embodiment of the present invention (hereinafter referred to as “this embodiment”) will be described in detail below, but the present invention is not limited thereto and various modifications can be made without departing from the gist of the invention.
[0043] [Conductive film]
[0044] The conductive film of this embodiment includes a substrate and a conductive portion including at least a fine line pattern formed on a first surface of the substrate, wherein the surface free energy SFE1 of the first surface is larger than the surface free energy SFE2 of a second surface of the substrate opposite to the first surface.
[0045] Figure 1 A schematic cross-sectional view of one embodiment of the conductive film of the present embodiment is shown. The conductive film 100 of the present embodiment includes a substrate 10 and a conductive portion 20. The substrate 10 may be a single-layer film or a laminated film. Figure 1 2 shows an example in which the substrate 10 is a laminated film. Figure 1 The substrate 10 shown includes a core layer 11 , an outermost layer 12 on the first surface 10 a side, and an outermost layer 13 on the second surface 10 b side.
[0046] The conductive portion 20 is formed on the first surface 10a. Figure 1 As shown, the conductive portion 20 includes at least a pattern composed of fine lines and may partially include a uniform metal layer.
[0047] To explain the sticking, Figure 2 FIG. 2 shows a wound body 200 of the conductive film 100. It should be noted that Figure 2 In order to facilitate the description, a schematic diagram of the occurrence of sticking is shown, but in fact, for the winding body 200 of this embodiment, Figure 2The sticking as shown is suppressed.
[0048] Figure 2 The figure shows a winding body 200 in which the conductive film 100 is wound in such a manner that the first surface 10a faces inward and the second surface 10b faces outward. This winding body 200 is sometimes formed by winding a conductive film 100 of a length of even 2000 m as required. Therefore, a corresponding load is applied between the conductive films of the winding body 200, and the conductive portion 20 is in close contact with the second surface 10b. The conductive portion 20 partially adheres to the second surface 10b due to the close contact between the conductive portion 20 and the second surface 10b, which is called sticking. If such sticking occurs, the conductive portion may be broken, defective products may be produced due to the adhesion of the conductive material to the unnecessary surface (the second surface 10b), etc.
[0049] In contrast, the conductive film 100 of the present embodiment ensures the adhesion of the conductive part to the first surface 10a and the releasability of the conductive part to the second surface 10b by making the surface free energy SFE1 of the surface (first surface 10a) of the substrate greater than the surface free energy SFE2 of the back surface (second surface 10b). Thus, even if the conductive films 100 are overlapped and the conductive part contacts the second surface 10b during storage, distribution, or use of the conductive film 100, the conductive part can be prevented from adhering to the second surface 10b (sticking).
[0050] In particular, the conductive portion 20 in the conductive film 100 of the present embodiment includes a fine line pattern. Compared with the conductive layer of a uniform film, the fine line pattern tends to be easily stained when the conductive films 100 are overlapped with each other and the conductive portion 20 is in contact with the second surface 10b. This is because staining is a phenomenon in which the layer of the conductive portion 20 is destroyed due to adhesion to the second surface 10b. In order to suppress this phenomenon, in addition to the adhesion with the first surface 10a, the strength of the conductive portion layer itself is also required. Therefore, in the case where the conductive layer is a uniform full film, staining is suppressed by the strength of the entire film. On the other hand, Figure 1 In the case of the metal fine wire pattern shown, the above-mentioned offset suppression mechanism by film strength does not function due to the fineness of the fine wires of the conductive portion 20 .
[0051] For the above reasons, in order to prevent the conductive film including a fine line pattern from being fouled, it is necessary to control the adhesion between not only the conductive portion 20 and the first surface 10a but also the second surface 10b to ensure mold release properties.
[0052] From the above viewpoint, the difference in surface free energy SFE2 (SFE1-SFE2) is preferably 1 mJ / m 2 More preferably 5mJ / m 2More preferably 10 mJ / m 2 Above, particularly preferably 16 mJ / m 2 Above, most preferably 20mJ / m 2 Above. The difference (SFE1-SFE2) is 1mJ / m 2 As a result, the sticking is further suppressed, and there is a tendency that the yield of the conductive film is further improved. In addition, there is no particular restriction on the upper limit of the difference (SFE1-SFE2) of the surface free energy SFE2, but it is preferably 100 mJ / m 2 Below, more preferably 40mJ / m 2 By doing so, the adhesiveness of the first surface 10a is excessively increased, and contamination by dust or the like can be suppressed.
[0053] From the same viewpoint, the surface free energy SFE1 is preferably 20 to 100 mJ / m 2 , more preferably 20 to 75 mJ / m 2 , more preferably 20 to 50 mJ / m 2 Surface free energy SFE1 is 40mJ / m 2 As described above, there is a tendency that the adhesion of the conductive portion 20 to the first surface 10a is further improved. 2 There is a tendency that contamination by dust etc. is further suppressed. The surface free energy SFE1 can be adjusted by the material of the outermost layer 12 when the substrate 10 has the outermost layer 12, and can be adjusted by the material of the core layer 11 when the substrate 10 does not have the outermost layer 12. In addition, it can also be adjusted by the surface roughness of the first surface 10a.
[0054] If the surface roughness (arithmetic mean roughness Ra1) of the first surface 10a is greater than 0.1nm and less than 20nm, the above-mentioned range of surface free energy SFE1 can be maintained, so it is preferred. If it is greater than 0.2nm and less than 10nm, the defects of the fine line pattern formed on the first surface 10a can be suppressed, so it is preferred. It is more preferably greater than 0.3nm and less than 5nm.
[0055] Furthermore, from the same viewpoint, the surface free energy SFE2 is preferably 5 to 42 mJ / m 2 , more preferably 11 to 42 mJ / m 2 , more preferably 11 to 30 mJ / m 2 , particularly preferably 11 to 25 mJ / m 2 Surface free energy SFE2 is 5mJ / m 2As described above, there is a tendency to improve the ease of processing when the second surface 10b is further coated with other layers or the second surface 10b is bonded to the surface of other components. Furthermore, when the surface free energy SFE2 is low, there is a tendency for the friction coefficient of the second surface 10b to decrease. In contrast, when the surface free energy SFE2 is 5 mJ / m 2 As described above, when the conductive film 100 or the substrate 10 is transported by a conveying device such as a roller during manufacturing, the slip between the conveying device and the second surface 10b can be suppressed, and there is a tendency that the tension control of the conductive film 100 or the substrate 10 becomes easy by the conveying device. In particular, in the printing method of forming the metal fine wire 21 on the surface of the substrate 10 while conveying the substrate 10, such tension control is required. In addition, the surface free energy SFE2 is 42mJ / m 2 The following further suppresses the sticking, and there is a tendency that the yield of the conductive film is further improved. The surface free energy SFE2 can be adjusted by the material of the outermost layer 13 when the substrate 10 has the outermost layer 13, and can be adjusted by the material of the core layer 11 when the substrate 10 does not have the outermost layer 13. In addition, it can also be adjusted by the surface roughness of the second surface 10b.
[0056] If the surface roughness (arithmetic mean roughness Ra2) of the second surface 10b is greater than 0.1nm and less than 20nm, the above-mentioned range of surface free energy SFE2 can be maintained, so it is preferred. If it is greater than 0.2nm and less than 10nm, when the conductive film 100 is wound, defects when the fine line pattern formed on the first surface 10a is overlapped with the second surface 10b can be suppressed, so it is preferred. It is further preferred to be greater than 0.3nm and less than 5nm.
[0057] The surface roughness of the first surface 10a and the second surface 10b, respectively, preferably have arithmetic mean roughness Ra1 and Ra2 satisfying the following formula (5). If formula (5) is satisfied, when the conductive film 100 is wound, it is possible to suppress defects when the fine line pattern formed on the first surface 10a overlaps with the second surface 10b, and therefore it is preferred.
[0058] Ra1≥Ra2 (5)
[0059] The detailed mechanism by which the defects during winding can be suppressed by satisfying equation (5) is not clear, but it is presumed as follows. That is, when the conductive film 100 is wound, the winding is tightened due to the winding tension, and the first surface 10a and the second surface 10b of the overlapped film are slightly offset and rubbed. At this time, the fine line pattern formed on the first surface 10a is defective due to the unevenness of the second surface 10b.
[0060] In addition, the difference between the surface roughness of the first surface 10a and the surface roughness of the second surface 10b is preferably small, and the absolute value of the difference between their respective arithmetic mean roughness Ra |Ra1-Ra2| is preferably 3nm or less. If it is 2nm or less, the defect suppression effect becomes significant and it is preferred, and more preferably 1nm or less.
[0061] Next, the surface free energy defined by this embodiment is described. Generally, the molecules present inside the resin exist in a state stabilized by the interaction with the surrounding molecules, but the molecules present on the surface of the resin are formed on the surface, so the stabilization effect achieved by the surrounding molecules is small. Therefore, the molecules present on the surface have a larger free energy than the molecules present inside. This energy is called surface free energy.
[0062] According to the theoretical formula of Kaelbel and Uy, the surface free energy γ of the material surface is based on the dispersion component (γ d ) and polar component (γ p ) can be represented by the following formula (1). In addition, the surface free energy γ of the solid SV and the surface free energy of the liquid γ LV It can be represented by the following formulas (2) and (3). It is known that if the contact angle obtained by dropping a certain solvent on the surface of a solid substrate is θ, the relationship of the following formula (4) holds.
[0063] γ=γ d +γ p (1)
[0064] γ SV =γ SV d +γ SV p (2)
[0065] γ LV =γ LV d +γ LV p (3)
[0066] γ L (1+cosθ) / 2=(γ SV d ×γ LV d ) 0.5 +(γ SV p ×γ LV p ) 0.5 (4)
[0067] In order to find the two unknown components in the surface free energy of the solid, two liquids with known surface free energy are used to measure the contact angle θ between the solvent and the first surface 10a or the second surface 10b. Then, these are substituted into the above equation (4) to solve the simultaneous equations, thereby finding the dispersion component (γ) of the surface free energy of the first surface 10a or the second surface 10b. SV d ) and polar component (γ SV p ), the surface free energy γ of the solid can be obtained by equation (2): SV .
[0068] [Base material]
[0069] There is no particular limitation on the substrate used in this embodiment, and for example, a transparent substrate or an opaque substrate can be used. Here, "transparent" means that the visible light transmittance is preferably 80% or more, more preferably 90% or more, and further preferably 95% or more. Here, the visible light transmittance can be measured according to JIS K 7361-1:1997. In addition, an opaque substrate refers to a substrate with a visible light transmittance of less than 80%, and an opaque substrate also includes a substrate that is completely non-transparent to a semi-transparent substrate that partially transmits visible light. It should be noted that, among them, the substrate is preferably a transparent substrate.
[0070] The substrate can be formed by one material or by stacking two or more materials. In addition, when the substrate is a laminate formed by stacking two or more materials, the substrate can be an organic substrate or an inorganic substrate stacked on each other, or an organic substrate and an inorganic substrate stacked on each other.
[0071] Figure 1 The substrate 10 including the core layer 11, the outermost layer 12 constituting the first surface 10a, and the outermost layer 13 constituting the second surface 10b is exemplified, but the structure of the substrate 10 is not limited thereto. As the form of the substrate 10, a single-layer film having the core layer 11, a laminated film having the core layer 11 and the outermost layer 12, a laminated film having the core layer 11 and the outermost layer 13, a laminated film having the outermost layer 12 and the outermost layer 13, and a laminated film having the core layer 11, the outermost layer 12, and the outermost layer 13 can be listed. In addition, in the above-mentioned laminated film, other layers may be further included between the core layer 11 and the outermost layer 12, between the core layer 11 and the outermost layer 13, or between the outermost layer 12 and the outermost layer 13. It should be noted that, in a laminated film having a core layer 11 and an outermost layer 12, the surface of the core layer 11 constitutes a first surface 10a, and in a laminated film having a core layer 11 and an outermost layer 13, the surface of the core layer 11 constitutes a second surface 10b. The structure of each layer is described in detail below.
[0072] (Core layer 11)
[0073] The material constituting the core layer 11 is not particularly limited, but is preferably a material that contributes to improving the mechanical strength of the base material.
[0074] The material of the core layer 11 is not particularly limited, and examples thereof include transparent inorganic substrates such as glass; transparent organic substrates such as acrylates, methacrylates, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyarylate, polyvinyl chloride, polyethylene, polypropylene, polystyrene, nylon, aromatic polyamide, polyetheretherketone, polysulfone, polyethersulfone, polyimide, and polyetherimide. Among them, by using polyethylene terephthalate, the productivity (cost reduction effect) for manufacturing the conductive film is better. In addition, by using polyimide, the heat resistance of the conductive film is better. Furthermore, by using polyethylene terephthalate and / or polyethylene naphthalate, the adhesion between the transparent substrate and the metal fine wire is better.
[0075] The core layer 11 may be formed of one material or may be formed by stacking two or more materials. In addition, when the core layer 11 is a laminated body formed by stacking two or more materials, the substrate may be an organic substrate or an inorganic substrate stacked on each other, or may be an organic substrate and an inorganic substrate stacked on each other.
[0076] The thickness of the core layer 11 is preferably 5 μm or more and 500 μm or less, and more preferably 10 μm or more and 100 μm or less.
[0077] (Outermost layer 12)
[0078] When the substrate 10 is a laminate, the outermost layer 12 is a layer constituting the first surface 10a. There is no particular limitation on the material of the outermost layer 12 constituting the first surface side, but it is preferably a material that helps improve the adhesion between the core layer 11 and the conductive portion 20. In addition, when the substrate 10 has the outermost layer 12 and the outermost layer 13 and does not have the core layer 11, the outermost layer 12 is preferably a material that helps improve the adhesion between the outermost layer 13 and the conductive portion 20. It should be noted that when the substrate 10 has the outermost layer 12, the surface free energy SFE1 is the surface free energy of the outermost layer 12.
[0079] The components contained in the outermost layer 12 are not particularly limited, and examples thereof include silicon compounds (e.g., (poly)silanes, (poly)silazines, (poly)silthiones, (poly)siloxanes, silicon, silicon carbide, silicon oxide, silicon nitride, silicon chloride, silicates, zeolites, silicides, etc.), aluminum compounds (e.g., aluminum oxide, etc.), magnesium compounds (e.g., magnesium fluoride), etc.
[0080] Among them, silicon compounds are preferred, and siloxanes are more preferred. By using such a component, the surface free energy of the first surface 10a is improved, the above-mentioned adhesion is improved, and in addition, there is a tendency that the transparency and durability of the conductive film are further improved.
[0081] The silicon compound is not particularly limited, and examples thereof include condensates of polyfunctional organosilanes, and polycondensates obtained by a hydrolysis reaction of polyfunctional organosilanes or oligomers thereof with polyvinyl acetate.
[0082] There are no particular restrictions on the polyfunctional organosilanes, and examples thereof include bifunctional organosilanes such as dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diphenyldimethoxysilane, and diphenyldiethoxysilane; trifunctional organosilanes such as methyltrimethoxysilane, methyltriethoxysilane, and phenyltrimethoxysilane; and quadrifunctional organosilanes such as tetramethoxysilane and tetraethoxysilane.
[0083] The outermost layer 12 can be formed by applying a composition containing the components contained in the outermost layer 12 to the core layer 11 and drying it. In addition, the outermost layer 12 can also be formed by a vapor phase film forming method such as PVD and CVD. The composition used to form the outermost layer 12 can contain a dispersant, a surfactant, a binder, etc. as needed.
[0084] The thickness of the outermost layer 12 is preferably 0.01 μm to 100 μm, more preferably 0.01 μm to 10 μm, and further preferably 0.01 μm to 1 μm. When the thickness of the outermost layer 12 is within the above range, the above-mentioned adhesion is further improved, and there is also a tendency that the transparency and durability of the conductive film are further improved.
[0085] When the outermost layer 12 is stacked on the core layer 11 and the metal component in the ink is sintered by plasma or other sintering means to form the conductive portion 20, etching of the core layer 11 in areas not covered by the conductive portion 20 due to plasma or other means can be prevented.
[0086] Furthermore, the outermost layer 12 preferably has an antistatic function in order to prevent disconnection of the metal fine wire pattern (conductive portion 20) due to static electricity. In order for the outermost layer 12 to have an antistatic function, the outermost layer 12 preferably contains at least one of a conductive inorganic oxide and a conductive organic compound.
[0087] Examples of the conductive organic compound include conductive organosilane compounds, aliphatic conjugated polyacetylene, aromatic conjugated poly(p-phenylene), heterocyclic conjugated polypyrrole, etc. Among them, conductive organosilane compounds are preferred.
[0088] Furthermore, for the purpose of antistatic function, the volume resistivity of the outermost layer 12 is preferably 100 Ωcm or more and 100,000 Ωcm or less, more preferably 1000 Ωcm or more and 10,000 Ωcm or less, and even more preferably 2000 Ωcm or more and 8000 Ωcm or less. By having a volume resistivity of the outermost layer 12 of 100,000 Ωcm or less, an antistatic function can be exhibited. In addition, by having a volume resistivity of the outermost layer 12 of 100 Ωcm or more, it can be suitably used for applications such as touch panels where conductivity between metal fine wire patterns is not preferred. The volume resistivity can be adjusted by the content of components that exert antistatic function, such as conductive inorganic oxides and conductive organic compounds in the outermost layer. For example, the outermost layer 12 contains silicon oxide (volume resistivity 10 14 Ω·cm or more) and an organosilane compound as a conductive organic compound, the volume resistivity can be reduced by increasing the content of the conductive organosilane compound. On the other hand, by increasing the content of silicon oxide, the volume resistivity increases, but it has high plasma resistance, so a thin film can be formed without impairing the optical properties.
[0089] The outermost layer 12 can be formed by a vapor phase film forming method such as PVD or CVD, or by applying an outermost layer forming composition in which the components contained in the outermost layer 12 are dispersed in a dispersion medium and drying the composition. The outermost layer forming composition can contain a dispersant, a surfactant, a binder, etc. as required.
[0090] (Outermost layer 13)
[0091] When the substrate 10 is a laminate, the outermost layer 13 is a layer constituting the second surface 10b. There is no particular limitation on the material of the outermost layer 13 constituting the second surface side, and it is preferably a material that helps reduce the adhesion to the conductive portion 20. It should be noted that when the substrate 10 has the outermost layer 13, the surface free energy SFE2 is the surface free energy of the outermost layer 13.
[0092] As the components contained in this outermost layer 13, there is no particular limitation, and examples thereof include melamine compounds, alkyd compounds, fluorine compounds, silicone compounds, polyethylene wax, fatty acids, and fatty acid esters. Among them, preferably at least one selected from the group consisting of melamine compounds, alkyd compounds, fluorine compounds, and silicone compounds, more preferably melamine compounds and alkyd compounds. By using such a component, the surface free energy of the second surface 10b is reduced and the demoulding property of the conductive part is improved. In addition, there is a tendency to further improve the transparency and durability of the conductive film.
[0093] The melamine compound is not particularly limited, and examples thereof include melamine, methylolated melamine derivatives obtained by condensation of melamine and formaldehyde, and compounds partially or completely etherified by reacting methylolated melamine derivatives with lower alcohols.
[0094] The methylolated melamine derivative is not particularly limited, and examples thereof include monomethylolmelamine, dimethylolmelamine, trimethylolmelamine, tetramethylolmelamine, pentamethylolmelamine, hexamethylolmelamine, and hexamethoxymethylolmelamine.
[0095] The lower alcohol constituting the melamine compound is not particularly limited, and examples thereof include methanol, ethanol, isopropanol, n-butanol, and isobutanol.
[0096] Examples of the alkyd compound include ester polymers of polybasic acids, fatty acids, and polyhydric alcohols.
[0097] The polybasic acid constituting the alkyd compound is not particularly limited, and examples thereof include phthalic anhydride, isophthalic acid, terephthalic acid, benzoic acid, rosin, tetrahydrophthalic anhydride, maleic anhydride, adipic acid, and succinic acid.
[0098] There are no particular restrictions on the fatty acids constituting the alkyd compound, and examples thereof include saturated fatty acids such as caproic acid, caprylic acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, and melissic acid; and unsaturated fatty acids such as oleic acid, elaidic acid, linoleic acid, linolenic acid, arachidonic acid, brassidic acid, erucic acid, and ricinoleic acid; linseed oil, soybean oil, castor seed oil, and the like.
[0099] The polyol constituting the alkyd compound is not particularly limited, and examples thereof include glycerin, pentaerythritol, ethylene glycol, propylene glycol, neopentyl glycol, and trimethylolpropane.
[0100] The fluorine-based compound is not particularly limited, and examples thereof include compounds containing a polyfluoroalkyl group or a polyfluoroalkyl ether group having 3 to 40 carbon atoms, particularly 5 to 20 carbon atoms.
[0101] The siloxane-based compound is not particularly limited, and examples thereof include silicone oils containing polydimethylsiloxane, phenyl-modified silicone oils in which a part of the methyl groups of polydimethylsiloxane are replaced with phenyl groups, alkyl-modified silicone oils in which a part of the methyl groups of polydimethylsiloxane are replaced with hydrogen or an alkyl group having 2 or more carbon atoms, halogen-modified silicone oils in which a part of the methyl groups of polydimethylsiloxane are replaced with halogenated phenyl groups, fluorine-modified silicone oils in which a part of the methyl groups of polydimethylsiloxane are replaced with fluoroester groups, epoxy-modified silicone oils such as polydimethylsiloxane having an epoxy group, amino-modified silicone oils such as polydimethylsiloxane having an amino group, alkylaralkyl silicone oils such as dimethylsiloxane and phenylmethylsiloxane, and polyether-modified silicone oils such as polydimethylsiloxane having a structure in which a part of the methyl groups of the dimethylsiloxane unit are replaced with polyethers.
[0102] As fatty acids, saturated or unsaturated fatty acids having 12 or more carbon atoms can be cited. Examples of fatty acids include lauric acid, tridecanoic acid, myristic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, stearic acid, nonadecanoic acid, behenic acid, lignoceric acid, cerotic acid, heptadecanoic acid, montanic acid, melissic acid, lacquer acid, oleic acid, elaidic acid, linoleic acid, linolenic acid, arachidonic acid, cetyl oleic acid, erucic acid, etc. As fatty acids, saturated fatty acids having 12 to 22 carbon atoms are preferred.
[0103] The fatty acid ester is not particularly limited, and examples thereof include fatty acid esters of the above-mentioned fatty acids and alcohols having 2 to 30 carbon atoms. The alcohol constituting the fatty acid ester is not particularly limited, and examples thereof include monohydric alcohols such as propanol, isopropanol, butanol, octyl alcohol, capryl alcohol, lauryl alcohol, myristyl alcohol, stearyl alcohol, and behenyl alcohol, and polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, glycerin, pentaerythritol, and sorbitan.
[0104] The polyethylene wax is not particularly limited, and examples thereof include low molecular weight polyethylene, low molecular weight polyethylene copolymers, and modified polyethylene waxes obtained by introducing polar groups therein through oxidation modification or acid modification.
[0105] The thickness of the outermost layer 13 is preferably 0.01 μm to 100 μm, more preferably 0.01 μm to 10 μm, and further preferably 0.01 μm to 1 μm. When the thickness of the outermost layer 13 is within the above range, the demolding property of the conductive portion 20 is improved, and there is also a tendency that the transparency and durability of the conductive film 100 are further improved.
[0106] (Other layers)
[0107] The other layer disposed between the core layer 11 and the outermost layer 12 , between the core layer 11 and the outermost layer 13 , or between the outermost layer 12 and the outermost layer 13 is not particularly limited, and examples thereof include an easy-adhesion layer.
[0108] The easy bonding layer is used to improve the adhesion between the core layer 11 and the outermost layer 12, the core layer 11 and the outermost layer 13, or the outermost layer 12 and the outermost layer 13. In addition, the easy bonding layer used between the core layer 11 and the outermost layer 13 can be used to improve the surface roughness of the outermost layer 13. That is, the surface roughness of the outermost layer 13 can be improved by increasing the surface roughness of the easy bonding layer that becomes the base. Thus, there is a tendency to further improve the demoulding property of the conductive portion 20.
[0109] [Conductive portion 20]
[0110] The conductive portion 20 is disposed on the first surface 10 a of the substrate 10 . Figure 1 In the figure, the conductive part 20 is shown as a metal fine line pattern composed of metal fine lines, but the conductive part 20 is not limited thereto and at least contains a fine line pattern, and a part thereof may be a metal pattern of the entire surface. In addition, the metal fine line pattern may be a regular pattern or an irregular pattern.
[0111] The conductive part 20 contains a conductive component. There is no particular restriction on the conductive component, and examples thereof include conductive metals and conductive polymers. In addition, the conductive part 20 may contain a non-conductive component. There is no particular restriction on the conductive metal, and examples thereof include gold, silver, copper, and aluminum. Among them, silver or copper is preferred, and relatively inexpensive copper is more preferred. By using such a conductive metal, there is a tendency that the conductivity of the conductive film is further improved. In addition, as the conductive polymer, a known conductive polymer can be used, and examples thereof include polyacetylene, polythiophene, and the like.
[0112] In addition, the non-conductive component is not particularly limited, and examples thereof include metal oxides, metal compounds, and organic compounds. More specifically, these non-conductive components include metal oxides, metal compounds, and organic compounds that are components derived from components contained in the ink described later and that remain in the metal thin wires after firing.
[0113] The content ratio of the conductive component in the conductive portion 20 is preferably 50% by mass or more, more preferably 60% by mass or more, and further preferably 70% by mass or more. The upper limit of the content ratio of the conductive component is not particularly limited, and is 100% by mass. In addition, the content ratio of the non-conductive component is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. The lower limit of the content ratio of the non-conductive component is not particularly limited, and is 0% by mass.
[0114] The metal fine wire pattern of the conductive portion 20 can be designed according to the purpose of the electronic device, and is not particularly limited. For example, a mesh pattern ( Figure 3 (a) and (b)), a line pattern formed by a plurality of substantially parallel metal thin wires ( Figure 3 (c) and (d)). In addition, the metal fine line pattern may be a combination of a grid pattern and a line pattern. The mesh of the grid pattern may be Figure 3 A square or rectangle as shown in (a), or Figure 3 In addition, the metal fine wires constituting the line pattern may be Figure 3 A straight line such as that shown in (c) or Figure 3 Furthermore, even for the metal thin wires constituting the mesh pattern, the metal thin wires can be formed into a curve.
[0115] The line width W of the thin metal wire 21 refers to the line width W0 of the thin metal wire 21 when the thin metal wire 21 is projected onto the surface of the substrate 10 from the side of the substrate 10 on which the conductive portion 20 is arranged. Figure 4 Shown in Figure 3 Partial cross-sectional view of the conductive film I-I'. Figure 4 As an example, in the case of the metal thin wire 21 having a trapezoidal cross section, the width of the surface of the metal thin wire 21 in contact with the substrate 10 is the line width W0.
[0116] The line width W0 of the metal fine wire 21 is preferably 0.1 to 30.0 μm, more preferably 0.2 to 20.0 μm, further preferably 0.3 to 10.0 μm, and particularly preferably 1.0 to 5.0 μm. When the line width W0 of the metal fine wire 21 is 0.1 μm or more, there is a tendency for the conductivity of the conductive portion 20 to be further improved. In addition, the reduction in conductivity caused by oxidation, corrosion, etc. on the surface of the metal fine wire 21 can be fully suppressed. Furthermore, when the aperture ratio is kept the same, the thinner the line width of the metal fine wire 21, the more the number of metal fine wires 21 can be increased. As a result, the electric field distribution of the conductive film 100 becomes more uniform, and higher-resolution electronic devices can be manufactured. In addition, even if a part of the metal fine wire 21 is broken, other metal fine wires 21 can also compensate for the impact caused by the break. On the other hand, when the line width W0 of the thin metal wires 21 is 30.0 μm or less, the visibility of the thin metal wires 21 is further reduced, and there is a tendency that the transparency of the conductive film 100 is further improved.
[0117] The thickness T of the metal fine wire 21 is preferably 10 to 1000 nm, more preferably 50 to 700 nm, and further preferably 75 to 500 nm. When the thickness T of the metal fine wire 21 is 10 nm or more, there is a tendency for the conductivity to be further improved. In addition, the reduction in conductivity caused by oxidation, corrosion, etc. on the surface of the metal fine wire 21 can be fully suppressed. On the other hand, when the thickness T of the metal fine wire 21 is 1000 nm or less, there is a tendency for high transparency to be exhibited at a wide viewing angle.
[0118] In addition, the cross-sectional shape of the metal fine wire 21 can be determined by the wire width W and thickness T of the metal fine wire. The thickness T of the metal fine wire 21 is used as a reference, and the height from the interface between the substrate 10 and the metal fine wire 21 is set to 0.50T and 0.90T. In addition, the width of the metal fine wire 21 at a height of 0.50T is set to W. 0.50 The width of the metal thin wire 21 when the height is 0.90T is set to W 0.90 At this time, W 0.50 / W0 is preferably 0.70 to 0.99, more preferably 0.75 to 0.99 or less, and still more preferably 0.80 to 0.95. 0.90 / W 0.50 It is preferably 0.50 to 0.95, more preferably 0.55 to 0.90, and still more preferably 0.60 to 0.85. 0.50 / W0 is greater than W 0.90 / W 0.50 That is, it is preferred that the width of the thin metal wire 21 gradually decreases from a height position at a thickness of 0.50T from the interface of the thin metal wire 21 on the substrate 10 side toward a height position at a thickness of 0.90T.
[0119] As described later, the conductive film of this embodiment can be formed by a printing method using ink, and the metal fine wire 21 formed by this method has the above-mentioned characteristic shape. As other methods for forming metal fine wires, methods using nanoimprinting, photolithography, and other methods using nanowires are also considered, but the metal fine wires produced by these methods are different from the metal fine wires formed by the printing method in the above-mentioned shape.
[0120] (Thickness to width ratio)
[0121] The aspect ratio represented by the thickness T of the metal fine wire 21 relative to the line width W0 of the metal fine wire 21 is preferably greater than 0.05 and less than 1.00. The lower limit of the aspect ratio is more preferably greater than 0.08, and further preferably greater than 0.10. By increasing the aspect ratio, there is a tendency that the conductivity can be further improved without reducing the transmittance.
[0122] (spacing)
[0123] The pitch P of the metal fine wire pattern is preferably 0.2 to 1000 μm, more preferably 10 to 750 μm, and further preferably 50 to 500 μm. When the pitch P of the metal fine wire pattern is 0.2 μm or more, good transmittance can be obtained. When the pitch P of the metal fine wire pattern is 1000 μm or less, there is a tendency that the conductivity can be further improved. It should be noted that when the shape of the metal fine wire pattern is a grid pattern, the pitch of the metal fine wire pattern with a line width of 1 μm is set to 200 μm, and an aperture ratio of 99% can be formed. It should be noted that the pitch P is the sum of the line width W0 and the distance between the metal fine wires.
[0124] The line width, aspect ratio, and spacing of the metal fine line pattern can be confirmed by observing the cross section of the conductive film using an electron microscope or the like. In addition, the line width and spacing of the metal fine line pattern can also be observed using a laser microscope or an optical microscope. In addition, since the spacing and the aperture ratio have a relationship described later, if one is known, the other can also be calculated. In addition, as a method for adjusting the line width, aspect ratio, and spacing of the metal fine line pattern to a desired range, a method of adjusting the grooves of the plate used in the method for manufacturing the conductive film described later, a method of adjusting the average particle size of the metal particles in the ink, etc. can be listed.
[0125] (Aperture ratio)
[0126] The aperture ratio of the metal fine wire pattern is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and particularly preferably 90% or more. By setting the aperture ratio of the metal fine wire pattern to be above the above-mentioned specific value, there is a tendency for the transmittance of the conductive film to be further improved. In addition, the aperture ratio of the metal fine wire pattern is preferably less than 100%, more preferably 95% or less, further preferably 90% or less, further preferably 80% or less, further more preferably 70% or less, and particularly preferably 60% or less. By setting the aperture ratio of the metal fine wire pattern to be below the above-mentioned specific value, there is a tendency for the conductivity of the conductive film to be further improved. The aperture ratio of the metal fine wire pattern also has different suitable values depending on the shape of the metal fine wire pattern. In addition, the aperture ratio of the metal fine wire pattern can appropriately combine the above-mentioned upper limit value and lower limit value according to the required performance (transmittance and sheet resistance) of the target electronic device.
[0127] It should be noted that the “aperture ratio of the metal fine line pattern” can be calculated by the following formula for the area on the transparent substrate where the metal fine line pattern is formed. The area on the transparent substrate where the metal fine line pattern is formed refers to Figure 3 The range shown by S is excluding the edge portion where the metal fine line pattern is not formed.
[0128] Opening ratio of metal fine line pattern = (1-area occupied by metal fine line pattern / area of transparent substrate) × 100
[0129] In addition, the relationship between the aperture ratio and the pitch varies depending on the shape of the metal fine line pattern, but can be calculated as follows. Figure 5 (a) of FIG. 1 is a schematic diagram of a mesh pattern (grid pattern) having pattern units 23. In the case of this mesh pattern, the aperture ratio and the pitch have the following relationship.
[0130] Aperture ratio = {area of the opening 22 / area of the pattern unit 23} × 100
[0131] ={((pitch P1-line width W1)×(pitch P2-line width W2)) / (pitch P1×pitch P2)}×100
[0132] in addition, Figure 5 (b) shows a schematic diagram of a line pattern. In the case of this line pattern, the aperture ratio and the pitch have the following relationship.
[0133] Aperture ratio = {(pitch P-line width W) / pitch P}×100
[0134] (Chip resistor)
[0135] The sheet resistance of the conductive film 100 is preferably 0.1 Ω / sq to 1000 Ω / sq, more preferably 0.1 Ω / sq to 500 Ω / sq, further preferably 0.1 Ω / sq to 100 Ω / sq, further preferably 0.1 Ω / sq to 20 Ω / sq, further more preferably 0.1 Ω / sq to 10 Ω / sq. The sheet resistance of the conductive film can be measured by the following method.
[0136] First, a portion of the conductive film on which a metal fine wire pattern is disposed is cut out in a rectangular shape to obtain a measurement sample. Collectors for measuring sheet resistance that are electrically connected to the metal fine wire pattern are formed at both ends of the obtained measurement sample, and the resistance R (Ω) between the collectors provided at both ends is measured. Using the above resistance R (Ω), and the length L (mm) in the width direction and the length D (mm) in the depth direction of the measurement sample corresponding to the distance between the collectors, the sheet resistance R can be calculated by the following formula: s (Ω / sq).
[0137] R s =R / L×D
[0138] There is a tendency that the lower the sheet resistance, the more the power loss is suppressed. Therefore, electronic paper, touch panels, and flat panel displays with low power consumption can be obtained.
[0139] The sheet resistance of the conductive film 100 tends to decrease by increasing the aspect ratio (height) of the metal thin wires. Alternatively, the sheet resistance can be adjusted by selecting the type of metal material constituting the metal thin wires.
[0140] (Visible light transmittance)
[0141] The visible light transmittance of the conductive film 100 is preferably 80% to 100%, more preferably 90% to 100%. The visible light transmittance can be measured by calculating the transmittance in the visible light (360 to 830 nm) range from the total light transmittance according to JIS K 7361-1:1997.
[0142] The visible light transmittance of the conductive film 100 tends to be increased by reducing the line width of the metal fine line pattern or increasing the aperture ratio.
[0143] (Haze)
[0144] The haze of the conductive film 100 is preferably 0.01% or more and 5.00% or less. The upper limit of the haze is more preferably 3.00% or less, and further preferably 1.00% or less. If the upper limit of the haze is 5.00% or less, the blurring of the conductive film to visible light can be sufficiently reduced. The haze in this specification can be measured according to the haze of JIS K7136:2000.
[0145] [Wound body]
[0146] The wound body 200 of the present embodiment is a wound body of the above-mentioned conductive film 100 , and is wound so that the conductive portion 20 is in contact with the second surface 10 b . Figure 2 One aspect of the wound body 200 according to the present embodiment is shown in FIG.
[0147] The conductive film 100 constituting the roll 200 is preferably a long film having a short side and a long side. In this case, the width of the roll 200 is consistent with the short side of the conductive film 100. For such a long roll 200 of conductive film 100, the conductive portion 20 is in contact with the second surface 10b in a large area, and the conductive portion 20 is easily pressed against the second surface 10b due to the tension during winding and the weight of the conductive film 100, so there is a tendency to easily cause dirt. Therefore, the present invention is particularly useful.
[0148] The size of the conductive film 100 can be appropriately adjusted according to various uses. As an example, the short side of the conductive film 100 constituting the winding body 200 is preferably 10 mm or more and 2000 mm or less, more preferably 50 mm or more and 1500 mm or less, and further preferably 100 mm or more and 1000 mm or less. In addition, the long side of the conductive film 100 constituting the winding body 200 is preferably 1.0 m or more and 2000 m or less, more preferably 5.0 m or more and 1500 m or less, and further preferably 10 m or more and 1000 m or less.
[0149] [Method for producing conductive thin film]
[0150] As a method for manufacturing a conductive film, there can be listed a method comprising: a substrate manufacturing process for manufacturing a substrate 10 in which a surface free energy SFE1 of a first surface 10a of the substrate 10 is greater than a surface free energy SFE2 of a second surface 10b of the substrate 10 on the opposite side of the first surface 10a, a pattern forming process for forming a pattern on the first surface 10a of the substrate 10 using ink containing a metal component, and a firing process for firing the ink to form a conductive portion 20. Figure 6 An example of a method for producing a conductive film according to this embodiment is shown in FIG.
[0151] [Base material production process]
[0152] In the substrate preparation step, a substrate 10 having different surface free energy on the front side (first side 10a) and the back side (second side 10b) is prepared. More specifically, a method of providing the outermost layer 12 and / or the outermost layer 13 on one side or both sides of the core layer 11 can be cited ( Figure 6 (a)) A method of making the surface roughness of the front and back sides of the substrate 10 different.
[0153] There are no particular limitations on the method for forming the outermost layer 12, and examples thereof include a method of forming a film of the components constituting the outermost layer 12 on the first surface 10a side of the core layer 11 using a vapor phase film forming method such as PVD or CVD. In addition, as another method, a method of forming the outermost layer 12 by applying a composition containing the components forming the outermost layer 12 to the surface on the first surface 10a side of the core layer 11 and drying the composition.
[0154] The method for forming the outermost layer 13 is not particularly limited, and examples thereof include a method of applying a composition containing components constituting the outermost layer 13 to the surface of the core layer 11 on the second surface 10 b side and drying the composition.
[0155] It should be noted that, when other layers are provided between the core layer 11 and the outermost layer 12 and / or the outermost layer 13 , the outermost layer 12 and / or the outermost layer 13 may be formed after the other layers are formed.
[0156] There are no particular limitations on the method of increasing the surface roughness of the generally smooth substrate 10, and examples thereof include a method of providing an easy-adhesion layer having a large surface roughness between the core layer 11 and the outermost layer 13, and forming the outermost layer 13 on the easy-adhesion layer. Thus, the outermost layer 13 reflects the surface roughness of the easy-adhesion layer.
[0157] [Pattern Formation Process]
[0158] The pattern forming step is a step of forming a pattern using ink containing a metal component. The pattern forming step is not particularly limited as long as it is a plate-printing method using a plate having grooves of a desired metal fine line pattern, and includes, for example, a step of applying ink to the surface of a transfer medium; a step of placing the surface of the transfer medium coated with ink opposite to the surface of the raised portion of the relief plate, pressing and contacting the surface to transfer the ink on the surface of the transfer medium to the raised portion of the relief plate; and a step of placing the surface of the transfer medium 30 with the ink 24 remaining thereon opposite to the first surface 10a of the substrate 10, pressing and contacting the surface to transfer the ink 24 remaining on the surface of the transfer medium to the first surface 10a of the substrate 10 ( Figure 6 (b) to (c)). It should be noted that, when the outermost layer 12 is formed on the substrate 10 , the ink 24 is transferred to the surface of the outermost layer 12 .
[0159] (Ink)
[0160] The ink used in the pattern forming step contains a conductive component and a solvent, and may contain a surfactant, a dispersant, a reducing agent, etc. as needed. When the conductive component is a metal component, the metal component may be contained in the ink in the form of metal particles or in the form of a metal complex.
[0161] The average primary particle size of the metal particles is preferably less than 100 nm, more preferably less than 50 nm, and further preferably less than 30 nm. In addition, there is no particular restriction on the lower limit of the average primary particle size of the metal particles, and 1 nm or more can be cited. The average primary particle size of the metal particles is less than 100 nm, and the line width W of the obtained metal fine wire can be made thinner. It should be noted that the "average primary particle size" refers to the particle size of each metal particle (so-called primary particle), which is different from the average secondary particle size of the particle size of the aggregate (so-called secondary particle) formed by a collection of multiple metal particles.
[0162] The metal particles are not particularly limited, and examples thereof include metal oxides such as copper oxide, metal compounds, and core / shell particles having a copper core and a copper oxide shell. The form of the metal particles can be appropriately determined from the viewpoints of dispersibility and sinterability.
[0163] The surfactant is not particularly limited, and examples thereof include fluorine-based surfactants. By using such a surfactant, the coating property of the ink on the transfer medium (blanket) and the smoothness of the coated ink are improved, and there is a tendency to obtain a more uniform coating film. It should be noted that the surfactant is preferably configured in a manner that can disperse the metal component and is not likely to remain during firing.
[0164] In addition, the dispersant is not particularly limited, and examples thereof include dispersants that achieve non-covalent bonding or interaction on the surface of the metal component and dispersants that achieve covalent bonding on the surface of the metal component. As a functional group that achieves non-covalent bonding or interaction, a dispersant having a phosphate group can be cited. By using such a dispersant, there is a tendency that the dispersibility of the metal component is further improved.
[0165] Furthermore, as solvents, alcohol solvents such as monohydric alcohols and polyhydric alcohols; alkyl ether solvents; hydrocarbon solvents; ketone solvents; ester solvents, etc. can be listed. They can be used alone or in combination of one or more. For example, a combination of a monohydric alcohol having a carbon number of less than 10 and a polyhydric alcohol having a carbon number of less than 10 can be listed. By using such a solvent, there is a tendency to further improve the coating property of the ink on the transfer medium (felt), the transfer property of the ink from the transfer medium to the relief plate, the transfer property of the ink from the transfer medium to the transparent substrate, and the dispersibility of the metal component. It should be noted that the solvent is preferably constituted in a manner that can disperse the metal component and is not easy to remain during firing.
[0166] [Firing process]
[0167] In the firing step, for example, the metal component in the ink 24 transferred to the first surface 10a of the substrate 10 is sintered to form the conductive portion 20 ( Figure 6 (d)). There is no particular limitation on the method of sintering as long as the metal components are melted to form a sintered film of the metal component. Firing can be carried out, for example, using a sintering furnace, or using plasma, a heating catalyst, ultraviolet rays, vacuum ultraviolet rays, an electron beam, an infrared lamp annealing, a flash lamp annealing, a laser, etc. In the case where the obtained sintered film is easily oxidized, it is preferably fired in a non-oxidizing atmosphere. In addition, in the case where it is difficult to reduce the metal oxide or the like using only a reducing agent that may be contained in the ink, it is preferably fired in a reducing atmosphere.
[0168] A non-oxidizing atmosphere refers to an atmosphere that does not contain oxidizing gases such as oxygen. There are inert atmospheres and reducing atmospheres. An inert atmosphere refers to an atmosphere filled with inert gases such as argon, helium, neon, and nitrogen. In addition, a reducing atmosphere refers to an atmosphere in which reducing gases such as hydrogen and carbon monoxide are present. These gases can be filled into a firing furnace and fired as a closed system to form a coating film (dispersion coating film) of the ink. In addition, the firing furnace can also form a circulation system to circulate these gases while firing the dispersion coating film. When firing the dispersion coating film in a non-oxidizing atmosphere, it is preferred to temporarily evacuate the firing furnace and remove the oxygen in the firing furnace and replace it with a non-oxidizing gas. In addition, firing can be carried out in a pressurized atmosphere or in a reduced pressure atmosphere.
[0169] There is no particular restriction on the firing temperature, but it is preferably 20°C to 400°C, more preferably 50°C to 300°C, and further preferably 80°C to 200°C. By setting the firing temperature to 400°C or below, a substrate with low heat resistance can be used, which is preferred. In addition, by setting the firing temperature to 20°C or above, the formation of the sintered film is fully carried out, and there is a tendency for the conductivity to become good, which is preferred. It should be noted that the obtained sintered film contains a conductive component derived from the metal component, and in addition, it may contain a non-conductive component depending on the components used in the ink and the firing temperature.
[0170] As described above, according to the present invention, it is possible to provide a conductive film, a conductive film roll, an electronic paper, a touch panel, and a flat panel display that are excellent in both conductivity and flexibility while sufficiently maintaining transparency.
[0171] Example
[0172] The present invention will be described in more detail below using Examples and Comparative Examples. The present invention is not limited to the following Examples in any way.
[0173] [Example 1]
[0174] A polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name COSMOSHINE A4100, film thickness 50 μm) having an easy-adhesive layer formed on one side was used as the core layer, and a composition consisting of 2% by mass of silicon oxide nanoparticles, 1% by mass of a conductive organosilane compound, 65% by mass of 2-propanol, 25% by mass of 1-butanol, and 7% by mass of water was applied to the surface (first surface 10a) where no easy-adhesive layer was formed, and dried to form a silicon oxide-containing film having a thickness of 50 nm and a volume resistivity of 5000 Ωcm as the outermost layer 12. In addition, a composition containing an alkyd compound (manufactured by Arakawa Chemical Co., Ltd., product name RL453) was applied to the surface (second surface 10b) where the easy-adhesive layer was formed on the core layer, and dried to form an outermost layer 13 having a thickness of 50 nm, thereby obtaining a substrate A.
[0175] Next, 20 parts by mass of cuprous oxide nanoparticles having a particle size of 21 nm, 4 parts by mass of a dispersant (manufactured by BYK Chemie, product name: Disperbyk-145), 1 part by mass of a surfactant (manufactured by AGC SEIMI CHEMICAL CO., LTD., product name: S-611), and 75 parts by mass of ethanol were mixed and dispersed to prepare an ink having a content ratio of 20% by mass of cuprous oxide nanoparticles.
[0176] Next, ink is applied to the surface of the transfer medium, and the surface of the transfer medium coated with ink is placed opposite to a plate having grooves with a metal fine line pattern, and pressed and contacted to transfer a portion of the ink on the surface of the transfer medium to the convex surface of the plate. Then, the surface of the transfer medium coated with the residual ink is placed opposite to substrate A, and pressed and contacted to transfer the desired metal fine line pattern ink A1 onto substrate A. Next, the metal fine line pattern ink (dispersion coating film) is fired by flash lamp annealing at room temperature using Pulseforge 1300 manufactured by NovaCentrix to obtain a conductive film containing metal fine lines with a grid pattern of line width 3μm and thickness 500nm. It should be noted that for the metal fine lines, W 0.50 / W0 is greater than W 0.90 / W 0.50 .
[0177] [Example 2]
[0178] A conductive thin film was obtained in the same manner as in Example 1 except that a urethane compound (product name P05, manufactured by Nakai Techno Co., Ltd.) was used as the outermost layer 13 instead of the alkyd compound (product name RL453, manufactured by Arakawa Chemical Co., Ltd.).
[0179] [Example 3]
[0180] A conductive thin film was obtained in the same manner as in Example 1 except that a siloxane compound (KS-847, manufactured by Shin-Etsu Silicones Co., Ltd.) was used as the outermost layer 13 instead of the alkyd compound (RL453, manufactured by Arakawa Chemical Co., Ltd.).
[0181] [Example 4]
[0182] A conductive thin film was obtained in the same manner as in Example 1 except that a fluorine compound (DH-120TH, manufactured by Harves Corporation) was used as the outermost layer 13 instead of the alkyd compound (RL453, manufactured by Arakawa Chemical Co., Ltd.).
[0183] [Example 5]
[0184] A conductive thin film was obtained in the same manner as in Example 2 except that the line width of the mesh pattern was 1 μm and the thickness was 150 nm.
[0185] [Example 6]
[0186] A composition containing silicon oxide nanoparticles and a conductive organosilane compound as in Example 1 was applied to the opposite side of the release layer (second side) of a release PET film (manufactured by HIGASHIYAMA FILM CO., LTD., product name HY-NS70) in a manner to form the first side, and dried to form a silicon oxide-containing film having a thickness of 50 nm and a volume resistivity of 5000 Ωcm.
[0187] Through the above operation, a thin film with the following structure was obtained.
[0188] Outermost layer 12: Silicon oxide-containing film
[0189] Core layer 11: polyethylene terephthalate (PET)
[0190] Outermost layer 13: release layer
[0191] Next, similarly to Example 1, metal fine wires having a mesh pattern with a line width of 3 μm and a thickness of 500 nm were formed on the outermost layer 12 (first surface 10 a ), thereby obtaining a conductive thin film having a mesh pattern.
[0192] [Example 7]
[0193] A conductive film was obtained in the same manner as in Example 6 except that a release PET film (manufactured by HIGASHIYAMA FILM CO., LTD., product name: HY-NS80) was used as the release PET film.
[0194] [Example 8]
[0195] A conductive film was obtained in the same manner as in Example 6 except that a release PET film (manufactured by HIGASHIYAMA FILM CO., LTD., product name: HY-NS85) was used as the release PET film.
[0196] [Comparative Example 1]
[0197] A conductive thin film was obtained in the same manner as in Example 1 except that the outermost layer 13 was not formed.
[0198] <Measurement of surface roughness (arithmetic mean roughness Ra)>
[0199] The method for measuring the surface roughness of each substrate is described below. The first and second surfaces of the substrates prepared in the examples and comparative examples are used as measurement samples, and the arithmetic mean roughness is measured. The surface roughness meter "αSTEP IQ" manufactured by KLA-Tencor Corporation is used for the measurement. The measurement conditions are as follows.
[0200] Step length: 500 μm
[0201] Style Force: 10.6mg
[0202] <Measurement of transmittance>
[0203] The visible light transmittance of the conductive film was measured by calculating the transmittance of visible light having a wavelength of 360 to 830 nm based on the total light transmittance of JIS K 7361-1:1997.
[0204] <Measurement of the dispersion term γSD and polar term γSP of surface free energy>
[0205] The method of measuring the dispersion term γSD and the polar term γSP of the surface free energy will be described.
[0206] The first and second surfaces of the substrates prepared in the examples and comparative examples were used as measurement samples. 2 μL of pure water and 2 μL of diiodomethane were added dropwise to the measurement samples as two solvents with known surface tension γL, dispersion term γLD and polar term γLP.
[0207] The droplets of the two solvents dropped on the measurement sample were observed and photographed from the front and side using a digital microscope (VHX-100 manufactured by KEYENCE), and the contact angle between the measurement sample and the droplets was directly measured using the measurement software attached to the digital microscope to obtain the contact angles when the two solvents were used.
[0208] Solution: Substitute the contact angle θ and the surface tension γ of water and diiodomethane. LV, the dispersion term of surface tension γ LV d , the polar term of surface tension γ LV p Substituting the following equation (4) into the obtained simultaneous equations, the dispersion term γ of the surface free energy of the measured sample is obtained: SV d , γ SV p .
[0209] γ L (1+cosθ) / 2=(γ SV d ×γ LV d ) 0.5 +(γ SV p ×γ LV p ) 0.5 (4)
[0210] [Sticky Evaluation]
[0211] The conductive film (short side 230mm, long side 150m) obtained as described above is wound around an axis of diameter φ75mm in the state of applying a tension of 10N in the length direction to obtain a 150m long winding body. After being kept at room temperature for 24 hours, the winding body is unwound, and 3 samples are cut out at a position 1m away from the short side end of the starting point of the film in contact with the center of the winding body. The sample is cut out from the long side and the center side of both ends in the width direction, and the size of one sample is set to 10mm×10mm. Then, the second surface of each sample is confirmed at 9 points of view using an optical microscope. For each view, the area of the conductive part that is sticky to the second surface is calculated, and the average value Ave is calculated. Then, under the same field of view area (0.5mm×0.5mm), if it is the first surface, the area of the conductive part formed is set to 100%, and the ratio of this average value Ave is calculated as the sticky rate.
[0212] In addition, the wound body of the conductive film obtained above was unwound before being fired by flash lamp annealing, and a 1 m portion from a position 1 m away from the short side end was wiped with BEMCOT M-3II (manufactured by Asahi Kasei Corporation) impregnated with ethanol in the same manner as above, and whether the ink adhered to the BEMCOT was visually confirmed as the ink adhesion before firing. The judgment index is as follows.
[0213] ◎Ink does not adhere at all
[0214] 〇Ink adhesion can be slightly confirmed
[0215] ×Ink adhesion found
[0216] [Table 1]
[0217]
[0218] In the sticking evaluation, the photos of the cut samples are as follows Figure 7 and 8 shown. Figure 7 This is a photograph showing the first and second surfaces of Example 1. Figure 8 These are photographs showing the first and second surfaces of Comparative Example 1.
[0219] As shown in Table 1, for Examples 1 to 7, the surface free energy SFE1 of the first surface was greater than the surface free energy SFE2 of the second surface, and the sticking of the fine line pattern was evaluated to be good. In particular, for Examples 2 to 7 in which the difference between SFE1 and SFE2 was large, the ink adhesion before firing was good. On the other hand, for Comparative Example 1 in which the surface free energy SFE1 of the first surface was less than the surface free energy SFE2 of the second surface, the sticking of the fine line pattern could not be suppressed.
[0220] Industrial Applicability
[0221] The conductive film of the present invention can be suitably used for transparent electrodes for electronic paper, touch panels, flat panel displays, etc., as well as thin heaters, and has industrial applicability.
[0222] Description of Reference Numerals
[0223] 10 ...substrate, 10a ...first surface, 10b ...second surface, 11 ...core layer, 12 ...outermost layer, 13 ...outermost layer, 20 ...conductive portion, 21 ...metal fine wire, 22 ...opening, 23 ...pattern unit, 24 ...ink, 100 ...conductive film, 200 ...wound body
Claims
1. A conductive film comprising a substrate and a conductive portion including at least a fine line pattern formed on a first surface of the substrate, The surface free energy SFE1 of the first surface is greater than the surface free energy SFE2 of the second surface of the substrate opposite to the first surface. The surface free energy SFE1 is 20 to 100 mJ / m 2 The surface free energy SFE2 is 5 to 42 mJ / m 2 , The difference SFE1-SFE2 between the surface free energy SFE1 and the surface free energy SFE2 is 1 mJ / m 2 Above and 100mJ / m 2 the following.
2. The conductive film according to claim 1, wherein The fine line width of the fine line pattern is 0.1 to 30.0 μm.
3. The conductive film according to claim 1, wherein The fine line width of the fine line pattern is 0.2 to 20.0 μm.
4. The conductive film according to claim 1, wherein The fine line width of the fine line pattern is 0.3 to 10.0 μm.
5. The conductive film according to claim 1, wherein The thin line width of the thin line pattern is 1.0 to 5.0 μm.
6. The conductive film according to any one of claims 1 to 5, wherein The pitch of the fine line pattern is 0.2 to 1000 μm.
7. The conductive film according to any one of claims 1 to 5, wherein The pitch of the fine line pattern is 10 to 750 μm.
8. The conductive film according to any one of claims 1 to 5, wherein The pitch of the fine line pattern is 50 to 500 μm.
9. The conductive film according to any one of claims 1 to 5, wherein The difference SFE1-SFE2 between the surface free energy SFE1 and the surface free energy SFE2 is 5 mJ / m 2 Above and 100mJ / m 2 the following.
10. The conductive film according to any one of claims 1 to 5, wherein The difference SFE1-SFE2 between the surface free energy SFE1 and the surface free energy SFE2 is 10 mJ / m 2 Above and 100mJ / m 2 the following.
11. The conductive film according to any one of claims 1 to 5, wherein The difference SFE1-SFE2 between the surface free energy SFE1 and the surface free energy SFE2 is 16 mJ / m 2 Above and 100mJ / m 2 the following.
12. The conductive film according to any one of claims 1 to 5, wherein The difference SFE1-SFE2 between the surface free energy SFE1 and the surface free energy SFE2 is 20 mJ / m 2 Above and 100mJ / m 2 the following.
13. The conductive film according to any one of claims 1 to 5, wherein The surface free energy SFE1 is 40 to 50 mJ / m 2 .
14. The conductive film according to any one of claims 1 to 5, wherein The substrate includes: a first outermost layer forming the first surface; a second outermost layer forming the second surface opposite to the first surface; and a core layer formed between the first outermost layer and the second outermost layer.
15. The conductive film according to any one of claims 1 to 5, wherein The substrate has a layer containing a silicon compound as an outermost layer on the first surface side.
16. The conductive film according to claim 15, wherein The outermost layer on the first surface side contains at least one of a conductive inorganic oxide and a conductive organic compound.
17. The conductive film according to claim 15, wherein The volume resistivity of the outermost layer on the first surface side is 100 Ωcm or more and 100,000 Ωcm or less.
18. The conductive film according to claim 15, wherein The volume resistivity of the outermost layer on the first surface side is 1000 Ωcm or more and 10000 Ωcm or less.
19. The conductive film according to claim 15, wherein The volume resistivity of the outermost layer on the first surface side is 2000 Ωcm or more and 8000 Ωcm or less.
20. The conductive film according to any one of claims 1 to 5, wherein The surface free energy SFE2 is 11 to 42 mJ / m 2 .
21. The conductive film according to any one of claims 1 to 5, wherein The surface free energy SFE2 is 11 to 30 mJ / m 2 .
22. The conductive film according to any one of claims 1 to 5, wherein The surface free energy SFE2 is 11 to 25 mJ / m 2 .
23. The conductive film according to any one of claims 1 to 5, wherein The substrate has a layer containing at least one selected from the group consisting of melamine compounds, alkyd compounds, fluorine compounds, and siloxane compounds as the outermost layer on the second surface side.
24. The conductive film according to claim 23, wherein The thickness of the outermost layer on the second surface side is 0.01 μm or more and 100 μm or less.
25. The conductive film according to claim 23, wherein The thickness of the outermost layer on the second surface side is 0.01 μm or more and 10 μm or less.
26. The conductive film according to claim 23, wherein The thickness of the outermost layer on the second surface side is 0.01 μm or more and 1 μm or less. 27 . A wound body, which is the wound body of the conductive film according to claim 1 , wherein the wound body is wound so that the conductive portion is in contact with the second surface.
28. The wound body according to claim 27, wherein The conductive film is a long film having a short side of 10 mm to 2000 mm and a long side of 1.0 m to 2000 m. The wound body is formed by winding the conductive film in a longitudinal direction.
29. The wound body according to claim 28, wherein The short side is greater than or equal to 50 mm and less than or equal to 1500 mm.
30. The wound body according to claim 28, wherein The short side is greater than or equal to 100 mm and less than or equal to 1000 mm.
31. The wound body according to any one of claims 28 to 30, wherein The long side is greater than or equal to 5.0 m and less than or equal to 1500 m.
32. The wound body according to any one of claims 28 to 30, wherein The long side is greater than or equal to 10 m and less than or equal to 1000 m.