Composite cooling film comprising a reflective non-porous organic polymer layer and a UV protection layer
By applying a passive radiation composite cooling film to the surface of a solid object, the problem of heat accumulation under solar radiation and internal heat energy is solved, achieving efficient passive cooling and anti-fouling protection.
Patent Information
- Application Number
- CN202180008031.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-16
- Filing Date
- 2021-01-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-01-13
AI Technical Summary
In existing technologies, there is a lack of efficient passive cooling solutions for entities affected by solar radiation and internal heat, leading to heat accumulation and increased energy consumption.
A passive radiation composite cooling film is used, which includes an organic polymer layer filled with reflective non-porous inorganic particles, an ultraviolet protection layer, and an anti-fouling layer. It achieves passive cooling by reflecting and absorbing solar radiation, thereby reducing heat accumulation.
It effectively reduces heat buildup on solid surfaces, improves cooling efficiency, extends the lifespan of the cooling film, and provides anti-fouling and UV protection.
Smart Images

Figure CN114902087B_ABST
Abstract
Description
Background Art
[0001] Entities such as, for example, vehicles and buildings, transformers, etc. are often equipped with active cooling systems in order to remove heat energy gained by solar radiation impinging on the entity, to remove heat energy generated within the entity itself, and so on. Summary of the invention
[0002] Broadly summarized, disclosed herein is a passive radiative composite cooling film suitable for passively cooling a substrate (which can be attached to an entity and / or a portion thereof, such as a vehicle or a building). Broadly summarized, the composite cooling film includes a reflective non-porous inorganic particle-filled organic polymer layer; an ultraviolet protection layer of an organic polymer material, which is disposed outwardly from the reflective non-porous inorganic particle-filled organic polymer layer; and an anti-fouling layer of an organic polymer material. The anti-fouling layer is disposed outwardly from the reflective non-porous inorganic particle-filled organic polymer layer and includes an exposed anti-fouling surface facing outward. The composite cooling film may exhibit an average absorptivity of at least 0.85 in a wavelength range of 8 microns to 13 microns; in some embodiments, the composite cooling film may exhibit such an absorptivity in a wavelength range of 4 microns to 20 microns.
[0003] These and other aspects will become apparent in the following detailed description. However, in no event should this broad summary be construed as a limitation on the subject matter that may be protected by the claims, whether such subject matter is presented in the claims of the initially filed application or in the claims of an amended application, or is presented in other ways during the prosecution process. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] Figure 1 Schematic side view of an exemplary composite cooling film bonded to a substrate secured to a body to be cooled.
[0005] Figure 2 is a schematic side view of another exemplary composite cooling film.
[0006] Figure 3 is a schematic side view of another exemplary composite cooling film.
[0007] Figure 4A , Figure 4B and Figure 4C is a view of an exemplary antifouling surface structure having a microstructure. Figure 4A A perspective view of a cross section relative to the xyz axis is shown. Figure 4C Shows Figure 4A Cross section in the xz plane. Figure 4B Another cross section in the yz plane is shown.
[0008] Figure 5for FIG. 4A to FIG. 4C Cross-sectional views of various nanostructures of the antifouling surface structure in the xz plane.
[0009] Figure 6 is a cross-sectional view of various nanostructures including masking elements in the xz plane, which can be used as FIG. 4A to FIG. 4C The surface structure is used together Figure 5 An alternative to nanostructures.
[0010] Fig. 7A and Figure 7B A diagram of lines representing the cross-sectional profile in the xz plane for different forms of microstructures for the surface structure is shown.
[0011] Figure 8 is a perspective view of a portion of a first surface structure having a discontinuous microstructure.
[0012] Fig. 9 is a perspective view of a portion of a second surface structure having a discontinuous microstructure.
[0013] Fig.10 and Fig.11 1 and 2 are perspective views of different portions of a third surface structure having a discontinuous microstructure.
[0014] Fig.12 is a schematic side view of an exemplary UV protection layer that is a UV reflective layer comprising a multilayer optical film.
[0015] Unless otherwise specified, all diagrams and drawings are not drawn to scale and are selected for the purpose of illustrating different embodiments of the present invention. In particular, unless otherwise specified, the sizes of various components are described only in exemplary terms, and the relationship between the sizes of various components should not be inferred from the drawings. DETAILED DESCRIPTION
[0016] As used in this article:
[0017] "Fluoropolymer" means any organic polymer containing fluorine;
[0018] Unless otherwise indicated, "infrared" (IR) refers to infrared electromagnetic radiation with wavelengths of >700 nm to 1 mm;
[0019] Unless otherwise indicated, "visible" (VIS) means visible electromagnetic radiation having a wavelength of 400 nm to 700 nm, inclusive;
[0020] Unless otherwise indicated, "ultraviolet" (UV) means ultraviolet electromagnetic radiation having a wavelength of at least 250 nm and up to but not including 400 nm;
[0021] "Microporous" means internal porosity (continuous and / or discontinuous) having an average pore size of 50 nm to 10,000 nm;
[0022] "Non-porous" means having a porosity of less than 10% (i.e., a void volume percentage of less than 10); in certain cases, a non-porous article will exhibit a void volume of less than 1% pores (having an average pore size greater than 50 nm);
[0023] "Microvoided" refers to internal discrete voids having an average void diameter of 50 nm to 10,000 nm;
[0024] “Non-fluorinated” means not containing fluorine;
[0025] Unless otherwise specified, “radiation” means electromagnetic radiation;
[0026] “Average reflectance” means the reflectance averaged over a specified wavelength range;
[0027] “Reflection” and “reflectivity” mean the property of reflected light or radiation, particularly reflectivity measured independently of the thickness of the material; and
[0028] "Reflectivity" is a measure of the proportion of light or other radiation that is reflected from a surface at normal incidence. Reflectivity typically varies with wavelength and is reported as the percentage of incident light reflected from a surface (0% - no reflected light, 100% - all light is reflected; typically, such reflectivity is normalized to a scale of 0 to 1). Reflectivity and reflection are used interchangeably herein. Reflectivity can be measured according to methods disclosed later herein.
[0029] Absorbance can be measured using the method described in ASTM E903-12 "Standard Test Method for Solar Absorptance, Reflectance, and Transmittance of Materials Using Integrating Spheres". Absorbance values can be obtained by making transmittance measurements and then calculating the absorptance using Formula 1 below.
[0030] As used herein, the term "absorptivity" refers to the logarithm to the base 10 of the ratio of incident radiant power to transmitted radiant power through a material. This ratio can be described as the radiant flux received by the material divided by the radiant flux transmitted by the material. The absorptivity (A) can be calculated based on transmittance (T) according to the following formula 1:
[0031] A=-log 10T (1)
[0032] Emissivity can be measured using an infrared imaging radiometer using the method described in ASTM E1933-14 (2018), "Standard Practice for Measuring and Compensating for Emissivity Using Infrared Imaging Radiometers."
[0033] When fixed to a substrate, terms such as outward, inward, and similar terms are used with reference to the composite cooling film. Outward refers to the direction away from the substrate and inward refers to the direction toward the substrate. The anti-fouling layer of the cooling film will generally be the outermost surface of the cooling film; in many embodiments, the innermost layer of the cooling film may be an adhesive layer that allows the cooling film to be fixed to the substrate. For clarity, the inward (I) and outward (O) directions are indicated in the various figures. It should be understood that the use of this term is for ease of description and does not limit the actual orientation (e.g., horizontal, angled to face the sun, etc.) in which the cooling film can be arranged during actual use.
[0034] "Disposed on top of," "disposed on," "secured to," and similar terms encompass arrangements where an item is directly or indirectly attached to (e.g., in direct contact with or adhesively bonded to) another item via a single adhesive layer. That is, such terms allow for the presence of intervening (e.g., bonding) layers.
[0035] A "composite" film comprises a plurality of layers (any of which may include sub-layers), and requires that all such layers and / or sub-layers be attached (e.g., bonded) to one another (e.g., by pressure-sensitive adhesion, by melt bonding to one another, or any similar method), rather than being abutted to one another and held in place by, for example, mechanical means.
[0036] Composite cooling film
[0037] like Figure 1 As shown in the general exemplary representation in , a composite cooling film 1 is disclosed herein, which includes a reflective non-porous inorganic particle-filled organic polymer layer 10; an ultraviolet (UV) protection layer 20 of an organic polymer material, which is disposed outwardly from the reflective layer 10; and an anti-fouling layer 30 of an organic polymer material. The anti-fouling layer 30 is disposed outwardly from the reflective layer 10 and includes an exposed anti-fouling surface 31 facing outwardly. The layers 10, 20, and 30 may be attached or otherwise bonded to each other via any suitable method as discussed herein.
[0038] The reflective layer 10 (and the cooling film 1 as a whole) can provide passive cooling in the general manner discussed in U.S. Provisional Patent Application No. 62 / 855,392, which is incorporated herein by reference in its entirety. The reflective layer 10 provides reflectivity in certain wavelengths and, as discussed herein, also serves to emit radiation in at least selected wavelengths and can be considered a reflective layer / absorbent layer / emitter layer. Thus, the layer 10 can exhibit an absorptivity of at least 0.5, 0.6, 0.7, 0.8, 0.9, or 0.95 over a wavelength range covering at least the range of 8 microns to 13 microns.
[0039] The UV protection layer 20 is disposed outwardly from the reflective layer 10 to provide UV protection for the reflective layer 10, which can increase the usable life of the cooling film 1. In some embodiments, the UV protection layer 20 can be a UV reflective layer. In some embodiments, the UV protection layer 20 can be a UV absorbing layer. In some embodiments, the UV protection layer 20 can function partially by absorbing UV and partially by reflecting UV. In some embodiments, there can be multiple UV protection layers, for example, one is a UV absorbing layer and another is a UV reflective layer.
[0040] The anti-fouling layer 30 is the outermost layer of the cooling film 1, provides physical protection for the other layers, and in particular can impart anti-fouling and / or easy-to-clean properties to the outermost surface of the cooling film 1. However, it should be understood that in some embodiments, the UV protection layer 20 and / or the anti-fouling layer 30 can contribute to the passive cooling achieved by the cooling film 1 at least to some extent.
[0041] In some embodiments, the cooling film 1 may include an adhesive (eg, a pressure sensitive adhesive) layer 40 that can be used to bond the cooling film 1 to a substrate 50, such as Figure 1 The substrate 50 may in turn be bonded, fixed, or otherwise in thermal contact with a portion of an entity 60 (eg, a vehicle or a building) to be passively cooled, such as Figure 1 As indicated in the exemplary embodiments.
[0042] A variety of options are included in the general arrangement disclosed above. Figure 1 In embodiments of the general type depicted, anti-fouling layer 30 is a separate layer from UV protective layer 20, wherein layer 30 is disposed outwardly from layer 20 and includes an exposed anti-fouling surface 31. Figure 2 In embodiments of the general type depicted, the anti-fouling layer 30 is the same layer as the UV protective layer 20 (i.e., in such embodiments, a single layer may be configured to function as both the anti-fouling layer 30 and the UV protective (e.g., UV absorbing) layer 20, as discussed later herein).
[0043] In some embodiments, the anti-fouling layer 30 can be directly attached to the UV protective layer 20, such as Figure 1As in the exemplary arrangement of . Figure 1 As shown, the UV protective layer 20 can be directly attached to the reflective layer 10. As will be readily appreciated, such an arrangement can be achieved, for example, by extruding, coating, or otherwise disposing one layer onto the major surface of another layer so that the layers are bonded together. In other embodiments, the anti-fouling layer 30 can be indirectly attached to the UV protective layer 20, for example, in the form of a pressure-sensitive adhesive layer. Similarly, in some embodiments, the UV protective layer 20 can be indirectly attached to the reflective layer 10, for example, in the form of a pressure-sensitive adhesive layer. Any combination of direct or indirect attachment of any of these layers is contemplated.
[0044] In some embodiments, the UV protective (eg, UV absorbing) layer 20 may take the form of a pressure sensitive adhesive layer that serves both to bond the anti-fouling layer 30 to the reflective layer 10 and to provide UV protection. Such an arrangement is referred to herein as Figure 1 General arrangement shown.
[0045] In some embodiments, the UV protection layer 20 and / or the anti-fouling layer 30 may be layers of a multi-layer structure (e.g., a multi-layer co-extruded laminate) disposed outwardly from the reflective layer 10. For example, Figure 3 An exemplary arrangement is depicted in which a multilayer structure 25 (in this case a three-layer structure) is disposed outwardly from a reflective layer 10. Figure 3 In the exemplary embodiment of the present invention, the multilayer structure 25 is bonded to the reflective layer 10 by the pressure-sensitive adhesive layer 45. The outermost layer of the multilayer structure provides the anti-fouling layer 30; another layer of the multilayer structure provides the UV protection layer 20, which is arranged inwardly from the anti-fouling layer. Figure 3 In the particular arrangement depicted, structure 25 includes three layers, wherein the innermost layer is UV protective layer 20, and wherein intermediate layer 26 is located between layer 30 and layer 20. However, it should be understood that such a multilayer structure may include any number of layers in any arrangement, so long as the structure includes an outermost layer suitable for use as anti-fouling layer 30. The compositions of the different layers may vary in any suitable manner. For example, the outermost layer may have a composition that provides enhanced anti-fouling (e.g., it may be a fluoropolymer), while the inner layers may have a composition that readily accepts high levels of UV blocking additives (e.g., poly(methyl methacrylate)). One or more intermediate layers (e.g., such as Figure 3 The layer 26 shown) can be used, for example, as an adhesive layer that bonds to both the anti-fouling layer and the UV protective layer.
[0046] In some embodiments, there may be multiple UV protections (whether UV reflecting and / or UV absorbing, and whether in direct contact with each other or separated by one or more intermediate layers). For example, there may be a UV absorbing layer as a layer of a multilayer structure (e.g., a coextruded laminate of the general type mentioned above), and another UV absorbing layer may be present in the form of a UV absorbing pressure sensitive adhesive for bonding the multilayer structure to the reflective layer.
[0047] In some embodiments, the UV protective layer 20 may take the form of or include a UV reflective layer. In some embodiments, such a layer may take the form of a collection of sub-layers that together provide UV reflection; for example, as in the case of a so-called multilayer optical film (MOF) configured to provide UV reflection. Any such UV reflective MOF may be attached to any of the other layers disclosed herein (e.g., to an anti-fouling layer and / or a reflective non-porous inorganic particle-filled organic polymer layer), for example, by way of a pressure-sensitive adhesive layer.
[0048] As described, the cooling film 1 includes an antifouling layer 30. In some embodiments, the antifouling layer 30 can exhibit enhanced antifouling and / or can be easily cleaned due to the chemical composition of at least the exposed surface 31 of the antifouling layer. In some embodiments, the chemical composition of the exposed surface 31 can be the same as the bulk composition of the layer 30. (In other embodiments, the surface 31 can be treated in a manner that specifically changes its chemical composition to provide enhanced antifouling; for example, the surface 31 can be plasma fluorinated.) In some embodiments, the antifouling layer 30 can be composed of a fluoropolymer, as discussed in detail later herein. In other embodiments, the antifouling layer 30 can be composed of a so-called hardcoat composition, also as discussed in detail later herein.
[0049] In some embodiments, the exposed surface 31 of the antifouling layer 30 may be provided with a texture or topography that provides enhanced antifouling. Such texture may, for example, take the form of a set of microstructures and / or nanostructures. In short, such texture may be formed, for example, by molding, embossing, or otherwise forming or pressing the layer 30 against a textured tool surface to impart the desired texture to the surface 31; removing material from the surface 31 (e.g., by etching, laser ablation, etc.) to impart the desired texture; and / or including particulate material (e.g., glass microspheres, etc.) in the layer 30 to impart the desired texture. Combinations of these methods may be used, if desired.
[0050] As described, the cooling film 1 includes a reflective non-porous inorganic particle-filled organic polymer layer 10. In some embodiments, such a layer may take the form of a prefabricated inorganic particle-filled film, for example. Prefabrication means that before being combined with other layers in the process of forming the cooling film 1, the layer already exists in a stable and processable form. Such a prefabricated inorganic particle-filled film may be, for example, a polymethyl methacrylate (PMMA) film loaded with a suitable amount of reflective inorganic particles. In some embodiments, the reflective layer 10 may be a painted layer derived from any suitable paint containing a suitable amount of inorganic particles. Any such paint may be, for example, applied to a suitable substrate by brushing or otherwise, and then allowed to harden. The painted substrate may then be combined with other layers to form the cooling film 1. Therefore, it should be understood that all references herein to, for example, using a pressure-sensitive adhesive layer to attach any layer to the reflective layer 10 encompass the case where the reflective layer 10 is a multilayer structure including, for example, a substrate having a painted layer thereon.
[0051] Reflective organic polymer layer
[0052] In more detail, the reflective non-porous inorganic particle-filled organic polymer layer 10 includes a porosity of less than 10%. By definition, such entities do not include, for example, porous layers (such as nonwoven fiber webs), microporous materials (especially microvoided materials), paper, etc. In various embodiments, such non-porous layers may include a porosity of less than 8%, 6%, 4%, 2%, 1% or 0.5%.
[0053] Layer 10 comprises an organic polymer material filled with (carrying) one or more suitable inorganic particles of a suitable amount providing the desired reflectivity. Such inorganic particles can be selected from, for example, titanium dioxide, magnesium oxide, aluminum oxide, zinc oxide, calcium carbonate, barium sulfate, silicon dioxide, zirconium dioxide, cerium oxide, aluminum silicate, kaolin, and combinations and blends thereof. Inorganic particles can be present in any amount (based on the weight % of the total weight of the layer) providing the desired reflectivity. According to the definition, the organic polymer layer filled with inorganic particles will include at least 5 weight % of reflective inorganic particles. In various embodiments, reflective inorganic particles can include at least 10 weight %, 15 weight %, 20 weight %, 30 weight %, 40 weight %, 50 weight %, 60 weight % or 70 weight % of layer 10.
[0054] The reflective inorganic particles may include any suitable average particle size and particle size distribution. In some embodiments, at least 20%, 40%, 60%, 80%, or 90% (by number average) of the reflective particles may exhibit a diameter (or equivalent diameter, e.g., if irregularly shaped) of less than 5.0, 2.0, or 1.0 microns. In some embodiments, at least 90%, 95%, or 98% (also by number average) of the particles may be nanoparticles having a diameter or equivalent diameter of less than 1000 nanometers. If desired, the particles may be surface treated, for example, to enhance the ability of the particles to be dispersed in an organic polymer material.
[0055] In some embodiments, the reflective layer 10 can take the form of a prefabricated inorganic particle-filled film, which means that the reflective layer is already in a stable and processable form before being combined with other layers to form the cooling film 1. Such prefabricated inorganic particle-filled films can be, for example, polymethyl methacrylate or copolymerized methyl methacrylate (e.g., co-PMMA, such as those available from Kuraray) blended in sufficient amounts with, for example, barium sulfate, titanium dioxide, and / or calcium carbonate. However, any suitable organic polymer material can be used as long as it exhibits sufficient mechanical properties and can be loaded with an acceptable amount of reflective inorganic particles. Any such layer can be combined with any other layer mentioned herein (e.g., with a UV protective layer and an antifouling layer) by, for example, laminating such layers with one or more layers of a pressure-sensitive adhesive.
[0056] In some embodiments, the reflective layer 10 can be a painted layer. Such layers can be derived from any suitable paint carrying a suitable amount of inorganic particles. Any such paint can be, for example, disposed on a suitable supporting substrate (in a flowable form), and then allowed to harden. The painted substrate can then be combined with other layers to form a cooling film 1. As described, it should be understood that all references herein to attaching a layer (e.g., a UV protective layer) to the reflective layer 10, for example, using a pressure-sensitive adhesive layer, encompass the case where the reflective layer 10 is a multilayer structure including, for example, a supporting substrate having a paint layer thereon. In some embodiments, such a supporting substrate can be used to provide pure mechanical support. In some embodiments, such a supporting substrate can be used at least in part to enhance or increase the reflectivity achieved by the reflective layer 10. For example, in some embodiments, the supporting substrate can be, for example, a reflective metal foil or sheet made of, for example, aluminum. In some embodiments, such a supporting substrate can be used at least in part to enhance or increase any absorption / emission characteristics exhibited by the layer 10. For example, in some embodiments, the support substrate can be, for example, a polyester film (e.g., MYLAR film), which, while it may not necessarily contribute to any reflectivity, can contribute to the absorption / emission achieved. Of course, in some embodiments, such a support substrate can be, for example, a metallized PET film that can be used for both purposes.
[0057] The reflective layer 10 of the paint can be derived from any suitable paint, and the paint includes an organic polymer film-forming material (commonly referred to as a binder) that can be hardened to form a stable layer (film). (Strictly speaking, the painted layer, paint layer, etc. as mentioned herein represent the final hardened layer obtained. However, the term "paint" is generally used to refer to the precursor flowable mixture of the hardened layer and its source.) The binder can be provided in any suitable liquid (for example, a solvent, a carrier or a diluent) to provide a mixture or solution, which can be arranged (for example, applied) on a suitable substrate, after which the binder can be hardened when the liquid is removed. Hardening can occur, for example, via removal of solvent (in the case of solvent-based paint). In some embodiments, hardening can occur at least partially by crosslinking, whether by thermal means or by a radiation curing process such as UV curing or electron beam curing to promote. If such crosslinking is desired, in some embodiments, the binder can include a multifunctional monomer to promote such crosslinking.
[0058] In some embodiments, the paint may be a water-based paint (e.g., an emulsion or dispersion of the type commonly referred to as latex paint) that forms a non-porous (e.g., film) layer upon removal of water. As will be well understood, such drying causes the organic polymer binder to coalesce to form a solid film. Also as will be well understood, such coalescence may leave a small amount of voids or cavities in the final hardened paint layer, by its statistical nature. However, such voids will generally be insignificant; in any case, the painted layer will be considered a non-porous layer as disclosed herein, and will be distinguished, inter alia, from a microvoided layer, etc.
[0059] In some embodiments, the hardening of the organic polymer binder of the paint may not involve any chemical reaction (formation of chemical bonds). In other embodiments, for example if the paint contains one or more thermosetting components, such as drying oils such as linseed oil, the hardening may involve at least some bond formation.
[0060] Generally speaking, the organic polymer binder of such paints can be selected from or include materials such as alkyd resins, acrylics, vinyl acrylics, styrene-acrylics, vinyl acetate / ethylene, polyurethanes, polyesters, melamine resins, epoxy resins, polysiloxanes, polylactic acid, cellulose, polysaccharides, etc. In a particular embodiment, such binders can be acrylic materials comprising, for example, polymethyl methacrylate and / or its copolymers. The binder will provide, for example, mechanical durability and toughness, wear resistance, etc. to the hardened paint layer. The paint may include any other materials required for any other purpose, for example, a leveling agent, a viscosity modifier, a dye, a biocide, an emulsifier, etc.
[0061] Suitable paints that can be used to form a reflective layer that can be used for the purposes described herein may include, for example, those described in U.S. Patent No. 10,323,151, which is incorporated herein by reference for this purpose. Examples of paints that may be suitable include products that can be purchased from various sources, such as Solarkote, Suntech Coatings, SkyCool, and Exterior Performance Coatings. It should be understood that many such paints may include one or more UV blocking additives of the general type mentioned later herein, etc. However, for the specific purposes described herein, the presence of such additives will not eliminate the need to provide a UV protective layer outward from the painted reflective layer in the general manner described herein.
[0062] "Paint" as disclosed herein encompasses any flowable mixture, solution, dispersion, or the like that can be applied to a suitable substrate (whether by, for example, knife coating, spraying, etc., and whether done manually or in a large-scale coating operation). Such coating operations and other operations required to assemble the cooling film 1 can be completed in any particular order. For example, a layer of paint can be applied to a substrate and allowed to harden, after which the painted substrate can be attached to a UV protective layer, for example by using a pressure-sensitive adhesive layer. Alternatively, a UV protective layer (e.g., a UV-reflecting multilayer optical film or a UV-absorbing hard coating that is itself applied to a suitable support such as, for example, a PET film) can be laminated to the substrate (e.g., in the form of a pressure-sensitive adhesive layer), after which a suitable paint can be applied to the other side of the substrate. In still another example, a suitable paint can be applied to the substrate described above with reference to Figure 3 The invention also provides a method for coating a plurality of substrates on an inwardly facing layer of a multilayer structure of the general type discussed. And, of course, in some embodiments, a UV protective layer in the form of a pressure sensitive adhesive layer loaded with a UV blocking additive may be attached to the painted substrate. Likewise, it will be apparent that a variety of specific embodiments are encompassed within the scope of the arrangements disclosed herein.
[0063] In various embodiments, layer 10 is diffusely reflective of visible radiation over most wavelengths in the range of, for example, 400 nanometers to 700 nanometers, inclusive. In some embodiments, the reflective layer can have an average reflectivity of at least 85% (in some embodiments, at least 90%, at least 91%, at least 92%, at least 93%, at least 94%, at least 95%, at least 96%, at least 97%, at least 98%, at least 99%, or even at least 99.5%) over a wavelength range of at least 400 nm up to 700 nm. In some embodiments, the reflective layer can be reflective over a wider wavelength range. Thus, in some embodiments, the layer may have an average reflectivity of at least 85% (in some embodiments, at least 90%, at least 91%, at least 92%, at least 93%, at least 94%, at least 95%, at least 96%, at least 97%, at least 98%, at least 99% or even at least 99.5%) over a wavelength range of at least 400 nm and up to 2.5 microns, preferably at least 300 nm to 3.0 microns, but this is not required.
[0064] The reflectivity of the reflective layer 10 (or any other layer of the cooling film 1 or the cooling film 1 as a whole) can be measured according to the method and equipment cited in ASTM E1349-06 (2015) to obtain values such as those listed above. Such methods can use an integrating sphere and a spectrophotometer, which scans a desired range (e.g., 400nm to 2500nm) at suitable intervals (e.g., 5nm) in a reflection mode, such as outlined in U.S. Provisional Patent Application No. 62 / 611639 and the resulting International Patent Application Publication WO 2019 / 130199, both of which are incorporated herein by reference in their entirety. The measured value can then be reported as an average value within a wavelength range. In some embodiments, any of the values listed above can be an average value obtained by weighting the data within a wavelength range according to the weight of the AM1.5 standard solar spectrum. This can be performed according to the procedure outlined in, for example, ASTM E903.
[0065] The above discussion clearly shows that in various embodiments, the reflective layer 10 can contain fluorinated polymers, non-fluorinated polymers, or blends thereof in any desired arrangement. As specified herein, non-fluorinated refers to an entity containing less than 1% by weight of fluorine atoms. In various embodiments, the non-fluorinated polymer and / or the non-fluorinated layer can contain less than 0.5%, 0.1%, or 0.01% by weight of fluorine atoms.
[0066] UV protection layer
[0067] The cooling film 1 will include at least one UV protection layer 20. The layer 20 is disposed outwardly from the reflective layer 10 and provides UV protection for the reflective layer 10 (and possibly one or more additional layers), which may, for example, increase the useful life of the cooling film 1. That is, the layer 20 may advantageously minimize or reduce damage to the reflective layer 10 by ultraviolet radiation.
[0068] In some embodiments, the UV protection layer can be a UV absorbing layer. A UV absorbing layer is defined as transmitting less than 20% of radiation over a 30 nm bandwidth in the wavelength range of 300 nm to 400 nm. In the special case where multiple UV absorbing layers are present outside the reflective layer 10, this requirement is imposed on the combined UV absorbing layers. That is, even if no single layer reaches the threshold, the layers combined will meet the threshold. In various embodiments, the UV absorbing layer will transmit (or the multiple layers will transmit in total) less than 15%, 10%, or 5% of radiation over a 30 nm bandwidth in the wavelength range of 300 nm to 400 nm.
[0069] As used herein, the term UV absorbing layer refers to a layer that absorbs, blocks, dissipates, or otherwise prevents UV radiation from reaching the reflective layer 10 by a mechanism or combination of mechanisms that is largely independent of reflectivity. In various embodiments, the reflectivity of the UV absorbing layer (or a group of layers) to ultraviolet radiation will be less than 40%, 30%, 20%, 10%, or 5% over most of the wavelength range from 300 nm to 400 nm. Thus, the UV absorbing layer as disclosed herein is distinguished from reflective layers such as, for example, vapor-coated metal layers, and is also distinguished from reflective articles such as reflective multilayer optical films (MOFs) and their individual optical layers, and from, for example, dielectric mirrors composed of inorganic layers.
[0070] In some embodiments, the UV absorbing layer may include additives having properties (e.g., wavelength-specific extinction coefficients, absorptivity, and / or transmittance, etc.) that allow the additive to convert the impinging UV radiation into heat that is subsequently dissipated. (Such additives are generally referred to as UV absorbers.) In some embodiments, such layers may include additives that act synergistically with the UV absorbers to enhance the performance of the UV absorbers. Such additives include many materials known as light stabilizers or UV stabilizers (e.g., hindered amine light stabilizers or HALS). Various categories of various additives are discussed in detail later herein. Although some such additives may be discussed in the context of being present in a particular layer (e.g., an adhesive layer or a hard coat layer), it is to be explicitly stated that any such additive may be incorporated into any of the layers disclosed herein.
[0071] In some embodiments, the UV absorbing layer may include opaque particles (e.g., inorganic fillers such as titanium dioxide, barium sulfate, kaolinite, etc.) that are inherently reflective to a certain extent (different fillers may exhibit different degrees of reflectivity and absorption). However, as described, the primary function of the UV absorbing layer is to block UV radiation by mechanisms other than reflection. Therefore, in some embodiments, any such particles may be primarily used to dissipate UV radiation by scattering it. In some embodiments, the UV absorbing layer may include less than 5%, 2%, 1%, 0.5%, 0.2%, or 0.1% by weight of any such inorganic filler.
[0072] Any such additive that, when present in layer 20 and that acts to block (e.g., mitigate or reduce) the passage of UV radiation to reflective layer 10, whether acting alone or in conjunction with some other additive, will be referred to herein as a UV blocking additive. (As noted, such terms encompass additives that may be commonly referred to as, for example, UV absorbing, UV scattering, and UV stabilizing.) For convenience, such layers may be referred to herein as UV absorbing layers. However, the term is used in a general sense; as discussed above, such layers are not limited to only including additives that act only by directly absorbing UV radiation and dissipating UV energy in the form of heat. Such layers may be equivalently referred to as UV blocking layers or UV dissipating layers.
[0073] In various embodiments, the UV absorbing layer may be present in the cooling film 1, for example, as an adhesive layer, as a hard coating layer (e.g., a coating layer), as a single layer (e.g., an extruded layer) of, for example, a fluoropolymer, and / or as a layer of a multilayer structure (e.g., as a layer of a stack of coextruded layers), all of which are discussed later in various aspects herein. If desired, multiple UV absorbing layers may be present, thereby acting in combination as described above.
[0074] In some embodiments, the UV protective layer 20 may be a UV reflective layer. A UV reflective layer is defined herein as having a reflectivity of at least 50% for UV radiation at most wavelengths in the range of at least 340 nanometers but less than 400 nanometers (i.e., at normal incidence). In some embodiments, the UV reflective layer has a reflectivity of at least 60%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or even at least 98% for UV radiation at most wavelengths in the range of at least 340 nanometers but less than 400 nanometers (i.e., at normal incidence).
[0075] In some embodiments, the UV protection layer 20 may include a UV-reflective multilayer optical film (MOF). Such UV-reflective MOFs typically include alternating layers of different polymers having different refractive indices and appropriate layer thicknesses. The various layers, their thicknesses, compositions, etc. may be configured to ensure that the MOF is UV-reflective. In some embodiments, the MOF may selectively be UV-reflective; for example, it may reflect UV radiation while passing other wavelengths of radiation (e.g., visible and / or IR radiation).
[0076] Fig.12 An exemplary UV protective layer 20 is shown in the form of a UV reflective multilayer optical film 320, which includes one or more first optical layers 312, one or more second optical layers 314, and optionally one or more UV / VIS transparent additional surface layers 318. The UV reflective multilayer optical film 320 includes a multilayer optical stack 308 having alternating layers 312, 314 of at least two materials (typically comprising different polymers). The in-plane refractive index n1 of the high refractive index layer 312 in one in-plane direction is higher than the in-plane refractive index n2 of the low refractive index layer 314 in the same in-plane direction. The difference in refractive index at each boundary between the layers 312, 314 causes a portion of the incident light to be reflected. The transmission and reflection characteristics of the multilayer optical film 320 are based on the coherent interference of light caused by the refractive index difference between the layers 312, 314 and the thickness of the layers 312, 314. When the effective refractive index (or in-plane refractive index at normal incidence) is different between layers 312, 314, a reflective surface is formed at the interface between adjacent layers 312, 314. The reflective power of the reflective surface depends on the square of the difference in the effective refractive index of the layers 312, 314 (e.g., (n1-n2) 2 ). By increasing the refractive index difference between layers 312, 314, improved optical power (higher reflectivity), thinner films (thinner or fewer layers), and wider bandwidth performance can be achieved. In an exemplary embodiment, the refractive index difference in one in-plane direction is at least about 0.05, preferably greater than about 0.10, more preferably greater than about 0.15, and even more preferably greater than about 0.20.
[0077] In some embodiments, the materials of layers 312, 314 inherently have different refractive indices. In another embodiment, the material of at least one layer 312, 314 has stress properties that induce birefringence, such that the refractive index (n) of the material is affected by the stretching process. By stretching the multilayer optical film 320 over a range of uniaxial to biaxial orientations, films having a range of reflectivities for incident light of different orientations of plane-polarization can be produced.
[0078] For reasons of film thickness, flexibility, and economy, the number of layers in the UV reflective multilayer optical film 320 is selected to obtain the desired optical properties using the minimum number of layers. For reflective films such as mirrors, the number of layers is preferably less than about 2,000, more preferably less than about 1,000, and even more preferably less than about 750. In some embodiments, the number of layers is at least 150 or 200. In other embodiments, the number of layers is at least 250.
[0079] In some embodiments, the UV reflective multilayer optical film 320 further includes optional additional non-optical layers or optical skin layers. The optical skin layer 318 can protect the optical layers 312, 314 from damage, facilitate coextrusion processing, and / or improve post-processing mechanical properties. The additional skin layer 318 is typically thicker than the optical layers 312, 314. The thickness of the skin layer 318 is typically at least twice, preferably at least four times, and more preferably at least ten times the thickness of each optical layer 312, 314. The thickness of the skin layer 318 can be varied to prepare a UV reflective multilayer optical film having a specific thickness. A bonding layer (not shown) may optionally be present between the skin layer and the optical layer. In addition, an optional top coating may be provided on the skin layer. One or more additional layers 318 are typically provided so that at least a portion of the light transmitted, polarized and / or reflected through the optical layers 312, 314 also passes through the additional layer (i.e., the additional layer is provided in the path of the light passing through the optical layers 312, 314 or reflected by the optical layers 312, 314). In order to provide a degree of anti-fouling properties, one or both of the skin layers (preferably at least the outermost skin layer) comprises a fluoropolymer.
[0080] Thus, in some embodiments, the multilayer optical film can provide a UV protection layer 20; and in some specific embodiments, the multilayer optical film (e.g., in a manner that includes a fluorinated outermost layer) can provide an anti-soiling layer 30. This is another example of an arrangement in which a layer (or at least a portion thereof) can function as both a UV protection layer 20 and an anti-soiling layer 30.
[0081] The UV reflective multilayer optical film 320 includes a plurality of low / high refractive index film layer pairs, wherein the combined optical thickness of each low / high refractive index layer pair 312, 314 is 1 / 2 of the center wavelength of the spectral band it is designed to reflect. Such film stacks are often referred to as quarter-wave stacks. In some embodiments, different low / high refractive index layer pairs may have different combined optical thicknesses, such as in the case of an optical film requiring broadband reflection.
[0082] Each constituent layer of the UV reflective multilayer optical film 320, whether skin layers or optical layers, is preferably resistant to ultraviolet radiation. Many fluoropolymers are resistant to UV radiation.
[0083] Examples of fluoropolymers that can be used include copolymers of tetrafluoroethylene (TFE), hexafluoropropylene (HFP), and vinylidene fluoride (e.g., available under the trade designation 3M DYNEON THV from 3M Company); copolymers of TFE, HFP, vinylidene fluoride, and perfluoropropyl vinyl ether (PPVE) (e.g., available under the trade designation 3M DYNEON THVP from 3M Company); polyvinylidene fluoride (PVDF) (e.g., available under the trade designation 3M DYNEON PVDF 6008 from 3M Company); ethylene-chlorotrifluoroethylene (ECTFE) (e.g., available under the trade designation HALAR 350LC ECTFE from Solvay, Brussels, Belgium); ethylene tetrafluoroethylene (ETFE) (e.g., available under the trade designation 3M DYNEON ETFE 6235 from 3M Company); Company); perfluoroalkoxyalkane polymer (PFA); fluorinated ethylene propylene copolymer (FEP); polytetrafluoroethylene (PTFE); copolymers of TFE, HFP and ethylene (HTE) (for example, 3M DYNEON HTE1705 available from 3M Company). Combinations of fluoropolymers may also be used. In some embodiments, the fluoropolymer includes FEP. In some embodiments, the fluoropolymer includes PFA.
[0084] Examples of non-fluorinated polymers that can be used in at least one layer of the UV-reflective multilayer optical film 320 include at least one of the following: polypropylene, polyethylene, polyethylene copolymers, polyethylene methacrylate copolymers, ethylene vinyl acetate copolymers, polymethyl methacrylate, methyl methacrylate copolymers (e.g., copolymers of ethyl acrylate and methyl methacrylate), polyurethane, extended chain polyethylene polymers (ECPE), or combinations thereof. In general, combinations of non-fluorinated polymers can be used.
[0085] Exemplary non-fluorinated polymers, particularly for high refractive index optical layers, can include homopolymers of polymethyl methacrylate (PMMA), such as those available from Ineos Acrylics, Inc., Wilmington, Delaware as CP71 and CP80; and polyethyl methacrylate (PEMA), which has a lower glass transition temperature than PMMA. Other useful polymers include copolymers of methyl methacrylate, such as, for example, copolymers made from 75% by weight methyl methacrylate and 25% by weight ethyl acrylate, such as those available from Ineos Acrylics, Inc., Wilmington, Delaware as PERSPEX CP63, or from Arkema, Philadelphia, Pennsylvania as ALTUGLAS 510, and copolymers of methyl methacrylate monomer units and n-butyl methacrylate monomer units. Blends of PMMA and PVDF may also be used.
[0086] Suitable triblock acrylic copolymers are available, for example, as KURARITY LA4285 from Kuraray America Inc., Houston, Texas. Other suitable polymers for optical layers, particularly for refractive index optical layers, may include at least one of the following: polyolefin copolymers, such as poly(ethylene-co-octene) (e.g., available as ENGAGE 8200 from Dow Elastomers, Midland, Michigan); polyethylene methacrylate (e.g., available as ELVALOY from Dow Elastomers); poly(propylene-co-ethylene) (e.g., available as Z9470 from Atofina Petrochemicals, Inc., Houston, Texas); and copolymers of atactic and isotactic polypropylene. Materials may be selected based on the absorptivity properties or transmittance properties described herein and based on the refractive index. Generally speaking, the greater the refractive index between the two materials, the thinner the film can be, which can be ideal for efficient heat transfer.
[0087] Multilayer optical films (including reflective polarizers and mirrors) can be prepared, for example, by coextruding alternating polymer layers having different refractive indices as described in U.S. Pat. Nos. 5,882,774 (Jonza et al.); 6,045,894 (Jonza et al.); 6,368,699 (Gilbert et al.); 6,531,230 (Weber et al.); 6,667,095 (Wheatley et al.); 6783349 (Neavin et al.); 7,271,951B2 (Weber et al.); 7,632,568 (Padiyath et al.); 7,652,736 (Padiyath et al.); and 7,952,805 (McGurran et al.); and PCT Publications WO 95 / 17303 (Ouderkirk et al.) and WO 99 / 39224 (Ouderkirk et al.).
[0088] In a preferred embodiment, the UV-reflective multilayer optical film reflects a wavelength range of 340 nanometers to 400 nanometers and is made of a 150 high refractive index layer comprising a methyl methacrylate copolymer (CoPMMA) (e.g., available as PERSPEX CP63 from Lucite International, Cordova, Tennessee) and a 150 low refractive index layer comprising a fluoropolymer (e.g., available as 3M DYNEON THV221 from 3M Company). In some preferred embodiments, at least one of the optical layers 312 and 314 of the UV-reflective multilayer optical film may include a UV blocking additive (e.g., a UV absorber of the general type described in detail later herein). In some preferred embodiments, at least one of the non-optical layers (e.g., skin layer 318) of the UV-reflective multilayer optical film may include a UV blocking additive, such as a UV absorber.
[0089] Anti-fouling layer
[0090] The composite cooling membrane 1 includes an antifouling layer 30 including an outwardly exposed surface 31. In some embodiments, the antifouling layer 30 may be composed of or consist of one or more fluoropolymers, including copolymers, blends of multiple fluoropolymers, etc. Examples of fluoropolymers that can be used include copolymers of tetrafluoroethylene (TFE), hexafluoropropylene (HFP), and vinylidene fluoride (e.g., available as 3M DYNEON THV from 3M Company); copolymers of TFE, HFP, vinylidene fluoride, and perfluoropropyl vinyl ether (PPVE) (e.g., available as 3M DYNEON THVP from 3M Company); polyvinylidene fluoride (PVDF) (e.g., available as 3M DYNEON PVDF 6008 from 3M Company); ethylene-chlorotrifluoroethylene (ECTFE) (e.g., available as HALAR 350LC ECTFE from Solvay, Brussels, Belgium); ethylene tetrafluoroethylene (ETFE) (e.g., available as 3M DYNEON ETFE 6235 from 3M Company); Company); perfluoroalkoxyalkane polymer (PFA); fluorinated ethylene propylene copolymer (FEP); polytetrafluoroethylene (PTFE); copolymers of TFE, HFP and ethylene (HTE) (for example, 3MDYNEON HTE1705 available from 3M Company). Combinations of fluoropolymers may also be used. In some embodiments, the fluoropolymer includes FEP. In some embodiments, the fluoropolymer includes PFA. In some embodiments, the anti-fouling layer 30 may include a single layer (e.g., of a fluoropolymer) bonded to the reflective layer 10 via a PSA layer (which, as described, may serve as a UV protective (e.g., UV absorbing) layer 20), such as Figure 1 The same as in the exemplary arrangement of .
[0091] In a particular embodiment in which the cooling film 1 comprises a multilayer structure 25 of the general type described earlier herein, the structure 25 may comprise, for example, a combination of an outward-most fluoropolymer layer providing an antifouling layer 30 and one or more inward layers of any suitable composition. Such inward layers may be fluoropolymer layers or non-fluoropolymer layers. Examples of non-fluoropolymers that may be used include at least one of polypropylene, polyethylene, polyethylene copolymers, polyethylene methacrylate copolymers, ethylene vinyl acetate copolymers, polymethyl methacrylate, methyl methacrylate copolymers (e.g., copolymers of ethyl acrylate and methyl methacrylate), polyurethanes and cross-linked polyurethanes, extended chain polyethylene polymers (ECPE), polysiloxanes and cross-linked polysiloxanes, and combinations thereof. In general, combinations of non-fluorinated polymers may be used.
[0092] Exemplary non-fluorinated polymers may include homopolymers of polymethyl methacrylate (PMMA), such as those available from Ineos Acrylics, Inc., Wilmington, Delaware as CP71 and CP80; and polyethyl methacrylate (PEMA). Other useful polymers include copolymers of methyl methacrylate, such as, for example, copolymers made from 75% by weight methyl methacrylate and 25% by weight ethyl acrylate, such as those available from Ineos Acrylics, Inc., Wilmington, Delaware as PERSPEX CP63, or those available from Arkema, Philadelphia, Pennsylvania as ALTUGLAS 510, and copolymers of methyl methacrylate monomer units and n-butyl methacrylate monomer units. It has been found that polymethyl methacrylate and similar polymers may advantageously exhibit the ability to accept high levels of UV blocking additives therein if it is desired to have a layer of the multilayer structure 25 function as a UV absorbing layer 20. In some embodiments, blends of PMMA and PVDF may be used.
[0093] In the embodiment where the cooling film 1 includes a multilayer structure 25, it may be advantageous to have physical and chemical properties on the outward surface and / or layer of the structure that are different from the physical and chemical properties on the inward layer of the structure. For example, highly fluorinated polymers are beneficial to stain resistance, chemical resistance and stain resistance, but inherently cannot adhere well to other polymers or adhesives. Therefore, in the multilayer structure 25, the first outermost fluoropolymer layer with a high tetrafluoroethylene (TFE) content can be used as the outermost anti-fouling layer 30. The second fluoropolymer layer can have a lower content of TFE and still adhere well to the first fluoropolymer layer. If the second fluoropolymer layer also includes vinylidene fluoride (VDF), it will adhere well to other fluoropolymers including VDF, such as polyvinylidene fluoride (PVDF). If the second fluoropolymer layer includes enough VDF, it will adhere well to a non-fluorinated third polymer layer, such as an acrylate polymer and even a urethane polymer. Such a third polymer layer may be particularly suitable for carrying a UV blocking additive.
[0094] Therefore, this method can provide Figure 33 and discussed elsewhere herein (wherein the multilayer structure 25 provides a first layer 30, a second layer 26, and a third layer 20). It should be understood that such methods are not limited to, for example, multilayer structures having a total of three layers and / or having two fluoropolymer layers. Instead, any number of fluoropolymer layers and / or other composition layers may be used as desired. Useful multilayer structures including fluoropolymer layers that may prove useful for antifouling applications (and may include surface textures that further enhance antifouling properties) are described in U.S. Patent Application Publication No. 2019-0111666, which is incorporated herein by reference in its entirety.
[0095] In some embodiments, the exemplary multilayer stack as used in cooling film 1 may include a first layer, a second layer and a third layer. In a particular embodiment, the first layer (outermost layer) comprises a first polymer, based on the total mole % of the first polymer, the first polymer comprises at least 35 mole % of tetrafluoroethylene comonomer, at least 15 mole % of vinylidene fluoride comonomer and at least 5 mole % of hexafluoropropylene comonomer. The second layer comprises a second polymer, based on the total mole % of the second polymer, the second polymer comprises at least 50 mole % of vinylidene fluoride comonomer. The third layer comprises a third polymer, based on the total mole % of the third polymer, the third polymer comprises at least 50 mole % of methyl methacrylate comonomer. Optionally, the third layer comprises polyurethane.
[0096] In various embodiments, the first polymer of the first layer may include at least 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, or even up to 80 mol% of tetrafluoroethylene comonomer, at least 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, or even up to 50 mol% of vinylidene fluoride comonomer, and at least 10 mol%, 15 mol%, or even at least 20 mol% of hexafluoropropylene comonomer, based on the total mol% of the first polymer. In some embodiments, the first polymer may include at least 0.5 mol%, 1 mol%, 5 mol%, 10 mol%, 25 mol%, or even 50 mol% of perfluorovinyl ether comonomer, based on the total mol% of the first polymer.
[0097] Exemplary fluoropolymers for use in the first layer include those available from 3M Dyneon, Oakdale, MN, under the trade designations “Fluoroplastic Particles THV221GZ” (39 mol % tetrafluoroethylene, 11 mol % hexafluoropropylene, and 50 mol % vinylidene fluoride), “Fluoroplastic Particles THV2030GZ” (46.5 mol % tetrafluoroethylene, 16.5 mol % hexafluoropropylene, 35.5 mol % vinylidene fluoride, and 1.5 mol % perfluoropropyl vinyl ether), “Fluoroplastic Particles THV610GZ” (61 mol % tetrafluoroethylene, 10.5 mol % hexafluoropropylene, and 28.5 mol % vinylidene fluoride), and “Fluoroplastic Particles THV815GZ” (72.5 mol % tetrafluoroethylene, 7 mol % hexafluoropropylene, 19 mol % vinylidene fluoride, and 1.5 mol % perfluoropropyl vinyl ether).
[0098] In various embodiments, the second polymer of the second layer may include at least 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, 85 mol%, 90 mol%, 95 mol%, or even 100 mol% of a vinylidene fluoride comonomer, based on the total mole % of the second polymer. In some embodiments, the second polymer includes at least 0.5 (in some embodiments, 0.5 to 50, 1 to 50, 1 to 40, 1 to 30, 1 to 25, 1 to 20, or even 1 to 10) mol% of a perfluorovinyl ether comonomer, at least 0.5 (in some embodiments, in the range of 0.5 to 50, 0.5 to 25, 1 to 25, or even 1 to 20) mol% of a hexafluoropropylene comonomer, at least 0.5 (in some embodiments, in the range of 0.5 to 50, 0.5 to 25, 1 to 25, or even 1 to 20) mol% of a poly(vinylidene fluoride) comonomer, based on the total mole % of the second layer. 20) mole % of chlorotrifluoroethylene comonomer, at least 0.1 (in some embodiments, at least 0.2, 0.3, 0.4, 0.5, or even at least 1; in some embodiments, 0.1 to 10, 1 to 20, 1 to 10, or even 1 to 5) weight % of UV absorbing additives, and / or at least 0.05 (in some embodiments, at least 0.1, 0.3, 0.4, 0.5, or even at least 1; in some embodiments, 0.05 to 5, 0.1 to 5, or even 0.1 to 2) weight % of hindered amine light stabilizer (HALS). Exemplary embodiments of the second layer include a UVA oligomer and an optional HALS oligomer.
[0099] Exemplary fluoropolymers for the second layer include those available from 3M Dyneon, Oakdale, MN, under the trade designations "3M DYNEON Fluoroplastic 6008 / 0001," "3M DYNEON Fluoroplastic 11010 / 0000," and "3M DYNEON Fluoroplastic 31508 / 0001."
[0100] In some embodiments, the first layer and / or the second layer of the multilayer fluoropolymer films described herein further comprise inorganic particles (eg, titanium dioxide, zinc oxide, and / or zirconium dioxide).
[0101] In various embodiments, the third polymer of the third layer comprises at least 50 (in some embodiments, 55, 60, 65, 70, 75, 80, 85, 90, 95, or even 100; in some embodiments, in the range of 50 to 100, 75 to 100, or even 85 to 100) mole % of methyl methacrylate comonomer, based on the total weight of the third polymer, and / or at least 0.1 (in some embodiments, at least 0.2, 0.3, 0.4, 0.5, 1, 5, 10, 15, 20, or even at least 25; in some embodiments, in the range of 0.1 to 50, 1 to 40, 10 to 40, 10 to 30) weight % of butyl acrylate comonomer, based on the total weight of the third polymer. In some embodiments, the third layer comprises polyurethane as the third polymer. In some embodiments, the third layer further comprises at least 0.1 (in some embodiments, at least 0.2, 0.3, 0.4, 0.5, or even at least 1; in some embodiments, 0.1 to 10, 1 to 20, 1 to 10, or even 1 to 5) weight % of a UV absorbing additive, at least 0.05 (in some embodiments, at least 0.1, 0.3, 0.4, 0.5, or even at least 1; in some embodiments, 0.05 to 5, 0.1 to 5, or even 0.1 to 2) weight % of a hindered amine light stabilizer (HALS). Exemplary embodiments of the third layer comprise a UVA oligomer and an optional HALS oligomer.
[0102] Exemplary polymers for the third layer include polymethyl methacrylate (PMMA) (e.g., available under the trade designation "VO44" from Arkema, Bristol, PA), PMMA-butyl acrylate block copolymer (e.g., available under the trade designation "LA4285" from Kuraray Ltd., Osaka, Japan), and polymer blends thereof.
[0103] This type of multilayer structure is described in more detail in U.S. Patent Application Publication No. 2019-0111666, which is incorporated herein by reference in its entirety. When such a multilayer structure is used in the cooling film 1, in many embodiments, the first layer can be used as the outermost anti-fouling layer 30, wherein the third layer is used as the ultraviolet absorbing layer 20, and wherein the second layer is used as a bonding layer therebetween. If desired, the outermost surface 31 of the first layer can be textured to enhance anti-fouling.
[0104] Any such multilayer structures 25 can be disposed atop the reflective layer 10 in any suitable manner. As noted, in some embodiments, the multilayer structures 25 can be coextruded atop the reflective layer 10 so that the rearward-facing surface of the innermost layer of the structures 25 is bonded thereto, such as melt-bonded thereto. The composition of the innermost layer of the multilayer structures 25 can be selected so as to provide enhanced bonding to a particular reflective layer 10. In some cases, an intermediate layer (e.g., a tie layer) can be deposited atop the reflective layer 10 to provide a surface for the multilayer structures 25 to bond to more easily.
[0105] In other embodiments, the multilayer structure 25 can be a preformed structure (e.g., made by coextrusion) that is then bonded (e.g., laminated via a pressure sensitive adhesive) to the reflective layer 10. (Again, if desired, an intermediate layer (e.g., a tie layer) can be disposed atop a major surface of the reflective layer 10, with the composition of the tie layer being selected to enhance bonding of the pressure sensitive adhesive thereto).
[0106] It should be emphasized that the layer to be loaded with, for example, a UV blocking additive (e.g., a UV absorbing additive) does not necessarily have to be, for example, a PMMA homopolymer. For example, in some embodiments, the layer may take the form of a copolymer or blend of a fluoropolymer and an organic polymer (e.g., a blend of PVDF and PMMA), to which a UV blocking additive is added. In fact, some UV blocking additives (e.g., UV absorbing additives) that are compatible with fluoropolymers having a high fluorine content (even, for example, PVDF) are available. Such arrangements are disclosed in, for example, U.S. Patents 9,670,300 and 10,125,251, both of which are incorporated herein by reference in their entirety. Therefore, in some embodiments, a fluoropolymer layer such as, for example, PVDF may be loaded with a suitable UV blocking additive. The additive may enhance the inherent UV resistance of the fluoropolymer, and may also enable the fluoropolymer layer to protect a reflective layer arranged backward from the fluoropolymer layer. In various embodiments, such a UV protective layer may be a layer of a multilayer structure; alternatively, it may be a single independent layer that is not, for example, a part of an extruded multilayer structure. Thus, such a layer can serve as both a UV protection layer 20 and an anti-fouling layer 30, and thus can allow for the realization of Figure 2 The general type of arrangement depicted in .
[0107] In some embodiments, the UV protective (e.g., UV absorbing) layer 20 and / or the anti-fouling layer 30 may take the form of a coating on the outward side of the reflective layer 10 (or on the outward side of any layer present thereon). Such coatings may be obtained by disposing a precursor coating composition atop the layer 10 and then hardening the precursor (e.g., by removing the solvent or any liquid carrier, by crosslinking, etc.) to form the final coating. The placement of the precursor may be performed in any suitable manner; for example, knife coating, gravure coating, slide coating, slot die coating, curtain coating, etc. The resulting coating may have protective properties (e.g., providing wear resistance, scratch resistance, etc.); such coatings are generally referred to as hard coatings, and this term will be used herein. A plurality of such general types of coatings are known in the art, including, for example, those described in the following patents: U.S. Patent Application Publication 2015 / 0175479 (Brown et al.), U.S. Patent Nos. 6,277,485 (Invie et al.) and 6,991,826 (Pellerite et al.) and WO 02 / 12404 (Liu et al.). Commercially available hard coatings include products purchased from Mitsubishi Chemicals under the trade name SHIKOH, and products purchased from California Hardcoating Company, Chula Vista, CA, under the trade name PERMA-NEW. Some such hard coatings may be of the general type described in U.S. Patent No. 6,265,029.
[0108] In some embodiments, such a hard coating layer may be used only as an anti-fouling layer 30, rather than a UV absorbing layer protecting the reflective layer 10. In such embodiments, little or no UV blocking additive may be present in the layer 30 (e.g., only as much as may be required for the stabilization layer 30 itself, if any). If desired, in some embodiments, the outwardly facing surface 31 of such a hard coating layer may be textured to enhance the anti-fouling properties of the hard coating layer. In some embodiments, such a hard coating layer may be used as both a UV absorbing layer 20 and an anti-fouling layer 30 (e.g., Figure 2 In such embodiments, the hard coating may include any suitable UV blocking additive in appropriate amounts and types, including any of the UV blocking additives specifically mentioned herein. If desired, the hard coating may include a textured surface 31 for the above purposes.
[0109] In some embodiments, the hard coat layer can be based on a coating composition that is at least partially dependent on a methacrylate material. For example, in some embodiments, the coating composition can include a poly (methyl methacrylate) (PMMA) polymer, which can be a homopolymer or a copolymer. The PMMA polymer or copolymer has a weight average molecular weight of at least 50,000 g / mol. In some embodiments, the PMMA polymer or copolymer has a weight average molecular weight of at least 75,000 g / mol, 100,000 g / mol, 120,000 g / mol, 125,000 g / mol, 150,000 g / mol, 165,000 g / mol, or 180,000 g / mol. The PMMA polymer or copolymer can have a weight average molecular weight of at most 500,000 g / mol, in some embodiments, a weight average molecular weight of at most 400,000 g / mol, and in some embodiments, a weight average molecular weight of at most 250,000 g / mol. The weight average molecular weight can be measured using techniques known in the art, such as by gel permeation chromatography (ie, size exclusion chromatography (SEC)).
[0110] The available copolymers of PMMA include those made by C2-C8 alkyl acrylate or methacrylate or C3-C8 cycloalkyl acrylate or methacrylate in combination with methyl methacrylate. In some embodiments, the copolymer of PMMA includes at least one of ethyl acrylate, ethyl methacrylate, butyl acrylate or butyl methacrylate. In some embodiments, the copolymer is made from a starting monomer, and the starting monomer comprises methyl methacrylate in the range of 50 wt % to 90 wt % (in some embodiments, 60 wt % to 85 wt %) and C2-C8 alkyl acrylate or methacrylate or C3-C8 cycloalkyl acrylate or methacrylate in the range of 10 wt % to 50 wt % (in some embodiments, 15 wt % to 40 wt %) based on the gross weight of the monomer. In some embodiments in these embodiments, C2-C8 alkyl acrylate or methacrylate or C3-C8 cycloalkyl acrylate or methacrylate is ethyl acrylate or n-butyl methacrylate. Useful copolymers of PMMA are commercially available, for example, under the trade designation "PARALOID" from Dow Chemical Company, Midland, Mich., and under the trade designations "PERSPEX" and "ELVACITE" from Lucite International, Inc., Memphis, Tenn. In some embodiments, the use of a copolymer of methyl methacrylate and n-butyl methacrylate in the coating composition can improve the abrasion resistance of the resulting hardcoat.
[0111] PMMA polymers or copolymers are linear polymers or copolymers and are generally non-functional. That is, PMMA polymers or copolymers generally do not contain reactive functional groups, such as carboxylic acid, sulfonic acid, amino groups, and polymerizable carbon-carbon double bonds.
[0112] The coating composition according to the present disclosure may include, for example, an alkylene diacrylate, an alkylene dimethacrylate, a cycloalkylene diacrylate, or a cycloalkylene dimethacrylate. The alkylene diacrylate, alkylene dimethacrylate, cycloalkylene diacrylate, or cycloalkylene dimethacrylate may conveniently be liquid at room temperature. The alkylene diacrylate or dimethacrylate is typically a C2-C4 alkylene diacrylate having no substituents on the alkylene or cycloalkylene groups. 10 Alkylene diacrylate or dimethacrylate or C4-C6 cycloalkylene diacrylate or dimethacrylate. According to definition, the alkylene group in diacrylate or dimethacrylate does not include any heteroatoms or functional groups inserted into the carbon chain, and according to definition, the cycloalkylene group in diacrylate or dimethacrylate does not include any heteroatoms in the ring. The alkylene group can be straight chain or branched. Not bound by theory, in some embodiments, it is believed that the branching in the alkylene group can lead to a cured coating with a lower modulus, which can increase the wear resistance of the cured coating composition. Available difunctional acrylates and methacrylates include hexanediol diacrylate, hexanediol dimethacrylate, neopentyl glycol diacrylate and neopentyl glycol dimethacrylate. It has been found that the coating composition disclosed herein has good adhesion to many polymer substrates after curing even in the absence of, for example, alkyleneoxy groups in acrylic monomers.
[0113] In the coating composition, alkylene diacrylate, alkylene dimethacrylate, cycloalkylene diacrylate and / or cycloalkylene dimethacrylate can provide, for example, at least 80% by weight of monomers. In some embodiments, alkylene diacrylate, alkylene dimethacrylate, cycloalkylene diacrylate and / or cycloalkylene dimethacrylate provide at least 85, 90, 95, 96, 97, 98, 99 or even 100% by weight of monomers. In other words, in addition to alkylene diacrylate, alkylene dimethacrylate, cycloalkylene diacrylate and / or cycloalkylene dimethacrylate, based on the total weight of monomers in the coating composition, monomers (e.g., acrylic monomers) constitute no more than (e.g., less than) 20, 15, 10, 5, 4, 3, 2 or 1% by weight. In some embodiments, in addition to alkylene diacrylate, alkylene dimethacrylate, cycloalkylene diacrylate, and / or cycloalkylene dimethacrylate, the coating composition can be considered to be substantially free of monomers (e.g., acrylic monomers). In some embodiments, the monomers in the coating composition can be considered to consist of alkylene diacrylates, alkylene dimethacrylates, cycloalkylene diacrylates, cycloalkylene dimethacrylates, or combinations thereof.
[0114] In many embodiments, the coating compositions disclosed herein thus do not have a significant amount of monofunctional acrylates or methacrylates (e.g., greater than about 15 weight percent based on the total weight of the monomers in the coating composition). In some embodiments, the monomers include no more than 15, 10, 5, 4, 3, 2, or 1 weight percent of monofunctional acrylates or methacrylates based on the total weight of the monomers in the coating composition.
[0115] In many embodiments, the coating compositions disclosed herein also do not have a significant amount of tri-, tetra-, or higher functional acrylates or methacrylates (e.g., greater than about 10 wt % based on the total weight of monomers in the coating composition). In some embodiments, the monomers include no more than 7.5, 5, 4, 3, 2, or 1 wt % of tri-, tetra-, or higher functional acrylates or methacrylates based on the total weight of monomers in the coating composition.
[0116] In some embodiments, the hard coating prepared from the coating compositions disclosed herein has an elongation of less than 50% (in some embodiments, less than 25% or less than 10%). In some embodiments, these acrylate-based coating compositions do not contain polyurethane acrylates or contain no more than 10%, 5%, 3%, or 1% by weight of polyurethane acrylates based on the total weight of monomers in the coating composition. In addition, by definition, alkylene or cycloalkylene diacrylates or dimethacrylates are not prepared from polyurethanes and do not contain polyurethane and urea groups.
[0117] In the coating compositions disclosed herein, a variety of ratios of monomers comprising at least one of alkylene diacrylates, alkylene dimethacrylates, cycloalkylene diacrylates, or cycloalkylene dimethacrylates to poly(methyl methacrylate) polymers or copolymers may be useful. In any of the embodiments of the PMMA polymers or copolymers or monomers described above, the weight ratio of monomers comprising at least one of alkylene diacrylates, alkylene dimethacrylates, cycloalkylene diacrylates, or cycloalkylene dimethacrylates to poly(methyl methacrylate) polymers or copolymers may be in the range of 0.75:1 to 15:1. Additionally, in any of the foregoing embodiments, the monomers may be present in the composition in the range of 20 wt % to 90 wt % (in some embodiments, 20 wt % to 80 wt % or 23 wt % to 75 wt %) based on the total weight of the non-volatile components of the composition. The PMMA polymer or copolymer may be present in the composition in a range of 2 wt % to 40 wt % (in some embodiments, 4 wt % to less than 40 wt %, such as 39 wt %, 38 wt %, or 37 wt %) based on the total weight of the non-volatile components of the composition. In some embodiments (e.g., embodiments in which the coating composition does not include any filler), the weight ratio of the monomer comprising at least one of an alkylene diacrylate, an alkylene dimethacrylate, a cycloalkylene diacrylate, or a cycloalkylene dimethacrylate to the poly(methyl methacrylate) polymer or copolymer is in a range of 0.75:1 to 5:1, 1:1 to 4:1, or 1.5:1 to 3:1. In any of these embodiments, the monomer may be present in the composition in a range of 40% to 90% by weight (in some embodiments, 41%, 42%, 43%, 44%, or 45% to 90% or 80% by weight) based on the total weight of the non-volatile components of the composition, and the PMMA polymer or copolymer may be present in the composition in a range of 20% to 40% by weight (in some embodiments, 20% to less than 40% by weight, such as 39%, 38%, or 37% by weight) based on the total weight of the non-volatile components of the composition. In some embodiments (e.g., embodiments in which the coating composition includes a filler as described in more detail below), the weight ratio of the monomer comprising at least one of an alkylene diacrylate, an alkylene dimethacrylate, a cycloalkylene diacrylate, or a cycloalkylene dimethacrylate to the poly(methyl methacrylate) polymer or copolymer is in a range of 0.75:1 to 15:1, 0.75:1 to 12.5:1, or 1:1 to 10:1. Acrylate based hardcoats are described in more detail in US Pat. No. 10,072,173, which is incorporated herein by reference in its entirety.
[0118] Regardless of the specific polymer composition, in some embodiments, the hard coat layer may include inorganic particles, such as, for example, inorganic oxide particles (e.g., silica, zirconium oxide, titanium dioxide, antimony oxide, aluminum oxide, etc.). In various embodiments, any such particles may have an average size of up to, for example, 500 nanometers. Such particles may, for example, enhance the strength, mechanical durability, wear resistance, scratch resistance, etc. of the hard coat layer. In some embodiments, such particles may, for example, enhance the ability of the hard coat layer to be textured (e.g., to further enhance antifouling) by, for example, removing the organic polymer material (e.g., by etching) while the inorganic particles remain in place, thereby imparting a texture to the surface of the hard coat layer. Various inorganic particles that can be used in the hard coat layer are discussed in detail in the '173 U.S. patent cited above. The '173 patent also includes an extensive discussion of UV blocking (e.g., UV absorbing) additives that can be incorporated into the hard coat layer; it should be understood that any such additive (and generally, any of the additives disclosed elsewhere herein) may be included in the hard coat layer.
[0119] It should be understood that the above-described acrylate-based hard coatings are merely exemplary and that the composition may vary in some cases. Generally speaking, such hard coatings (whether used as UV absorbing layers, antifouling layers, or both) are not limited to acrylate-based compositions. Other potentially suitable compositions (exhibiting, for example, scratch resistance, etc.) are disclosed, for example, in U.S. Pat. No. 9,523,516, which is incorporated herein by reference in its entirety.
[0120] Regardless of the specific composition, a hardcoat layer is to be distinguished from any layer that fails to exhibit hardness, wear resistance, and durability properties commensurate with a layer that acts as a hardcoat. In some embodiments, a hardcoat layer as disclosed herein may exhibit a pencil hardness of at least 3H, 5H, 7H, or 9H (as typically obtained according to the procedure outlined in ASTM test method D3363-05 (2011) e2, for example using a GARDCO 5021 pencil hardness tester or equivalent). By definition, materials such as pressure-sensitive adhesive layers are not hardcoats as disclosed herein.
[0121] In some embodiments, a hardcoat layer (e.g., a UV absorbing textured hardcoat that provides both UV protection and antifouling) can be disposed on a suitable substrate (e.g., a MYLAR film layer) with a reflective non-porous inorganic particle-filled organic polymer layer disposed on the back side of the substrate. For example, such a reflective layer can be painted onto the back surface of the substrate.
[0122] Textured stain-resistant surface
[0123] In some embodiments, the outward-facing surface 31 of the antifouling layer 30 (i.e., opposite the reflective layer 10) can be textured on part or all of its surface for micro-structuring and / or nano-structuring; for example, as described in U.S. Provisional Patent Application No. 62 / 611,636 and the resulting PCT International Application Publication No. WO 2019 / 130198, both of which are incorporated herein by reference in their entirety. The use of such micro-structuring and / or nano-structuring for the specific purpose of enhancing antifouling of cooling films is discussed in U.S. Patent Application No. 62 / 855,392, which is incorporated herein by reference in its entirety.
[0124] In some embodiments, nanostructures can be superimposed on the microstructures on the surface of the antifouling layer. In some such embodiments, the antifouling layer has a main surface (i.e., an antifouling surface) comprising microstructures and / or nanostructures. The microstructures can be arranged as a series of alternating micropeaks and microspaces. The size and shape of the microspaces between the micropeaks can alleviate the adhesion of dirt particles to the micropeaks. The nanostructures can be arranged as at least a series of nanopeaks arranged on at least the microspaces. Micropeaks may be more resistant to environmental effects than nanopeaks. Since the micropeaks are only separated by microspaces, and the microspaces are significantly higher than the nanopeaks, the micropeaks can be used to protect the nanopeaks on the surface of the microspaces from wear and tear.
[0125] With reference to the antifouling layer, the term or prefix "micron" refers to at least one dimension of a structure or shape defined within the range of 1 micron to 1 millimeter. For example, a micron structure may have a height or width within the range of 1 micron to 1 millimeter.
[0126] As used herein, the term or prefix "nano" refers to at least one dimension defining a structure or shape that is less than 1 micrometer. For example, a nanostructure may have at least one of a height or a width that is less than 1 micrometer.
[0127] Figure 4A , Figure 4B and Figure 4C A cross section 400, 401 of an antifouling surface structure is shown, which is shown as an antifouling layer 408 having an antifouling surface 402 defined by a series of microstructures 418. Specifically, Figure 4A A perspective view of the cross section 401 relative to the xyz axis is shown. Figure 4C A cross section 401 in an xz plane parallel to an axis 410 is shown. Figure 4B A cross section 400 is shown in a yz plane that is orthogonal to the cross section 401 and to the axis 410 . FIG. 4A to FIG. 4C The anti-fouling surface 402 is shown as if the anti-fouling layer 408 is located on a flat, horizontal surface. However, the anti-fouling layer 408 can be flexible and can conform to a non-flat substrate.
[0128] In some embodiments, the microstructures 418 are formed in the antifouling layer 408. The microstructures 418 and the remainder of the antifouling layer 408 below the microstructures may be formed of the same material. The antifouling layer 408 may be formed of any suitable material capable of defining the microstructures 418, which may at least partially define the antifouling surface 402. The antifouling layer 408 may be transparent to various frequencies of light. In at least one embodiment, the antifouling layer 408 may be non-transparent or even opaque to various frequencies of light. In some embodiments, the antifouling layer 408 may include or be made of a UV stable material, and / or may include a UV blocking additive. In some embodiments, the antifouling layer 408 may include a polymer material, such as a fluoropolymer or a polyolefin polymer.
[0129] Antifouling surface 402 can extend along axis 410, e.g., parallel to or substantially parallel to axis 410. Plane 412 can contain axis 410, e.g., be parallel to or intersect axis 410, such that axis 410 is in plane 412. Axis 410 and plane 412 can both be imaginary constructions used herein to illustrate various features associated with antifouling surface 402. For example, the intersection of plane 412 and antifouling surface 402 can define a region described as follows: Figure 4C Line 414 is shown as a cross-sectional profile of a surface including micro-peaks 420 and micro-spaces 422 as described in more detail herein. Line 414 may include at least one straight segment or a curved segment.
[0130] Lines 414 may at least partially define a series of microstructures 418, which may be three-dimensional (3D) structures disposed on anti-fouling layer 408, and lines 414 may describe only two dimensions (e.g., height and width) of the 3D structures. Figure 4B As can be seen in FIG. 4 , the microstructure 418 may have a length extending from one side 430 to another side 432 along the surface 402 .
[0131] The microstructure 418 may include a series of alternating micro-peaks 420 and micro-spaces 422 along an axis 410 or in the direction of the axis 410, which axis 410 may be defined by a line 414 or included in the line 414. The direction of the axis 410 may coincide with the width dimension. The micro-spaces 422 may each be disposed between a pair of micro-peaks 420. In other words, a plurality of micro-peaks 420 may be separated from each other by at least one micro-space 422. In at least one embodiment, at least one pair of micro-peaks 420 may not include a micro-space 422 therebetween. The pattern of alternating micro-peaks 420 and micro-spaces 422 may be described as a "skipped serrated rib" (STR). Each of the micro-peaks 420 and micro-spaces 422 may include at least one straight segment or a curved segment.
[0132] The slope of line 414 (eg, rise with extension) may be defined relative to the direction of axis 410 as the x-axis (extension) and relative to the direction of plane 412 as the y-axis (rise).
[0133] A maximum absolute slope may be defined for at least a portion of the line 414. As used herein, the term "maximum absolute slope" refers to a maximum value selected from the absolute values of the slopes throughout a particular portion of the line 414. For example, the maximum absolute slope of one microspace 422 may refer to a maximum value selected from the absolute values of the slopes calculated at each point along the line 414 defining the microspace.
[0134] The line defining the maximum absolute slope of each micron space 422 can be used to define an angle relative to the axis 410. In some embodiments, the angle corresponding to the maximum absolute slope can be at most 30 degrees (in some embodiments, at most 25 degrees, 20 degrees, 15 degrees, 10 degrees, 5 degrees, or even at most 1 degree). In some embodiments, the maximum absolute slope of at least some (in some embodiments, all) of the micron peaks 420 can be greater than the maximum absolute slope of at least some (in some embodiments, all) of the micron spaces 422.
[0135] In some embodiments, line 414 may include a boundary 416 between each adjacent micron peak 420 and micron space 422. Boundary 416 may include at least one of a straight segment or a curved segment. Boundary 416 may be a point along line 414. In some embodiments, boundary 416 may include a bend. A bend may include the intersection of two segments of line 414. A bend may include a point at which line 414 changes direction in position (e.g., a change in slope between two different straight lines). A bend may also include a point at which line 414 has the sharpest change in direction in position (e.g., a sharper turn than an adjacent curved segment). In some embodiments, boundary 416 may include an inflection point. An inflection point may be a point of the line at which the direction of curvature changes.
[0136] Figure 5 The antifouling surface 402 of the antifouling layer 408 is shown with nanostructures 530, 532, which are visible in two magnified stacks. At least one micro-peak 420 may include at least one first micro-segment 424 or at least one second micro-segment 426. The micro-segments 424, 426 may be disposed on opposite sides of the apex 448 of the micro-peak 420. The apex 448 may be, for example, the highest point or local maximum of the line 414. Each micro-segment 424, 426 may include at least one: a straight segment or a curved segment.
[0137] The line 414 defining the first micro-segment 424 and the second micro-segment 426 may have a first average slope and a second average slope, respectively. The slope may be defined relative to the baseline 450 as the x-axis (extension), with the orthogonal direction being the z-axis (ascent).
[0138] As used herein, the term "average slope" refers to the average slope over a particular portion of a line. In some embodiments, the average slope of the first micro-segment 424 may refer to the slope between the endpoints of the first micro-segment. In some embodiments, the average slope of the first micro-segment 424 may refer to an average value calculated from slopes measured at multiple points along the first micro-segment.
[0139] Generally speaking, the first average slope of the micro-peak may be defined as positive, and the second average slope of the micro-peak may be defined as negative. In other words, the first average slope and the second average slope have opposite signs. In some embodiments, the absolute value of the first average slope of the micro-peak may be equal to the absolute value of the second average slope of the micro-peak. In some embodiments, the absolute values may be different. In some embodiments, the absolute value of each average slope of the micro-segments 424, 426 may be greater than the absolute value of the average slope of the micro-space 422.
[0140] Angle A of micro-peak 420 may be defined between a first average slope of the micro-peak and a second average slope of the micro-peak. In other words, a first average slope and a second average slope may be calculated, and then the angle between these calculated lines may be determined. For purposes of illustration, angle A is shown as being associated with first micro-segment 424 and second micro-segment 426. However, in some embodiments, when the first micro-segment and the second micro-segment are not straight lines, angle A may not necessarily be equal to the angle between the two micro-segments 424, 426.
[0141] Angle A can be within a range that provides sufficient anti-fouling properties for surface 202. In some embodiments, angle A can be up to 120 degrees (in some embodiments, up to 110 degrees, 100 degrees, 95 degrees, 90 degrees, 85 degrees, 80 degrees, 75 degrees, 70 degrees, 65 degrees, 60 degrees, 55 degrees, 50 degrees, 45 degrees, 40 degrees, 35 degrees, 30 degrees, 25 degrees, 20 degrees, or even up to 10 degrees). In some embodiments, angle A is up to 85 degrees (in some embodiments, up to 75 degrees). In some embodiments, angle A is at least 30 degrees at the low end (in some embodiments, at least 25 degrees, 40 degrees, 45 degrees, or even at least 50 degrees). In some embodiments, angle A is at most 75 degrees at the high end (in some embodiments, up to 60 degrees, or even up to 55 degrees).
[0142] Micro-peak 420 can be any suitable shape capable of providing angle A based on the average slope of micro-segments 424, 426. In some embodiments, micro-peak 420 is generally formed in a triangular shape. In some embodiments, micro-peak 420 is not triangular in shape. The shape can be symmetrical across the z-axis that intersects vertex 448. In some embodiments, the shape can be asymmetrical.
[0143] Each micro-space 422 may define a micro-space width 242 . The micro-space width 442 may be defined as the distance between corresponding boundaries 416 , which may be between adjacent micro-peaks 420 .
[0144] The minimum value of the micron space width 442 can be defined in microns. In some embodiments, the micron space width 442 can be at least 10 microns (in some embodiments, at least 20 microns, 25 microns, 30 microns, 40 microns, 50 microns, 60 microns, 70 microns, 75 microns, 80 microns, 90 microns, 100 microns, 150 microns, 200 microns, or even at least 250 microns). In some applications, the micron space width 442 is at least 50 microns at the low end (in some embodiments, at least 60 microns). In some applications, the micron space width 442 is at most 90 microns at the high end (in some embodiments, at most 80 microns). In some applications, the micron space width 442 is 70 microns.
[0145] As used herein, the term "peak distance" refers to the distance between consecutive peaks or between the closest pairs of peaks measured at each apex or highest point of the peaks.
[0146] The micron space width 442 may also be defined relative to the micron peak distance 440. Specifically, the minimum value of the micron space width 442 may be defined relative to the corresponding micron peak distance 440, which may refer to the distance between the nearest pair of micron peaks 420 surrounding the micron space 422 measured at each vertex 448 of the micron peak. In some embodiments, the micron space width 442 may be at least 10% (in some embodiments, at least 20%, 25%, 30%, 40%, 50%, 60%, 70%, 80%, or even at least 90%) of the maximum value of the micron peak distance 440. In some embodiments, the minimum value of the micron space width 442 is at least 30% (in some embodiments, at least 40%) of the maximum value of the micron peak distance 440 at the low end. In some embodiments, the minimum value of the micron space width 442 is at most 60% (in some embodiments, at most 50%) of the maximum value of the micron peak distance 440 at the high end. In some embodiments, micron space width 442 is 45% of micron peak distance 440 .
[0147] The minimum value of micro-peak distance 440 can be defined in microns. In some embodiments, micro-peak distance 440 can be at least 1 micron (in some embodiments, at least 2 microns, 3 microns, 4 microns, 5 microns, 10 microns, 25 microns, 50 microns, 75 microns, 100 microns, 150 microns, 200 microns, 250 microns, or even at least 500 microns). In some embodiments, micro-peak distance 440 is at least 100 microns.
[0148] The maximum value of the micron-peak distance 440 can be defined in microns. The micron-peak distance 440 can be at most 1000 microns (in some embodiments, at most 900 microns, 800 microns, 700 microns, 600 microns, 500 microns, 400 microns, 300 microns, 250 microns, 200 microns, 150 microns, 100 microns, or even at most 50 microns). In some embodiments, the micron-peak distance 440 is at most 200 microns at the high end. In some embodiments, the micron-peak distance 440 is at least 100 microns at the low end. In some embodiments, the micron-peak distance 440 is 150 microns.
[0149] Each micron peak 420 may define a micron peak height 446. Micron peak height 446 may be defined as the distance between baseline 550 and apex 448 of micron peak 420. The minimum value of micron peak height 446 may be defined in microns. In some embodiments, micron peak height 446 may be at least 10 microns (in some embodiments, at least 20 microns, 25 microns, 30 microns, 40 microns, 50 microns, 60 microns, 70 microns, 80 microns, 90 microns, 100 microns, 150 microns, 200 microns, or even at least 250 microns). In some embodiments, micron peak height 446 is at least 60 microns (in some embodiments, at least 70 microns). In some embodiments, micron peak height 446 is 80 microns.
[0150] The plurality of nanostructures 530, 532 may be at least partially defined by the wire 414. The plurality of nanostructures 530 may be disposed on at least one micron space 422. Specifically, the wire 514 defining the nanostructures 530 may include at least one series of nanopeaks 520 disposed on at least one micron space 422. In some embodiments, at least one series of nanopeaks 520 of the plurality of nanostructures 532 may also be disposed on at least one micropeak 420.
[0151] At least due to their size difference, microstructures 418 can be more durable in terms of wear resistance than nanostructures 530, 532. In some embodiments, plurality of nanostructures 532 are disposed only on microspaces 422, or at least not disposed proximal or adjacent to apex 448 of micropeak 420.
[0152] Each nanopeak 520 may include at least one of a first nanosegment 524 and a second nanosegment 526. Each nanopeak 520 may include both nanosegments 524, 526. The nanosegments 524, 526 may be disposed on opposite sides of an apex 548 of the nanopeak 520.
[0153] The first nanosegment 524 and the second nanosegment 526 can define a first average slope and a second average slope, respectively, which describe the line 514 defining the nanosegment. For the nanostructures 530, 532, the slope of the line 514 can be defined relative to the baseline 550 as the x-axis (extension), with the orthogonal direction being the z-axis (rise).
[0154] Generally speaking, the first average slope of the nanopeak may be defined as positive, and the second average slope of the nanopeak may be defined as negative, or vice versa. In other words, the first average slope and the second average slope have at least opposite signs. In some embodiments, the absolute value of the first average slope of the nanopeak may be equal to the absolute value of the second average slope of the nanopeak (e.g., nanostructure 530). In some embodiments, the absolute values may be different (e.g., nanostructure 532).
[0155] Angle B of nanopeak 520 can be defined between lines defined by the first average slope of the nanopeak and the second average slope of the nanopeak. Similar to angle A, angle B is shown for illustrative purposes and may not necessarily be equal to any directly measured angle between nanosegments 524, 526.
[0156] Angle B can be within a range that provides sufficient anti-fouling properties for surface 402. In some embodiments, angle B can be at most 120 degrees (in some embodiments, at most 110 degrees, 100 degrees, 90 degrees, 85 degrees, 80 degrees, 75 degrees, 70 degrees, 65 degrees, 60 degrees, 55 degrees, 50 degrees, 45 degrees, 40 degrees, 35 degrees, 30 degrees, 25 degrees, 20 degrees, or even at most 10 degrees). In some embodiments, angle B is at most 85 degrees at the high end (in some embodiments, at most 80 degrees, or even at most 75 degrees). In some embodiments, angle B is at least 55 degrees at the low end (in some embodiments, at least 60 degrees, or even at least 65 degrees). In some embodiments, angle B is 70 degrees.
[0157] Angle B may be the same or different for each nano-peak 520. For example, in some embodiments, angle B of nano-peak 520 on micro-peak 420 may be different from angle B of nano-peak 520 on micro-space 422.
[0158] Nanopeak 520 may be any suitable shape capable of providing angle B based on a line defined by the average slope of nanosegments 524, 526. In some embodiments, nanopeak 520 is generally formed in a triangular shape. In at least one embodiment, nanopeak 520 is not in a triangular shape. The shape may be symmetrical across vertex 548. For example, nanopeak 520 of nanostructure 530 disposed on micron space 422 may be symmetrical. In at least some embodiments, the shape may be asymmetrical. For example, nanopeak 520 of nanostructure 532 disposed on micron peak 420 may be asymmetrical, wherein one nanosegment 524 is longer than another nanosegment 526. In some embodiments, nanopeak 520 may be formed without undercut.
[0159] Each nanopeak 520 can define a nanopeak height 546. Nanopeak height 546 can be defined as the distance between baseline 550 and apex 548 of nanopeak 520. The minimum value of nanopeak height 546 can be defined in nanometers. In some embodiments, nanopeak height 546 can be at least 10 nanometers (in some embodiments, at least 50 nanometers, 75 nanometers, 100 nanometers, 120 nanometers, 140 nanometers, 150 nanometers, 160 nanometers, 180 nanometers, 200 nanometers, 250 nanometers, or even at least 500 nanometers).
[0160] In some embodiments, nanopeak height 546 is at most 250 nanometers (in some embodiments, at most 200 nanometers), particularly for nanostructures 530 on micron spaces 422. In some embodiments, nanopeak height 546 is in the range of 100 nanometers to 250 nanometers (in some embodiments, 160 nanometers to 200 nanometers). In some embodiments, nanopeak height 546 is 180 nanometers.
[0161] In some embodiments, nanopeak height 546 is at most 160 nanometers (in some embodiments, at most 140 nanometers), particularly for nanostructures 532 on micro-peak 420. In some embodiments, nanopeak height 546 is in the range of 75 nanometers to 160 nanometers (in some embodiments, 100 nanometers to 140 nanometers). In some embodiments, nanopeak height 546 is 120 nanometers.
[0162] As used herein, the term "corresponding micro-peak" or "corresponding micro-peaks" refers to the micro-peak 420 on which the nano-peak 520 is disposed, or if the nano-peak is disposed on the corresponding micro-space 422, it refers to one or both of the nearest micro-peaks surrounding the micro-space. In other words, the micro-peak 420 corresponding to the micro-space 422 refers to the micro-peak in a series of micro-peaks before and after the micro-space.
[0163] Nanopeak height 546 may also be defined relative to micropeak height 446 of corresponding micropeak 420. In some embodiments, corresponding micropeak height 446 may be at least 10 times (in some embodiments, at least 50 times, 100 times, 150 times, 200 times, 300 times, 400 times, 500 times, 600 times, 700 times, 800 times, 900 times, or even at least 1000 times) greater than nanopeak height 546. In some embodiments, corresponding micropeak height 446 is at least 300 times (in some embodiments, at least 400 times, 500 times, or even at least 600 times) greater than nanopeak height 546 at the low end. In some embodiments, corresponding micropeak height 446 is at most 900 times (in some embodiments, at most 800 times, or even at most 700 times) greater than nanopeak height 546 at the high end.
[0164] Nanopeak distance 540 may be defined between nanopeaks 520. A maximum value for nanopeak distance 540 may be defined. In some embodiments, nanopeak distance 540 may be at most 1000 nanometers (in some embodiments, at most 750 nanometers, 700 nanometers, 600 nanometers, 500 nanometers, 400 nanometers, 300 nanometers, 250 nanometers, 200 nanometers, 150 nanometers, or even at most 100 nanometers). In some embodiments, nanopeak distance 540 is at most 400 nanometers (in some embodiments, at most 300 nanometers).
[0165] A minimum value for nanopeak distance 540 may be defined. In some embodiments, nanopeak distance 540 may be at least 1 nanometer (in some embodiments, at least 5 nanometers, 10 nanometers, 25 nanometers, 50 nanometers, 75 nanometers, 100 nanometers, 150 nanometers, 200 nanometers, 250 nanometers, 300 nanometers, 350 nanometers, 400 nanometers, 450 nanometers, or even at least 500 nanometers). In some embodiments, nanopeak distance 540 is at least 150 nanometers (in some embodiments, at least 200 nanometers).
[0166] In some embodiments, nanopeak distance 540 is in the range of 150 nanometers to 400 nanometers (in some embodiments, 200 nanometers to 300 nanometers). In some embodiments, nanopeak distance 540 is 250 nanometers.
[0167] Nanopeak distance 540 can be defined relative to micropeak distance 440 between corresponding micropeaks 420. In some embodiments, corresponding micropeak distance 440 is at least 10 times (in some embodiments, at least 50 times, 100 times, 200 times, 300 times, 400 times, 500 times, 600 times, 700 times, 800 times, 900 times, or even at least 1000 times) greater than nanopeak distance 540. In some embodiments, corresponding micropeak distance 440 is at least 200 times (in some embodiments, at least 300 times) greater than nanopeak distance 540 at the low end. In some embodiments, corresponding micropeak distance 440 is at most 500 times (in some embodiments, at most 400 times) greater than nanopeak distance 540 at the high end.
[0168] In some embodiments of forming an antifouling surface, the method may include extruding a hot melt material with a UV stable material. The extruded material may be formed with a micro-replication tool. The micro-replication tool may include a mirror image of a series of micro-structures that may form a series of micro-structures on the surface of the antifouling layer 208. The series of micro-structures may include a series of alternating micro-peaks and micro-spaces along an axis. A plurality of nano-structures may be formed on the surface of the layer on at least the micro-spaces. The plurality of nano-peaks may include at least one series of nano-peaks along an axis.
[0169] In some embodiments, a plurality of nanostructures can be formed by exposing the surface to reactive ion etching.For example, a masking element can be used to define nanopeaks.
[0170] In some embodiments, the plurality of nanostructures may be formed by shaping the extruded material with a microreplication tool that also has ion-etched diamond. The method may involve providing a diamond tool, wherein at least a portion of the tool includes a plurality of tool tips, wherein the tool tips may be spaced less than 1 micron apart; and cutting the substrate with the diamond tool, wherein the diamond tool may move in and out in a certain direction at a spacing (p1). The diamond tool may have a maximum cutter width (p2), and
[0171] The nanostructures can be characterized as being embedded within the microstructured surface of the antifouling layer.Except for the portions of the nanostructures that are exposed to air, the shapes of the nanostructures can generally be defined by the adjacent microstructured material.
[0172] The microstructured surface layer including nanostructures can be formed by using a multi-tip diamond tool. A diamond turning machine (DTM) can be used to generate a micro-replication tool, which is used to produce an anti-fouling surface structure including a nanostructure, as described in U.S. Patent Publication 2013 / 0236697 (Walker et al.). A microstructured surface also including a nanostructure can be formed by using a multi-tip diamond tool, which can have a single radius, wherein the multiple tool tips have a spacing of less than 1 micron. Such multi-tip diamond tools can also be referred to as "nanostructured diamond tools". Therefore, a microstructured surface (wherein the microstructure also includes a nanostructure) can be formed simultaneously during the manufacture of a diamond tool of a microstructured tool. A focused ion beam milling process can be used to form a tool tip, and can also be used to form a valley of a diamond tool. For example, focused ion beam milling can be used to ensure that the inner surface of the tool tip meets along a common axis to form the bottom of the valley. Focused ion beam milling can be used to form features in valleys, such as concave or convex arcs, ellipses, parabolas, mathematically defined surface patterns, or random or pseudo-random patterns. Valleys of various other shapes can also be formed. Exemplary diamond turning machines and methods for producing discontinuous or inconsistent surface structures can include and utilize a fast tool servo (FTS) as described in, for example, PCT Publication WO 00 / 48037, published on August 17, 2000; U.S. Patent Nos. 7,350,442 (Ehnes) and 7,328,638 (Gardiner); and U.S. Patent Publication No. 2009 / 0147361 (Gardiner).
[0173] In some embodiments, multiple nanostructures can be formed by shaping an extruded material or an antifouling layer with a microreplication tool that also has a nanostructured granular electroplated layer for embossing. Electrodeposition, or more specifically electrochemical deposition, can also be used to generate various surface structures (including nanostructures) to form a microreplication tool. The tool can be made using a two-part electroplating process, wherein a first electroplating procedure can form a first metal layer having a first major surface, and a second electroplating procedure can form a second metal layer on the first metal layer. The second metal layer may have a second major surface having an average roughness less than the average roughness of the first major surface. The second major surface can be used as a structured surface of the tool. A replica of the surface can then be prepared in the major surface of the optical film to provide light diffusion properties. An example of an electrochemical deposition technique is described in PCT Publication WO 2018 / 130926 (Derks et al.).
[0174] Figure 6A cross-section 600 of an antifouling layer 608 is shown having an antifouling surface 602. The antifouling surface 602 can be similar to the antifouling surface 402, for example, the microstructures 418, 618 of the antifouling layers 408, 608 can have the same or similar dimensions and can also form a skipped, serrated pattern of alternating micropeaks 620 and microspaces 622. The antifouling surface 602 differs from the surface 402 in that, for example, the nanostructures 720 can include nano-sized masking elements 722.
[0175] The nanostructure 720 can be formed using a masking element 722. For example, the masking element 722 can be used in a subtractive manufacturing process, such as reactive ion etching (RIE), to form the nanostructure 720 having the surface 602 of the microstructure 618. Methods of making nanostructures and nanostructured articles can involve depositing a layer, such as the anti-fouling layer 408, onto a major surface of a substrate by plasma chemical vapor deposition from a gaseous mixture while substantially simultaneously etching the surface with a reactive species. The method can include providing a substrate; mixing a first gaseous species capable of depositing a layer onto the substrate when a plasma is formed and a second gaseous species capable of etching the substrate when a plasma is formed, thereby forming a gaseous mixture. The method can include forming the gas mixture into a plasma, and exposing a surface of the substrate to the plasma, wherein the surface can be etched and a layer can be substantially simultaneously deposited on at least a portion of the etched surface, thereby forming the nanostructure.
[0176] The substrate may be a (co)polymer material, an inorganic material, an alloy, a solid solution or a combination thereof. The deposited layer may include a reaction product of a plasma chemical vapor deposition using a reactive gas comprising a compound selected from the group consisting of an organosilicon compound, a metal alkyl compound, a metal isopropoxy compound, an acetylacetonato metal compound, a metal halide and a combination thereof. Nanostructures with high aspect ratios may be prepared, and optionally have random sizes in at least one dimension, or even in three orthogonal dimensions.
[0177] In some embodiments of the method of the anti-fouling layer 608, an anti-fouling layer can be provided having a series of microstructures 618 disposed on the anti-fouling surface 602 of the layer. The series of microstructures 618 can include a series of alternating micropeaks 620 and microspaces 622.
[0178] A series of nanometer-sized masking elements 722 may be disposed on at least the micrometer space 622. The anti-fouling surface 602 of the anti-fouling layer 608 may be exposed to reactive ion etching to form a plurality of nanostructures 718 on the surface of the layer including the series of nanopeaks 720. Each nanopeak 720 may include a masking element 722 and a pillar 760 of layer material between the masking element 722 and the layer 608.
[0179] The masking element 722 can be formed of any suitable material that is more resistant to RIE effects than the material of the anti-fouling layer 608. In some embodiments, the masking element 722 includes an inorganic material. Non-limiting examples of inorganic materials include silica and silicon dioxide. In some embodiments, the masking element 722 is hydrophilic. Non-limiting examples of hydrophilic materials include silica and silicon dioxide.
[0180] As used herein, the term "maximum diameter" refers to the longest dimension based on a straight line passing through an element having any shape.
[0181] The masking elements 722 can be nanometer-sized. Each masking element 722 can define a maximum diameter 742. In some embodiments, the maximum diameter of the masking elements 722 can be at most 1000 nanometers (in some embodiments, at most 750 nanometers, 500 nanometers, 400 nanometers, 300 nanometers, 250 nanometers, 200 nanometers, 150 nanometers, or even at most 100 nanometers).
[0182] The maximum diameter 742 of each masking element 722 can be described relative to the micro-peak height 640 of the corresponding micro-peak 620. In some embodiments, the corresponding micro-peak height 640 is at least 10 times (in some embodiments, at least 25 times, 50 times, 100 times, 200 times, 250 times, 300 times, 400 times, 500 times, 750 times, or even at least 1000 times) the maximum diameter 742 of the masking element 722.
[0183] Each nanopeak 720 can define a height 722. The height 722 can be defined between the base line 750 and the apex 748 of the masking element 722.
[0184] Fig. 7A and Figure 7B Lines 800 and 820 are shown representing cross-sectional profiles of different forms of peaks 802, 822 for any antifouling surface, such as surfaces 402, 602, which may be micro-peaks for micro-structures or nano-peaks for nano-structures. As mentioned, the structures need not be strictly triangular in shape.
[0185] Line 800 shows that a first portion 804 (top portion) of peak 802 including apex 812 may have a generally triangular shape, while adjacent side 806 may be curved. In some embodiments, as shown, side 806 of peak 802 may not have a sharper turn when transitioning into space 808. Boundary 810 between side 806 of peak 802 and space 808 may be defined by a threshold slope of line 800, as described herein, for example, with respect to FIG. 4A to FIG. 4C and Figure 5 discussed.
[0186] The space 808 may also be defined in terms of a height relative to the height 814 of the peak 802. The height 814 of the peak 802 may be defined between one of the boundaries 810 and the vertex 812. The height of the space 808 may be defined between the bottom 816 or the lowest point of the space 808 and one of the boundaries 810. In some embodiments, the height of the space 808 may be at most 40% (in some embodiments, at most 30%, 25%, 20%, 15%, 10%, 5%, 4%, 3%, or even at most 2%) of the height 814 of the peak 802. In some embodiments, the height of the space 808 is at most 10% (in some embodiments, at most 5%, 4%, 3%, or even at most 2%) of the height 814 of the peak 802.
[0187] Line 820 shows that a first portion 824 (top portion) of peak 820 including the apex can have a generally rounded shape without sharp turns between adjacent sides 826. Apex 832 can be defined as the highest point of structure 820, for example, where the slope changes from positive to negative. Although first portion 824 (top portion) can be rounded at apex 832, peak 820 can still define an angle between the first average slope and the second average slope, such as angle A (see Figure 5 ).
[0188] The boundary 830 between the side 826 of the peak 820 and the space 828 can be defined, for example, by a sharper turn. The boundary 830 can also be defined by a slope or relative height, as described herein.
[0189] like Figures 8 to 11 As shown, the antifouling surface can be discontinuous, intermittent or inconsistent. For example, the antifouling surface can also be described as comprising micro-pyramids with micron spaces surrounding the micro-pyramids (see Figure 8 and Fig.11 ).
[0190] Figure 8 A first antifouling surface 1001 is shown that is at least partially defined by a non-uniform microstructure 1210. For example, if the antifouling surface 1000 is observed in the yz plane (similar to Figure 4B ), then at least one micron peak 1012 may have a non-uniform height from the left side of the view to the right side, which may be consistent with the micron peak 420 shown to have a uniform height from the left side of the view to the right side. Figure 4B Specifically, at least one of the height or shape of the micro-peaks 1012 defined by the micro-structures 1010 may be non-uniform. The micro-peaks 1012 are separated by micro-spaces (not shown in this perspective view), similar to other surfaces described herein, such as the micro-spaces 422 ( Figure 4A and Figure 4C ).
[0191] Fig. 9 A second antifouling surface 1002 having discontinuous microstructures 1020 is shown. For example, if the antifouling surface 1002 (similar to Figure 4B ), more than one nano-peak 1022 separated by micro-structures 1020 may be shown, which may be different from the micro-peak 420 shown extending continuously from the left side of the view to the right side. Figure 4B In contrast. Specifically, the micro-peaks 1022 of the micro-structure 1020 may be surrounded by micro-spaces 1024. The micro-peaks 1022 may each have a semi-dome-like shape. For example, the semi-dome-like shape may be a hemisphere, a semi-oval, a semi-prolate sphere, or a semi-oblate sphere. The edge 1026 of the base of each micro-peak 1022 extending around each micro-peak may be a rounded shape (e.g., a circle, an ellipse, or a rounded rectangle). The shape of the micro-peaks 1022 may be consistent, as depicted in the illustrated embodiment, or may be inconsistent.
[0192] Fig.10 and Fig.11 The first portion 1004 of the third antifouling surface 1003 having a discontinuous microstructure 1030 ( Fig.10 ) and Section 2 1005( Fig.11 ) are perspective drawings. Both are perspective drawings. Fig.10 The view shows the "front" side of the microstructure 1030 at a more 45 degree angle, while Fig.11 The view shows some of the "back" sides of the microstructures closer to the top corners.
[0193] The micron peak 1032 of the micron structure 1030 surrounded by the micron space 1034 may have a pyramid-like shape (e.g., a micro-pyramid). For example, the pyramid-like shape may be a rectangular pyramid or a triangular pyramid. The side 1036 of the pyramid-like shape may be non-uniform in shape or area (as shown in the illustrated embodiment), or may be uniform in shape or area. The edge 1038 of the pyramid-like shape may be non-linear (as shown in the illustrated embodiment), or may be linear. The total volume of each micron peak 1032 may be non-uniform, as depicted in the illustrated embodiment, or may be uniform.
[0194] The above detailed discussion clearly shows that, if desired, the antifouling surface 31 of the antifouling layer 30 can be textured, such as microstructured and / or nanostructured to enhance its antifouling properties. In general, texturing can be achieved in any suitable manner, whether, for example, by molding or stamping the surface 31 against an appropriate tool surface, or by removing material from an existing surface 31, such as by reactive ion etching, laser ablation, etc. In some methods, the antifouling layer 30 may include inorganic particles of appropriate size and / or shape to provide the desired surface texture. In some embodiments, any such particles may, for example, be deposited onto the surface 31 and adhere to the surface. In other embodiments, any such particles may be incorporated (e.g., blended) into the material that will form the layer 30, wherein the layer 30 is then formed in a manner that allows the presence of particles within the layer 30 so that the surface 31 exhibits a corresponding texture. In some embodiments, the presence of such particles may cause the surface of the layer 30 to exhibit a texture in the layer 30 when it is made. In other embodiments, such particles may allow, for example, the formation of a texture when an organic polymer material is removed from the surface of layer 30 (e.g., by reactive ion etching) while the inorganic particles remain in place, as described earlier herein. In a variation of such methods, inorganic material may be deposited onto the major surface of layer 30, for example, by plasma deposition, simultaneously with the organic material removal (e.g., reactive ion etching) process to achieve a similar effect. Such an arrangement is discussed in U.S. Pat. No. 10,134,566.
[0195] Any such inorganic particles may include, for example, titanium dioxide, silicon dioxide, zirconium oxide, barium sulfate, calcium carbonate or zinc oxide. In some embodiments, the inorganic particles may be in the form of nanoparticles, including: nano titanium dioxide, nano silicon dioxide, nano zirconium oxide or even nanoscale zinc oxide particles. In some embodiments, the inorganic particles may be in the form of beads or microbeads. The inorganic particles may be formed by ceramic materials, glass (e.g., borosilicate glass particles available from Potter Industries) or their various combinations. Suitable glass beads available from Potter Industries for use in the reflective layer filled with inorganic particles include trade name "EMB-20". In some embodiments, the inorganic particles may have an effective D90 particle size of at least 1 μm to at most 40 μm (as defined in NIST "Particle Size Characterization", ASTM E-2578-07 (2012)).
[0196] Potentially suitable inorganic particles include ceramic microspheres available from 3M Company under the trade designations "3M CERAMIC MICROSPHERES WHITE GRADE W-210", "3M CERAMIC MICROSPHERES WHITE GRADE W-410", "3M CERAMIC MICROSPHERES WHITE GRADE W-610", or various combinations thereof. Potentially suitable inorganic particles also include any of the products available from 3M Company under the trade designations "3M GLASS BUBBLES" (K, S or iM series). In general, various combinations of inorganic particles of the same or different sizes can be used.
[0197] In some embodiments, cross-linked polymer microspheres available from Soken Chemical & Engineering Co., under the trade name "Chemisnow" can be added to the anti-fouling layer or the particle-filled reflective layer. Potentially suitable cross-linked polymer microspheres available from Soken Chemical & Engineering Co. include products under the trade names "MX-500" and "MZ-5HN". In some embodiments, semi-crystalline polymer beads available from 3M Company under the trade name "PTFE micro-powder TF 9207Z" can be added to the particle-filled reflective layer or the anti-fouling layer.
[0198] While the primary purpose of any such texturing (e.g., microstructuring and / or nanostructuring) to the exterior surface 31 may be to provide enhanced antifouling, texturing may provide additional benefits. For example, some textures (depending on, for example, the size of the various structures relative to the wavelength of the electromagnetic radiation) may enhance the passive cooling effect achieved by the reflective layer 10 and the cooling film 1 as a whole. Furthermore, in the case where the cooling film 1 is applied to, for example, the exterior surface of a vehicle, texturing may achieve drag reduction. That is, the presence of the microstructures and / or nanostructures may result in a reduced coefficient of friction between the surface 31 and the air through which the vehicle moves, which may save cost and / or fuel.
[0199] In some embodiments, one or more antistatic agents may also be incorporated into the anti-fouling layer to reduce the undesirable attraction of dust, dirt, and debris. An ionic antistatic agent (e.g., available from 3M Company under the trade name 3M IONIC LIQUID ANTI-STAT FC-4400 or 3M IONIC LIQUID ANTI-STAT FC-5000) may be incorporated into, for example, a PVDF fluoropolymer layer to provide static dissipation. Antistatic agents for PMMA and methyl methacrylate copolymer (CoPMMA) optical polymer layers may be purchased from STATRITE from Lubrizol Engineered Polymers, Brecksville, Ohio. Additional antistatic agents for PMMA and CoPMMA optical polymer layers may be purchased from Sanyo Chemical Industries, Ltd., Tokyo, Japan. Chemical Industries, Tokyo, Japan). Optionally, the antistatic properties can have a transparent conductive coating, such as: indium tin oxide (ITO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), metal nanowires, carbon nanotubes or a thin layer of graphene, any of which can be disposed or coated on one of the layers of the antifouling surface structured film described herein. Other suitable polymeric antistatic additives can be purchased from CRODA International.
[0200] Adhesive layer
[0201] As previously mentioned, in some embodiments, the cooling film 1 may include at least one adhesive (e.g., a pressure sensitive adhesive) layer. For example, such an adhesive layer may provide a means of attaching the cooling film 1 to a suitable substrate 50. Alternatively, such an adhesive layer may bond the various layers of the cooling film 1 together. In some embodiments, there may be multiple adhesive layers of various types and for various purposes.
[0202] Such adhesive layers may include any adhesive (e.g., thermosetting adhesives, hot melt adhesives, and / or pressure sensitive adhesives). In some convenient embodiments, such adhesive layers may be pressure sensitive adhesive layers. In some embodiments, the adhesive may be resistant to damage from ultraviolet radiation (either inherently or due to the presence of added UV stabilizers). Exemplary adhesives that are typically resistant to damage from ultraviolet radiation include silicone adhesives and acrylic adhesives containing UV stabilizing / absorbing / blocking additives.
[0203] In some embodiments, any such adhesive layer may include thermally conductive particles to facilitate heat transfer. Exemplary thermally conductive particles include aluminum oxide particles, aluminum oxide nanoparticles, hexagonal boron nitride particles and agglomerates (e.g., available from 3M Company as 3M BORONDINITRIDE), graphene particles, graphene oxide particles, metal particles, and combinations thereof.
[0204] The adhesive layer 40 to be used for bonding the cooling film 1 to the substrate 50 may be provided with a release liner on its inward surface (i.e., the surface to be bonded to the substrate after the release liner is removed). The release liner may include, for example, a polyolefin film, a fluoropolymer film, a coated PET film, or a siliconized film or paper. (Of course, if the cooling film 1 is provided already bonded to the substrate, such a release liner may not be required except for processing in the factory.)
[0205] If the adhesive layer relies on a pressure sensitive adhesive ("PSA"), the PSA may be of any suitable composition. PSAs are well known to those of ordinary skill in the art and have properties including: (1) strong and durable tack, (2) adhesion with no more than finger pressure, (3) the ability to remain on an adherend, and (4) sufficient cohesive strength to be cleanly removed from an adherend. Materials that have been found to function well as PSAs are polymers that are designed and formulated to exhibit the desired viscoelastic properties to achieve a desired balance of tack, peel adhesion, and shear holding power.
[0206] One method that can be used to identify pressure sensitive adhesives is the Dahlquist criterion. As described in the Handbook of Pressure Sensitive Adhesive Technology (Donatas Satas, ed., 2nd ed., p. 172, Van Nostrand Reinhold Publishers, New York, NY, USA, 1989), which is incorporated herein by reference, this standard defines a pressure sensitive adhesive as having a pressure greater than 1×10 -6 centimeter 2 / dyne 1 second creep compliance. Alternatively, since the modulus is roughly the inverse of the creep compliance, a pressure sensitive adhesive can be defined as having a storage modulus less than about 1×10 6 Dyne / cm 2 Adhesive.
[0207] The PSA that can be used to implement the present invention is generally non-flowing and has sufficient barrier properties to provide slow or minimal penetration of oxygen and moisture through the adhesive bond line. In at least some embodiments, the PSA disclosed herein is generally transmissive to visible light and infrared light so that they do not interfere with the passage of visible light. In various embodiments, the average transmittance of the PSA to the visible part of the spectrum measured along the normal axis is at least about 75% (in some embodiments, at least about 80%, 85%, 90%, 92%, 95%, 97% or 98%). In some embodiments, the average transmittance of the PSA to the range of 400nm to 1400nm is at least about 75% (in some embodiments, at least about 80, 85, 90, 92, 95, 97 or 98%). Exemplary PSAs include acrylates, silicones, polyisobutylenes, ureas, and combinations thereof. Some useful commercially available PSAs include UV-curable PSAs, such as those available under the trade designations “ARclear 90453” and “ARclear 90537” from Adhesive Research, Inc., Glen Rock, PA, and acrylic optically clear PSAs, such as those available under the trade designations “OPTICALLY CLEAR LAMINATING ADHESIVE 8171,” “OPTICALLY CLEARLAMINATING ADHESIVE 8172CL,” and “OPTICALLY CLEAR LAMINATING ADHESIVE 8172PCL” from 3M Company, St. Paul, MN.
[0208] In some embodiments, the PSAs useful in practicing the present disclosure have a maximum pressure of 50,000 psi (3.4×10 8 The tensile modulus can be measured, for example, by a tensile testing instrument such as a testing system commercially available from Instron, Norwood, MA, under the trade designation "INSTRON 5900". In some embodiments, the tensile modulus of the PSA is at most 40,000, 30,000, 20,000, or 10,000 psi (2.8×10 8 Pa, 2.1×10 8 pa, 1.4×10 8 pa or 6.9×10 8 Pa).
[0209] In some embodiments, the PSA useful in practicing the present invention is an acrylic PSA. As used herein, the term "acrylic acid" or "acrylate" includes compounds having at least one of an acrylic acid or methacrylic acid group. Useful acrylic PSAs can be made, for example, by combining at least two different monomers (a first and a second monomer). Exemplary suitable first monomers include 2-butyl methacrylate, 2-ethylhexyl acrylate, isooctyl acrylate, lauryl acrylate, n-decyl acrylate, 4-methyl-2-pentyl acrylate, isopentyl acrylate, sec-butyl acrylate, and isononyl acrylate. Exemplary suitable second monomers include (meth)acrylic acids (such as acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid), (meth)acrylamides (such as acrylamide, methacrylamide, N-ethylacrylamide, N-hydroxyethylacrylamide, N-octylacrylamide, N-tert-butylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide and N-ethyl-N-dihydroxyethylacrylamide), (meth)acrylates (such as 2-hydroxyethylacrylate or methacrylate, cyclohexyl acrylate, tert-butyl acrylate or isobornyl acrylate), N-vinyl pyrrolidone, N-vinyl caprolactam, α-olefins, vinyl ethers, allyl ethers, styrene monomers or maleic acid esters.
[0210] Acrylic PSAs can also be prepared by including a crosslinking agent in the formulation. Exemplary crosslinking agents include copolymerizable multifunctional ethylenically unsaturated monomers (e.g., 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and 1,2-ethylene glycol diacrylate); ethylenically unsaturated compounds that are capable of abstracting hydrogens in an excited state (e.g., acrylated benzophenones, such as described in U.S. Pat. No. 4,737,559 (Kellen et al.); p-acryloyloxybenzophenone available from Sartomer, Inc., Exton, Pennsylvania; U.S. Pat. No. 5,073,611 (Reh mer, etc.), including p-N-(methacryloyl-4-oxapentamethylene)-carbamoyloxybenzophenone, N-(benzoyl-p-phenylene)-N'-(methacryloyloxymethylene)-carbodiimide and p-acryloyloxybenzophenone; a nonionic crosslinking agent that is substantially free of ethylenically unsaturated groups and is capable of reacting with, for example, the carboxylic acid groups in the above-mentioned second monomer (such as 1,4-bis(ethyleneiminocarbonylamino)benzene; 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane; 1,8-bis(ethyleneiminocarbonylamino) Octane; 1,4-toluene diisocyanate; 1,6-hexamethylene diisocyanate, N,N'-bis-1,2-propylene isophthalamide, diepoxide, dianhydride, bis(amide) and bis(imide)); and a nonionic crosslinking agent that is substantially free of ethylenically unsaturated groups, cannot copolymerize with the first monomer and the second monomer, and can abstract hydrogen in an excited state (such as 2,4-bis(trichloromethyl)-6-(4-methoxy)phenyl)-s-triazine; 2,4-bis(trichloromethyl)-6-(3,4-dimethoxy)phenyl)-s-triazine; 2,4-bis(trichloromethyl)-6-(3,4-dimethoxy)phenyl)-s-triazine; 2,4-bis(trichloromethyl)- 4-bis(trichloromethyl)-6-(3-methoxy)phenyl)-s-triazine as described in U.S. Pat. No. 4,330,590 (Vesley); 2,4-bis(trichloromethyl)-6-naphthyl-s-triazine and 2,4-bis(trichloromethyl)-6-(4-methoxy)naphthyl-s-triazine as described in U.S. Pat. No. 4,329,384 (Vesley).
[0211] Typically, the first monomer is used in an amount of 80-100 parts by weight (pbw) based on 100 parts of the total weight of the copolymer, and the second monomer is used in an amount of 0-20 pbw based on 100 parts of the total weight of the copolymer. The crosslinking agent can be used in an amount of 0.005 wt % to 2 wt %, such as about 0.01 wt % to about 0.5 wt % or about 0.05 wt % to 0.15 wt %, based on the combined weight of the monomers. Acrylic PSAs are described in detail, for example, in U.S. Pat. No. 9,614,113, which is incorporated herein by reference in its entirety.
[0212] Acrylic PSAs useful in practicing the present invention can be prepared, for example, by a solvent-free batch free radical polymerization process (e.g., using heat, electron beam radiation, or ultraviolet radiation). Such polymerization is typically promoted by a polymerization initiator (e.g., a photoinitiator or a thermal initiator). Exemplary suitable photoinitiators include benzoin ethers such as benzoin methyl ether and benzoin isopropyl ether, substituted benzoin ethers such as anisole methyl ether, substituted acetophenones such as 2,2-dimethoxy-2-phenylacetophenone, and substituted α-ketones such as 2-methyl-2-hydroxypropiophenone. Examples of commercially available photoinitiators include IRGACURE 651 and DAROCUR 1173, both available from Ciba-Geigy Corp., Hawthorne, NY; and LUCERIN TPO, available from BASF, Parsippany, NJ. Examples of suitable thermal initiators include, but are not limited to, peroxides such as dibenzoic acid peroxide, dilauric acid peroxide, methyl ethyl ketone peroxide, cumene hydroperoxide, dicyclohexyl peroxydicarbonate, and 2,2-azo-bis(isobutyronitrile) and tert-butyl perbenzoate. Examples of commercially available thermal initiators include VAZO64 available from ACROS Organics, Pittsburgh, PA, and LUCIDOL 70 available from Elf Atochem North America, Philadelphia, PA. The polymerization initiator is used in an amount effective to promote polymerization of the monomers (e.g., 0.1 to about 5.0 parts by weight or 0.2 to about 1.0 parts by weight based on 100 parts of the total monomer content).
[0213] If a photocrosslinker is used, the applied adhesive may be exposed to ultraviolet radiation having a wavelength of about 250 nm to about 400 nm. The radiation energy within this wavelength range required to crosslink the adhesive is about 100 mJ / cm 2 to about 1,500 mJ / cm 2 , or more specifically, about 200 mJ / cm2 to about 800 mJ / cm 2 .
[0214] Useful solventless polymerization methods are disclosed in U.S. Pat. No. 4,379,201 (Heilmann et al.). Initially, a mixture of the first and second monomers may be polymerized with a portion of the photoinitiator by exposing the mixture to UV radiation in an inert environment for a time sufficient to form a coatable base slurry, and then adding the crosslinker and the remainder of the photoinitiator. This final slurry (e.g., having a Brookfield viscosity of about 100 centipoise to about 6000 centipoise at 23°C, as measured with a No. 4 LTV rotor at 60 rpm) including the crosslinker may then be coated onto a weatherable sheet. After the slurry is coated onto the weatherable sheet, polymerization and crosslinking may be further performed in an inert environment (e.g., nitrogen, carbon dioxide, helium, and argon, excluding oxygen). A sufficiently inert atmosphere may be achieved by covering a layer of the photosensitive slurry with a polymer film (such as a silicone-treated PET film that is transparent to UV radiation or electron beams) and irradiating through the film in air.
[0215] In some embodiments, the PSA useful in practicing the present invention comprises polyisobutylene. The polyisobutylene may have a polyisobutylene backbone in the main chain or in the side chain. Useful polyisobutylene may be prepared by polymerizing isobutylene alone or in combination with n-butene, isoprene or butadiene, for example, in the presence of a Lewis acid catalyst (e.g., aluminum chloride or boron trifluoride).
[0216] Useful polyisobutylene materials are available from several manufacturers. Homopolymers are commercially available, for example, from BASF Corporation (Floham Park, New Jersey) under the trade names "OPPANOL" and "GLISSOPAL" (e.g., OPPANOL B15, B30, B50, B100, B150, and B200, and GLISSOPAL 1000, 1300, and 2300); from United Chemical Products (UCP) in St. Petersburg, Russia, under the trade names "SDG", "JHY", and "EFROLEN". Polyisobutylene copolymers can be prepared by polymerizing isobutylene in the presence of a small amount (e.g., up to 30, 25, 20, 15, 10, or 5 weight percent) of another monomer (e.g., for example, styrene, isoprene, butylene, or butadiene). Exemplary suitable isobutylene / isoprene copolymers are available from Mobil Corp. in Irving, TX., under the trade designation "EXXON BUTYL" (e.g., EXXON BUTYL 065, 068, and 268); from UCP as "BK-1675N" and from Sarnia, Ontario, Canada as "LANXESS" (e.g., LANXESS BUTYL 301, LANXESS BUTYL 101-3, and LANXESS BUTYL 402). Exemplary suitable isobutylene / styrene block copolymers are commercially available from Kaneka (Osaka, Japan) under the trade designation "SIBSTAR". Other exemplary suitable polyisobutylene resins are available, for example, under the trade designation "VISTANEX" from Exxon Chemical Co., under the trade designation "HYCAR" from Goodrich Corp., Charlotte, NC, and under the trade designation "JSR BUTYL" from Japan Butyl Co., Ltd., Kanto, Japan. The polyisobutylenes useful in practicing the present invention can have a wide range of molecular weights and a wide range of viscosities. Polyisobutylenes of many different molecular weights and viscosities are commercially available.
[0217] In some embodiments of the PSAs comprising polyisobutylene, the PSA further comprises a hydrogenated hydrocarbon tackifier (in some embodiments, a poly(cycloolefin)). In some of these embodiments, about 5-90 weight percent of the hydrogenated hydrocarbon tackifier (in some embodiments, a poly(cycloolefin)) is blended with about 10-95 weight percent of the polyisobutylene, based on the total weight of the PSA composition. Useful polyisobutylene PSAs include adhesive compositions comprising hydrogenated poly(cycloolefins) and polyisobutylene resins, such as those disclosed in International Patent Application Publication No. WO 2007 / 087281 (Fujita et al.).
[0218] "Hydrogenated" hydrocarbon tackifier component can include partially hydrogenated resin (e.g., with any hydrogenation ratio), fully hydrogenated resin, or a combination thereof. In some embodiments, the hydrogenated hydrocarbon tackifier is fully hydrogenated, which can reduce the moisture permeability of PSA and improve compatibility with polyisobutylene resin. The hydrogenated hydrocarbon tackifier is typically a hydrogenated cycloaliphatic resin, a hydrogenated aromatic resin, or a combination thereof. For example, some tackifier resins are hydrogenated C9 type petroleum resins obtained by copolymerizing the C9 fraction prepared by thermal decomposition naphtha, hydrogenated C5 type petroleum resins obtained by copolymerizing the C5 fraction prepared by thermal decomposition naphtha, or hydrogenated C5 / C9 type petroleum resins obtained by polymerizing the combination of the C5 fraction prepared by thermal decomposition naphtha and the C9 fraction. The C9 fraction can include, for example, indene, vinyl toluene, alpha-methyl styrene, beta-methyl styrene, or a combination thereof. The C5 fraction can include, for example, pentane, isoprene, piperine, 1,3-pentadiene, or a combination thereof. In some embodiments, the hydrogenated hydrocarbon tackifier is a hydrogenated poly(cycloolefin) polymer. In some embodiments, the hydrogenated poly(cycloolefin) is a hydrogenated poly(dicyclopentadiene), which can provide advantages to the PSA (e.g., low moisture permeability and transparency). The tackifying resin is typically amorphous and has a weight average molecular weight of no greater than 5000 g / mole.
[0219] Some suitable hydrogenated hydrocarbon tackifiers are available under the trade designations "ARKON" (e.g., ARKON P or ARKON M) from Arakawa Chemical Industries Co., Ltd. (Osaka, Japan); "ESCOREZ" from Exxon Chemical; "REGALREZ" (e.g., REGALREZ 1085, 1094, 1126, 1139, 3102, and 6108) from Eastman (Kingsport, TN); "WINGTACK" (e.g., WINGTACK 95 and RWT-7850) resins from Cray Valley (Exton, Pennsylvania); "PICCOTAC" (e.g., PICCOTAC as “PENCEL A”, “ESTERGUM H”, “SUPER ESTERA” and “PINECRYSTAL” from Arakawa Chemical Industries Co., Ltd., Osaka, Japan; as “EASTOTAC H” from Eastman; and as “IMARV” from Idemitsu Petrochemical Co., Tokyo, Japan.
[0220] In some embodiments, the adhesive layer can be a so-called hot melt adhesive, such as extruded at high temperature, and exhibits PSA properties after cooling and hardening. Extrudable hot melt adhesives can be formed as pressure-sensitive adhesives, for example, by extruding and blending with tackifiers. Exemplary pressure-sensitive adhesives can be purchased from 3M Company, St. Paul, MN, for example, under the trade names "OCA8171" and "OCA8172". Extrudable pressure-sensitive adhesives can be purchased from Kuraray, Osaka, Japan, for example, under the trade names "LIR-290", "LA2330", "LA2250", "LA2140E" and "LA1114"; and Exxon Mobil Corporation, Irving, Texas, under the trade name "ESCORE". o bil, Irving, TX).
[0221] Exemplary extrudable adhesives also include isobutylene / isoprene copolymers, such as those available under the trade designations "EXXON BUTYL 065," "EXXON BUTYL 068," and "EXXON BUTYL 268" from Exxon Mobil Corp.; under the trade designation "BK-1675N" from United Chemical Products of Velizy-Villacoublay, France; under the trade designations "LANXESS BUTYL 301," "LANXESS BUTYL 101-3," and "LANXESS BUTYL 402" from LANXESS, Sarnia, Ontario, Canada; and under the trade designation "SIBSTAR" (both diblock and triblock) from Kaneka, Osaka, Japan. Exemplary polyisobutylene resins are available, for example, from Exxon Chemical Co., Irving, TX, under the trade name "VISTANEX"; from Goodrich Corp., Charlotte, NC, under the trade name "HYCAR"; and from Japan Butyl Co., Ltd., Kanto, Japan, under the trade name "JSR BUTYL". Various compositions and uses thereof are described in U.S. Patent Application Publication No. 2019-0111666.
[0222] Such PSA layers can be provided by techniques known in the art, such as hot melt extrusion of an extrudable composition comprising components of a PSA composition. Advantageously, the PSA layer can be prepared by this method in the absence of a solvent. Exemplary methods for preparing extrudable adhesives are described, for example, in PCT Publication No. WO1995 / 016754A1 (Leonard et al.), the disclosure of which is incorporated herein by reference in its entirety.
[0223] In some embodiments, at least one PSA layer present in the cooling film 1 may include a UV blocker. As previously mentioned, such terms broadly encompass materials commonly referred to as UV absorbers (UVA), light stabilizers (e.g., hindered amine light stabilizers), antioxidants, etc. It should be understood that there may not necessarily be a clear standard dividing line between these various types of UV blockers. For example, some materials may work through more than one of these mechanisms.
[0224] Examples of useful UVAs include those available under the trade names "TINUVIN 328", "TINUVIN 326", "TINUVIN 783", "TINUVIN 770", "TINUVIN 479", "TINUVIN 928", "TINUVIN 1600" and "TINUVIN 1577" from Ciba Specialty Chemicals Corporation. When used, some such UVAs may be present, for example, in an amount of about 0.01% to 3% by weight of the total weight of the pressure-sensitive adhesive composition. Examples of useful antioxidant-type UV blockers include hindered phenol-based compounds and phosphate-based compounds (e.g., those available under the trade names "IRGANOX 1010", "IRGANOX 1076" and "IRGAFOS 126" and butylated hydroxytoluene (BHT) from Ciba Specialty Chemicals Corporation). When used, antioxidants can be present in an amount of, for example, about 0.01% to 2% by weight of the total weight of the pressure-sensitive adhesive composition. Examples of available stabilizer-type UV blockers include phenolic stabilizers, hindered amine-based stabilizers (e.g., those available under the trade name "CHIMASSORB", such as "CHIMASSORB2020" purchased from BASF (BASF)), imidazole-based stabilizers, dithiocarbamate-based stabilizers, phosphorus-based stabilizers, and thioester-based stabilizers. When used, such compounds can be present in an amount of about 0.01 to 3% by weight of the total weight of the pressure-sensitive adhesive composition.
[0225] It should be understood that in some embodiments, the PSA layer may not contain a UV blocker or may only need to include an amount of UV blocker sufficient to protect the PSA layer itself. Figure 1 As shown, the PSA layer 40 used to bond the cooling film 1 to the substrate 50 may not require any UV blocking agent. (However, since the side edges of the PSA layer 40 may be exposed to sunlight in some cases, such a PSA layer may advantageously include a sufficient amount of UV blocking additives to protect the PSA layer in some embodiments.) If the PSA layer is arranged outward from the reflective layer 10 (such as Figure 3 45), such PSA layer may contain an amount of UV blocking additive commensurate with the desire to protect the reflective layer 10 (rather than just the PSA layer itself). Thus, in such embodiments, the level of UV blocking additive may be increased, for example, above the exemplary range disclosed above to any suitable level.
[0226] UV blocking additives have been mentioned previously herein in the context of incorporating such materials into adhesives (e.g., PSA), hardcoats, independent layers (e.g., fluoropolymer layers used as antifouling layers), or layers of multilayer structures. UV blocking additives will now be discussed further in general. Any such UV blocking additive may be added to any layer (or any component, portion, or phase thereof) of the cooling film 1. As described, in some embodiments, a UV blocking additive may be incorporated into an adhesive used to connect the layers of the cooling film together. In some embodiments, a UV blocking additive may be incorporated into a hardcoat layer used as an antifouling layer of a cooling film (and may be textured, such as microstructured and / or nanostructured). In some embodiments, a UV blocking additive may be incorporated into a fluoropolymer layer used, for example, as an antifouling layer of a cooling film (and may be textured, such as microstructured and / or nanostructured). In some embodiments, a UV blocking additive may be incorporated into a suitable layer of a multilayer structure, which also includes other layers that do not include any UV blocking additives. In various embodiments, a plurality of such layers or components thereof may include a UV blocking additive.
[0227] As described above, UV blockers as disclosed herein encompass those compounds known as UV absorbers (UVAs) and those compounds known as UV stabilizers, particularly hindered amine light stabilizers (HALS) that can, for example, intervene to prevent photooxidative degradation of various polymers (e.g., PET, PMMA, and CoPMMA). Exemplary UVAs for incorporation into, for example, PET, PMMA, or CoPMMA include benzophenones, benzotriazoles, and benzotriazines. Commercially available UVAs for incorporation into, for example, PET, PMMA, or CoPMMA include those purchased from BASF Corporation, Florham Park, New Jersey, as TINUVIN 1577 and TINUVIN 1600. Another exemplary UV absorber is, for example, a polymethyl methacrylate (PMMA) UVA masterbatch available under the trade name "TA11-10 MB03" from Sukano Polymers Corporation, Duncan, SC, Duncan, South Carolina. UVA can be incorporated into these polymers or any other suitable polymer, for example, at a concentration of 1% to 10% by weight. Exemplary HALS compounds for incorporation into PET, PMMA or CoPMMA include those available from BASF Corporation as CHIMMASORB 944 and TINUVIN 123. Another exemplary HALS can be purchased from BASF Corp., for example, under the trade name "TINUVIN 944". HALS compounds can be present in these polymers or any other polymer, for example, at a concentration of 0.1% to 1.0% by weight. Preferably, a 10:1 ratio of UVA to HALS can be used. As described, in some cases, HALS can synergistically enhance the performance of UVA. Exemplary antioxidants include those available from BASF under the trade names "IRGANOX 1010" and "ULTRANOX626".
[0228] UVA and HALS compounds may also be incorporated into the fluoropolymer layer (e.g., whether it is an antifouling layer or a reflective layer). U.S. Pat. Nos. 9,670,300 (Olson et al.) and 10,125,251 (Olson et al.) describe exemplary UVA oligomers that are compatible with PVDF fluoropolymers. Other UV blocking additives may be included in the fluoropolymer layer (or generally in any polymer layer). For example, non-pigment grade particulate zinc oxide and titanium oxide may be used. Nanoscale particles of zinc oxide, calcium carbonate, and barium sulfate may scatter UV light (and reflect to some extent) while being transparent to visible and near infrared light. Small zinc oxide and barium sulfate particles ranging in size from 10 nanometers to 100 nanometers that can scatter or reflect UV radiation are available, for example, from Kobo Products Inc., South Plainfield, New Jersey. Any such material is suitable as long as the resulting UV blocking layer (or layers) meet the criteria previously established herein.
[0229] In some embodiments, the UV absorbing additive may be a red-shifted UV absorber (RUVA), which, for example, absorbs at least 70% (in some embodiments, at least 80% or even at least 90%) of UV light in the wavelength region of 180 nm to 400 nm. The RUVA has increased spectral coverage in the long-wave UV region (i.e., 300 nm to 400 nm), enabling it to block long-wavelength UV light. Exemplary RUVAs include, for example, 5-trifluoromethyl-2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole (available from BASF Corporation of Florham Park, New Jersey under the trade name "CGL-0139"). Corporation, Florham, NJ)), benzotriazoles (e.g., 2-(2-hydroxy-3,5-di-α-cumylphenyl)-2H-benzotriazole, 5-chloro-2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-2H-benzotriazole, 5-chloro-2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3-α-cumyl-5-tert-octylphenyl)-2H-benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole), and 2-(-4,6-diphenyl-1-3,5-triazin-2-yl)-5-hexyloxy-phenol.
[0230] Uses of cooling film
[0231] Composite cooling films according to the present disclosure can be used to cool entities that are thermally connected (e.g., induction, convection, radiation). By reflecting sunlight that would otherwise be absorbed by the entity, reflection in the solar region can be particularly effective in promoting the cooling of the entity when it is subjected to sunlight during the day. By radiating or emitting infrared light in the previously mentioned atmospheric window, absorption in the aforementioned atmospheric window can be particularly effective in promoting nighttime cooling (note that according to Kirchoff's law, articles that show high absorption in a specific wavelength range will also show high emissivity in this wavelength range). Energy can also be radiated or emitted to some extent within a day. In some embodiments, the cooling film will absorb the least solar energy at 0.3 microns to 2.5 microns and absorb the most solar energy at 8 microns to 13 microns.
[0232] See again Figure 1 , the composite cooling film 1 can be fixed to the substrate 50 so that the composite cooling film 1 is in thermal communication with the substrate 50. The shape of the composite cooling film 1 can be generally planar; however, it does not need to be planar, and can be flexible to conform to a non-planar substrate 50. In some embodiments, the substrate 50 can be an item (e.g., a sheet metal plate) fixed to any suitable entity 60 (e.g., a vehicle or a building). In some embodiments, the substrate 50 can be a component of the entity itself (e.g., the substrate 50 can be a roof or panel of a vehicle such as a car or bus). In some embodiments, the composite cooling film will be arranged so that it is at least generally facing the sky.
[0233] In some embodiments, the cooling film may form part of a cooling panel that may be disposed on the exterior of at least a portion of a building or heat transfer system, for example. The cooling panel and / or heat transfer system may cool a fluid, liquid, or gas, which may then be used to remove heat from any desired entity, such as a building, transformer, broadcast antenna, server, server farm, or data center (e.g., to cool a fluid in which a server is immersed), or a vehicle or component thereof (including an electric vehicle battery). In particular embodiments, the cooling panel may remove heat from a heat rejection component (e.g., a condenser) of a cooling / refrigeration / heat pump system.
[0234] In some embodiments, the composite cooling film 1 as disclosed herein may exhibit, for example, relatively broadband absorption (and therefore emission) outside the solar radiation wavelength range of 400nm to 2500nm. The work herein has shown that the use of a cooling film 1 exhibiting broadband emission can advantageously enhance the ability of the cooling film 1 to passively cool an entity that is typically at a temperature higher than (e.g., significantly higher than) the ambient temperature of the surrounding environment in normal operation. Such entities may include, for example, heat removal units (e.g., heat exchangers, condensers, and / or compressors and any associated items) of cooling / refrigeration / heat pump systems. Such heat removal entities may be, for example, external (e.g., outdoor) units of residential cooling or HVAC systems or commercial or large cooling or HVAC systems. Alternatively, such heat removal entities may be external units of commercial refrigeration or freezing systems. In specific embodiments, such entities may be external components of a cooling unit of a large refrigerated shipping container such as a truck trailer, rail car, or intermodal container. (Such large-scale refrigerated shipping containers, etc., are referred to as "refrigerated boxes" in the trade.) In some embodiments, such entities may be high-voltage transformers or high-power broadcast antennas (e.g., such as those used in mass elements / beamforming systems for 5G wireless communications). In any such embodiments, the cooling film 1 may exhibit an average absorptivity of at least 0.7, 0.8, 0.85, or 0.9 over a wavelength range having a lower limit of, for example, 4 microns, 5 microns, 6 microns, or 7 microns, and / or may exhibit such absorptivity over wavelengths extending to an upper limit of, for example, 14 microns, 16 microns, 18 microns, or 20 microns.
[0235] Various uses for which cooling films may be applied are discussed, for example, in U.S. Provisional Patent Application No. 62 / 611,639 and the resulting PCT International Application Publication No. WO 2019 / 130199 and U.S. Patent Application U.S. Provisional Patent Application No. 62 / 855,392, all of which are incorporated herein by reference in their entirety.
[0236] The composite cooling film as disclosed herein may exhibit an average absorptivity of at least 0.85 in the wavelength range of 8 microns to 13 microns (measured according to the procedure outlined in the '392 U.S. Provisional Application cited above). The amount of cooling and the amount of temperature reduction may depend, among other parameters, on the reflective and absorptive properties of the composite cooling film 1. The cooling effect of the composite cooling film 1 may be described with reference to a first temperature of ambient air near or adjacent to the substrate and a second temperature of a portion of the substrate 50 near or adjacent to the composite cooling film 1. In some embodiments, the first temperature is at least 2.7 (in some embodiments, at least 5.5, 8.3, or even at least 11.1) degrees Celsius (e.g., at least 5, 10, 15, or even at least 20 degrees Fahrenheit) higher than the second temperature.
[0237] In various embodiments, the composite cooling film as disclosed herein may exhibit an average electromagnetic radiation reflectivity of at least 85%, 90%, or 95% in the wavelength range of 400 nanometers to 2500 nanometers. As previously described, in some embodiments, this may be an average value obtained by weighting the data in this wavelength range according to the weight of the AM1.5 standard solar spectrum, which provides an indication of the ability of the cooling film to reflect solar radiation.
[0238] It will be apparent to those skilled in the art that the specific exemplary embodiments, elements, structures, features, details, arrangements, configurations, etc. disclosed herein can be modified and / or combined in many ways. It should be emphasized that any embodiment disclosed herein can be used in combination with any other embodiment or any other embodiment disclosed herein, as long as the embodiments are compatible. For example, any arrangement described herein of the various layers of the cooling film can be used in combination with any composition features described herein of any such layer, as long as such features and arrangements produce a compatible combination. Similarly, the method disclosed herein can be used with a cooling film comprising any of the arrangements, composition features, etc. disclosed herein. Although a limited number of exemplary combinations are presented herein, it is emphasized that all such combinations are contemplated and are only prohibited in specific instances of incompatible combinations.
[0239] In summary, it is expected that multiple variations and combinations are within the scope of the conceived invention, not just those representative designs selected as exemplary illustrations. Therefore, the scope of the present invention should not be limited to the specific illustrative structures described herein, but should at least be extended to the structures described by the language of the claims and the equivalents of these structures. Any element cited positively as an alternative in this specification may be explicitly included in the claims or excluded from the claims in any combination as needed. Any element or combination of elements cited in this specification with open language (e.g., including and its derivatives) is considered to be quoted in closed language (e.g., consisting of ... and its derivatives) and in part of closed language (e.g., substantially consisting of ... and its derivatives). Although various theories and possible mechanisms may have been discussed herein, such discussions should not be used to limit the subject matter that can be protected by the claims in any case. If there is any conflict or difference between the disclosure of the present specification described and any document incorporated herein by reference but not claiming priority, then the present specification described shall prevail.
Claims
1. A composite cooling film, comprising: a reflective nonporous inorganic particle-filled organic polymer layer, said reflective nonporous inorganic particle-filled organic polymer layer exhibiting an average reflectivity of electromagnetic radiation of at least 85% in the wavelength range of 400 nanometers to 2500 nanometers, a UV protection layer of an organic polymer material, the UV protection layer being disposed outwardly from the organic polymer layer filled with the reflective nonporous inorganic particles; and an anti-fouling layer of an organic polymer material disposed outwardly from the reflective nonporous inorganic particle-filled organic polymer layer and including an exposed anti-fouling surface facing outwardly; wherein the composite cooling film has an average absorptivity of at least 0.85 in the wavelength range of 8 μm to 13 μm; and The reflective nonporous inorganic particle-filled organic polymer layer has a void volume percentage of less than 10% by volume and contains at least 5 wt% reflective inorganic particles, wherein at least 20% of the reflective inorganic particles exhibit a diameter less than 5.0 microns on a number average basis.
2. The composite cooling film of claim 1, wherein the reflective non-porous inorganic particle-filled organic polymer layer is a pre-made inorganic particle-filled film. 3 . The composite cooling film of claim 1 , wherein the reflective non-porous inorganic particle-filled organic polymer layer is an inorganic particle-filled paint layer.
4. The composite cooling film according to claim 3, wherein the paint layer contains a binder, and the binder is an organic polymer material selected from the group consisting of polymethyl methacrylate, copolymerized methyl methacrylate, polyurethane, polyolefin and fluorine-containing polymer. 5 . The composite cooling film according to claim 1 , wherein the inorganic particles are selected from the group consisting of titanium dioxide, aluminum oxide, calcium carbonate, zinc oxide, barium sulfate, and kaolin.
6. The composite cooling film of claim 1, wherein the UV protection layer of organic polymer material comprises a UV reflection layer.
7. The composite cooling film of claim 6, wherein the UV reflective layer comprises a multilayer optical film.
8. The composite cooling film of claim 1, wherein the UV protection layer of organic polymer material comprises a UV absorbing layer. 9 . The composite cooling film of claim 1 , wherein the composite cooling film further comprises a pressure sensitive adhesive layer disposed inwardly from the reflective nonporous inorganic particle-filled organic polymer layer.
10. The composite cooling film of claim 1, wherein the UV protection layer is bonded to the reflective non-porous inorganic particle-filled organic polymer layer via a pressure sensitive adhesive layer.
11. The composite cooling film of claim 1, wherein the anti-fouling layer is bonded to the UV protection layer by a pressure sensitive adhesive layer.
12. The composite cooling film according to claim 1, wherein the ultraviolet protection layer of the organic polymer material comprises a UV absorbing layer, the UV absorbing layer is a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer carries at least one UV blocking additive and is arranged between the organic polymer layer filled with reflective non-porous inorganic particles and the anti-fouling layer so that the organic polymer layer filled with reflective non-porous inorganic particles and the anti-fouling layer are bonded to each other in an adhesive manner.
13. The composite cooling film of claim 1, wherein the anti-fouling layer of organic polymer material is a fluorinated organic polymer material.
14. The composite cooling film according to claim 1, wherein the UV protection layer of an organic polymer material is an UV absorption layer of an organic polymer material, and the UV absorption layer of an organic polymer material is the same layer as the antifouling layer of an organic polymer material.
15. A composite cooling film according to claim 1, wherein the composite cooling film comprises a multilayer structure arranged outward from the organic polymer layer filled with reflective non-porous inorganic particles; and wherein the outermost layer of the multilayer structure provides the anti-fouling layer of the composite cooling film, and another layer of the multilayer structure provides a UV protection layer of the composite cooling film in the form of a UV absorbing layer, the other layer being arranged inward from the anti-fouling layer.
16. A composite cooling film according to claim 15, wherein the multilayer structure is a coextruded structure, wherein the layer of the multilayer structure providing the anti-fouling layer of the composite cooling film comprises a fluorinated polymer material; and wherein the other layer of the multilayer structure providing the UV absorbing layer of the composite cooling film comprises a non-fluorinated polymer material loaded with at least one UV blocking additive.
17. The composite cooling film of claim 1, wherein the outwardly facing exposed anti-fouling surface of the anti-fouling layer is a textured surface comprising microstructures and / or nanostructures.
18. The composite cooling film of claim 17, wherein the outwardly facing exposed anti-fouling surface of the anti-fouling layer extends along an axis, and a plane containing the axis defines a cross-section of the anti-fouling layer and intersects the surface to define lines describing the surface in two dimensions, the layer comprising: a series of microstructures defined at least in part by the line, the line defining a series of alternating micropeaks and microspaces along the axis, wherein each microspace comprises a maximum absolute slope, the maximum absolute slope defining an angle of at most 30 degrees relative to the axis, wherein each micropeak comprises a first microsegment defining a first average slope and a second microsegment defining a second average slope, and wherein an angle formed between the first average slope and the second average slope is at most 120 degrees; and a plurality of nanostructures defined at least in part by said wire, said wire defining at least a series of nanopeaks disposed along said axis on at least said micrometer space, Each nanopeak has a height, and each corresponding micropeak has a height at least 10 times the height of the nanopeak. 19 . The composite cooling film of claim 18 , wherein the first average slope of the micron peak is positive, and the second average slope of the micron peak is negative.
20. The composite cooling film of claim 18, wherein the width of each micron space is at least one of: at least 10% of the corresponding micron peak distance, or at least 10 microns.
21. The composite cooling film of claim 18, wherein a micro-peak distance between micro-peaks is in the range of 1 micron to 1000 microns.
22. The composite cooling film of claim 18, wherein the height of the micro-peaks is at least 10 microns.
23. The composite cooling film of claim 18, wherein the plurality of nanostructures are also disposed on the micro-peaks.
24. The composite cooling film of claim 17, wherein at least some of the microstructures and / or nanostructures are provided by inorganic particles present on the outwardly facing exposed antifouling surface.
25. A composite cooling film, comprising: a reflective nonporous inorganic particle-filled organic polymer layer, said reflective nonporous inorganic particle-filled organic polymer layer exhibiting an average reflectivity of electromagnetic radiation of at least 85% in the wavelength range of 400 nanometers to 2500 nanometers, a UV protection layer of an organic polymer material, the UV protection layer being disposed outwardly from the organic polymer layer filled with the reflective nonporous inorganic particles; and an antifouling layer of an organic polymeric material, the antifouling layer disposed outwardly from the UV protection layer and including an exposed antifouling surface facing outwardly; wherein the composite cooling film has an average absorptivity of at least 0.85 in a wavelength range of 4 μm to 20 μm; and The reflective nonporous inorganic particle-filled organic polymer layer has a void volume percentage of less than 10% by volume and contains at least 5 wt% reflective inorganic particles, wherein at least 20% of the reflective inorganic particles exhibit a diameter less than 5.0 microns on a number average basis.
26. An assembly comprising the composite cooling film of claim 1 secured to an outer surface of a substrate such that the anti-fouling surface of the anti-fouling layer is outwardly facing and exposed, and such that the composite cooling film and the substrate are in thermal communication with each other.
27. The assembly of claim 26, wherein the composite cooling film is secured to the outer surface of the substrate via a pressure sensitive adhesive loaded with a UV blocking additive.
28. The assembly of claim 26, wherein the substrate is a component of a cooling panel and / or heat transfer system configured to cool a fluid, liquid or gas, which can then remove heat from any desired entity.
29. A method for passively cooling a substrate, the method comprising fixing the composite cooling film according to claim 1 to the outer surface of the substrate so that the anti-fouling surface of the anti-fouling layer is facing outward and exposed, so that the composite cooling film and the substrate are thermally connected to each other, and so that the substrate on which the composite cooling film is fixed is arranged so that it at least generally faces the sky.
Citation Information
Patent Citations
Polymethylmethacrylate based hardcoat composition and coated article
US10072173B2
Fluoropolymer composition including at least one oligomer
US10125251B2
Method of making a nanostructure and nanostructured articles
US10134566B2
Coating to cool a surface by passive radiative cooling
US10323151B2
Microreplicated films having diffractive features on macro-scale features
US20090147361A1