Catalyst layer, membrane electrode assembly for solid polymer fuel cell, and solid polymer fuel cell

By loading platinum catalyst on a carbon support and optimizing the distribution of ionomers, a pseudo-three-phase interface is formed, which solves the problems of high catalyst usage and low fuel cell output efficiency, and reduces the catalyst usage and high fuel cell output. .

CN114902453BActive Publication Date: 2024-11-29AGC INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080089855.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-29
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

The prior art is difficult to uniformly cover platinum catalyst particles in the catalyst layer, resulting in a high catalyst usage and low output efficiency of the fuel cell, making it difficult to take into account both the reduction of the catalyst usage and the high output of the fuel cell.

Method used

By loading a platinum catalyst on a carbon support, the pore distribution is prepared by nitrogen adsorption method to ensure the occupancy and distribution of ionomers in specific mesopories, forming a pseudo-three-phase interface to improve catalyst activity, reduce catalyst usage and increase fuel cell output.

Benefits of technology

The reduction of catalyst usage and the higher output of fuel cells are achieved. By optimizing the structure of the catalyst layer, the platinum catalyst is effectively utilized, and the performance and efficiency of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114902453B_ABST
    Figure CN114902453B_ABST
Patent Text Reader

Abstract

A catalyst layer comprising: catalyst-supported carbon having a catalyst containing platinum supported on a carbon carrier, and an ionomer, wherein the catalyst-supported carbon has mesopores having a pore diameter of not less than 2 nm and not more than 10 nm in a pore distribution obtained by a nitrogen adsorption method, at least a portion of the ionomer is present in the mesopores having a pore diameter of not less than 2 nm and not more than 10 nm, the content of the ionomer is not less than 100 parts by mass relative to 100 parts by mass of the carbon carrier, and the occupancy rate of the ionomer in the total volume of the mesopores having a pore diameter of not less than 2 nm and not more than 10 nm is not more than 50% by volume.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a catalyst layer, a membrane electrode assembly for a polymer electrolyte fuel cell, and a polymer electrolyte fuel cell. Background Art

[0002] A polymer electrolyte fuel cell is formed by, for example, sandwiching a membrane electrode assembly between two separators to form a cell, and stacking a plurality of cells.

[0003] The membrane electrode assembly includes, for example, an anode including a catalyst layer and a gas diffusion layer, a cathode including a catalyst layer and a gas diffusion layer, and a polymer electrolyte membrane disposed between the anode and the cathode.

[0004] The catalyst layer used in the anode and the cathode is composed of, for example, a catalyst-supported body in which a catalyst is supported on a carrier, and an ionomer as a polymer electrolyte.

[0005] Platinum, which is mainly used as a catalyst, is expensive, so it is desirable to reduce the amount of catalyst used. Therefore, in order to effectively utilize the catalyst, attempts have been made to reduce the amount of catalyst used and increase the output of the fuel cell by covering as many catalyst particles as possible with ionomers (e.g., Patent Documents 1 to 3, etc.).

[0006] Patent Document 1: Japanese Patent Application Publication No. 2010-167379

[0007] Patent Document 2: Japanese Patent Application Publication No. 2010-186678

[0008] Patent Document 3: Japanese Patent Application Publication No. 2011-081977 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] As described above, conventionally, in order to achieve both reduction in catalyst usage and increase in fuel cell output, it has been considered necessary to cover as many catalyst particles as evenly as possible with ionomers in order to widely form a three-phase interface of catalyst, ionomer, and water as a reaction site in the catalyst layer.

[0011] However, when a catalyst containing platinum is used as a catalyst, there is a demand for reducing the amount of catalyst used and for further increasing the output of the fuel cell.

[0012] The present disclosure is made in view of the above-mentioned situation, and its purpose is to provide a catalyst layer that reduces the amount of catalyst used and realizes high output of the fuel cell by using it in a solid polymer fuel cell, a membrane electrode assembly for a solid polymer fuel cell using the above-mentioned catalyst layer, and a solid polymer fuel cell having the above-mentioned membrane electrode assembly for a solid polymer fuel cell.

[0013] Solutions for solving problems

[0014] The specific means for achieving the above-mentioned objects are as follows.

[0015] <1> A catalyst layer comprising: catalyst-supported carbon in which a catalyst containing platinum is supported on a carbon carrier, and an ionomer,

[0016] The catalyst-supported carbon has mesopores having a pore diameter of 2 nm or more and less than 10 nm in a pore distribution obtained by a nitrogen adsorption method,

[0017] At least a portion of the ionomer is present in the mesopores having a pore diameter of 2 nm or more and less than 10 nm.

[0018] The content of the ionomer is 100 parts by mass or more relative to 100 parts by mass of the carbon support.

[0019] The ionomer accounts for 50% by volume or less of the total volume of the mesopores having a pore diameter of 2 nm or more and less than 10 nm.

[0020] <2> according to <1> The catalyst layer, wherein the catalyst-supported carbon in the catalyst layer has a thickness of 0.03 cm 3 / g catalyst or more, and contains macropores with a pore diameter of 50 nm or more in the pore distribution obtained by a nitrogen adsorption method.

[0021] <3> according to <1> or <2> The catalyst layer, wherein the content of the catalyst per unit area of ​​the catalyst layer is 0.2 mg / cm 2 the following.

[0022] <4> according to <1> ~ <3> The catalyst layer described in any one of the above aspects, wherein the catalyst includes at least one selected from the group consisting of platinum particles and platinum alloy particles.

[0023] <5> according to <4> The catalyst layer, wherein the number average particle size of the catalyst is 1nm to 20nm.

[0024] <6> according to <1> ~ <5> The catalyst layer according to any one of the preceding claims, wherein the content of the catalyst relative to the entire catalyst-supported carbon is 10% by mass to 70% by mass.

[0025] <7> A membrane electrode assembly for a solid polymer fuel cell, comprising:

[0026] an anode having a first gas diffusion layer and a first catalyst layer provided on one side of the first gas diffusion layer;

[0027] a cathode having a second gas diffusion layer and a second catalyst layer provided on one side of the second gas diffusion layer; and

[0028] a polymer electrolyte membrane disposed between the first catalyst layer and the second catalyst layer;

[0029] At least one of the first catalyst layer and the second catalyst layer is <1> ~ <6> The catalyst layer as described above.

[0030] <8> A solid polymer fuel cell having <7> The membrane electrode assembly for solid polymer fuel cell.

[0031] Effects of the Invention

[0032] According to the present disclosure, by using it in solid polymer fuel cells, it is possible to provide a catalyst layer that reduces the amount of catalyst used and achieves high output of the fuel cell, a membrane electrode assembly for a solid polymer fuel cell using the above-mentioned catalyst layer, and a solid polymer fuel cell having the above-mentioned membrane electrode assembly for a solid polymer fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic cross-sectional view showing an example of a membrane electrode assembly for a polymer electrolyte fuel cell. DETAILED DESCRIPTION

[0034] Hereinafter, the scheme for implementing the present disclosure is described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, for its constituent elements (including element steps, etc.), except for the cases specifically indicated, it is not necessary. The same is true about numerical values ​​and their ranges, which do not limit the present disclosure.

[0035] The term "step" in this specification includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.

[0036] In the present specification, a numerical range expressed using "to" includes the numerical values ​​described before and after "to" as a minimum value and a maximum value, respectively.

[0037] In the present specification, each component may include a plurality of corresponding substances. When a plurality of substances corresponding to each component are present in the composition, the content rate or content of each component refers to the total content rate or content of the plurality of substances present in the composition unless otherwise specified.

[0038] When the embodiments are described in this specification with reference to the drawings, the configuration of the embodiments is not limited to the configuration shown in the drawings. In addition, the sizes of the components in each figure are conceptual, and the relative relationship between the sizes of the components is not limited to this.

[0039] [Catalyst layer]

[0040] The catalyst layer of the present embodiment is a catalyst layer containing catalyst-supported carbon in which a catalyst containing platinum is supported on a carbon carrier, and an ionomer.

[0041] Mesopores generally refer to pores with a pore diameter of 2 nm or more and less than 50 nm. In the present embodiment, ionomers occupying a specific volume ratio exist in the mesopores with a pore diameter of 2 nm or more and less than 10 nm. That is, the catalyst-supported carbon has mesopores with a pore diameter of 2 nm or more and less than 10 nm in the pore distribution obtained by the nitrogen adsorption method, at least a part of the ionomers exist in the mesopores with a pore diameter of 2 nm or more and less than 10 nm, the content of the ionomer is 100 parts by mass or more relative to 100 parts by mass of the carbon carrier, and the ionomer occupies a proportion of 50% by volume or less in the total volume of the mesopores with a pore diameter of 2 nm or more and less than 10 nm.

[0042] Hereinafter, the pore distribution obtained by the nitrogen adsorption method is also referred to as "pore distribution", pores of 2 nm or more and less than 50 nm are also referred to as "mesopores", mesopores with a pore diameter of 2 nm or more and less than 10 nm in the pore distribution are also referred to as "specific mesopores", and the occupancy rate of ionomers in the total volume of specific mesopores is also referred to as "ionomer occupancy rate". In addition, the "macropores" described below refer to pores with a pore diameter of 50 nm or more and less than 300 nm.

[0043] The above-mentioned "pore distribution" is obtained by analyzing the sample of the measurement object based on the BJH method using an automatic specific surface area / pore distribution measuring device (for example, manufactured by Shimadzu Corporation, model: Tristar II3020, measuring method: nitrogen adsorption method based on constant volume method). It should be noted that the specific surface area and pore volume of the catalyst-supported carbon described later are calculated based on the above-mentioned pore distribution.

[0044] In addition, the above-mentioned "ionomer occupancy rate" is a value represented by the following formula (1) when the total volume of specific mesopores obtained by the above-mentioned measurement and analysis of the sample of the catalyst-supported carbon to which the ionomer is attached is set as P1, and the total volume of specific mesopores obtained by the above-mentioned measurement and analysis of the sample of the catalyst-supported carbon to which the ionomer is not attached is set as P0. It should be noted that the above-mentioned total volume of specific mesopores refers to the total pore area of ​​specific mesopores.

[0045] Ionomer occupancy (volume %) = (P0-P1) × 100 / P0····(1)

[0046] It should be noted that as the sample of the above-mentioned catalyst-loaded carbon with an ionomer attached, for example, the following material is used: a coating liquid for forming a catalyst layer is applied on a substrate film such as a PET film, and the coating layer is dried at 80°C to remove the solvent, thereby forming a coating layer, and the obtained coating layer is scraped off and made into a powder.

[0047] In addition, as the sample of the catalyst-supported carbon to which the ionomer is not attached, for example, the following is used: a mixture of the catalyst-supported carbon and a solvent is applied to a substrate film such as a PET film, dried to remove the solvent, thereby forming a coating layer, and the obtained coating layer is scraped off and made into a powder. Here, the above-mentioned "PET" refers to polyethylene terephthalate. It should be noted that the above-mentioned mixture is preferably subjected to the same mixing treatment as the mixing treatment performed in the process of preparing the coating liquid for catalyst layer formation (for example, mixing treatment based on a bead mill, etc.).

[0048] The catalyst layer is used in a polymer electrolyte fuel cell, thereby reducing the amount of catalyst used and achieving higher output of the fuel cell. The reason for this is not yet determined, but it is presumed as follows.

[0049] For specific mesopores, the pore surface area is large relative to the pore capacity. Therefore, the surface area of ​​the carbon carrier with specific mesopores is very large. For example, even if the total pore capacity of the specific mesopores in the carbon carrier accounts for about 30% of the total pore capacity of the mesopores and macropores as a whole, sometimes the total pore surface area of ​​the specific mesopores in the carbon carrier accounts for more than 85% of the total pore surface area of ​​the mesopores and macropores as a whole. That is, in the catalyst-loaded carbon in which catalyst particles containing platinum are loaded on the surface of the carbon carrier, although there are catalysts loaded on the surface other than the pores in the carbon carrier or the surface of the macropores, most of the catalysts are loaded on the surface of the specific mesopores.

[0050] Therefore, conventionally, in order to bring the ionomer into contact with as much catalyst as possible, attempts have been made to bring the catalyst inside the pores into contact with the ionomer.

[0051] However, it is known that when the ionomer comes into contact with the platinum catalyst particles, the ionomer is poisoned by the acidic functional groups thereof, and the catalytic activity of the platinum is reduced.

[0052] Therefore, in the catalyst layer of the present embodiment, the content of the ionomer is more than 100 parts by mass relative to 100 parts by mass of the carbon carrier, at least a portion of the ionomer is present in a specific mesopore and the ionomer occupancy is set to less than 50% by volume. In the catalyst layer of the present embodiment described above, the catalyst-supported carbon is surrounded by a sufficient amount of ionomer, and the amount of ionomer entering the interior of the specific mesopore decreases. The ionomer surrounding the catalyst-supported carbon and not entering the interior of the specific mesopore is in a state of being close to but not in contact with the catalyst loaded on the interior of the specific mesopore. It is believed that the ionomer in a state of being close but not in contact forms a pseudo three-phase interface with the aid of water in the reaction gas (for example, hydrogen, oxygen, etc. used in battery operation) and water generated by the reaction. Thus, it is believed that the catalyst activity of platinum caused by suppressing direct contact between the ionomer and platinum is reduced, and the catalyst activity of platinum can be effectively utilized by the formation of a pseudo three-phase interface.

[0053] Based on the above reasons, it is estimated that the catalyst layer of the present embodiment can reduce the amount of catalyst used and achieve high output of the fuel cell.

[0054] Hereinafter, each component constituting the catalyst layer will be described.

[0055] <Catalyst-supported carbon>

[0056] The catalyst-supported carbon comprises: a carbon support having specific mesopores and a catalyst containing platinum supported on the carbon support. The carbon support and the catalyst are described below.

[0057] The carbon support is not particularly limited as long as it is carbon having at least specific mesopores.

[0058] As the carbon carrier, activated carbon, carbon black, etc. can be cited. From the perspective of high chemical durability, it is recommended to perform at least a portion of graphitization by heat treatment, etc. In addition, as the carbon carrier, from the perspective of suppressing the ionomer occupancy to a low level, mesoporous carbon in which the ratio of the total pore volume occupied by macropores is less than 40% relative to the total pore volume of mesopores and macropores as a whole is preferred. The ratio of the total pore volume occupied by macropores is preferably 5 to 35%, and more preferably 10 to 30%.

[0059] The catalyst is not particularly limited as long as it contains platinum and promotes the redox reaction in the solid polymer fuel cell. The catalyst is preferably at least one selected from the group consisting of platinum and platinum alloys, and more preferably at least one selected from the group consisting of platinum particles and platinum alloy particles.

[0060] The platinum alloy is preferably an alloy of platinum and one or more metals selected from the group consisting of platinum group metals other than platinum (ruthenium, rhodium, palladium, osmium, iridium), gold, silver, chromium, iron, titanium, manganese, cobalt, nickel, molybdenum, tungsten, aluminum, silicon, zinc, and tin. The platinum alloy may include an intermetallic compound of a metal alloyed with platinum and platinum.

[0061] When the catalyst comprises at least one selected from the group consisting of platinum particles and platinum alloy particles, the number average particle size of the catalyst can be, for example, in the range of 1 nm to 20 nm. From the viewpoint of power generation performance and catalyst durability, the range of 2 nm to 10 nm is preferred, and the range of 2 nm to 7 nm is more preferred.

[0062] The number average particle size of the catalyst is a value obtained by averaging the equivalent circle diameters of 300 to 400 particles in an image observed at 300,000 times using a transmission electron microscope (TEM) HT7700 manufactured by Hitachi High-Technologies Corporation.

[0063] The method for supporting the catalyst on the carbon support is not particularly limited, and a known method such as a sputtering method, a solution method, an electrolytic deposition method, and an electroless plating method can be used.

[0064] The content of the catalyst relative to the entire catalyst-supported carbon is, for example, in the range of 10% to 70% by mass. From the viewpoint of achieving both reduction in the amount of catalyst used and increased output, the range is preferably 20% to 60%, and more preferably 30% to 60%.

[0065] The content of the catalyst in the catalyst layer per unit area is preferably 0.01 mg / cm from the viewpoint of the optimum thickness of the catalyst layer for efficiently performing the electrode reaction. 2 ~0.50mg / cm 2 From the perspective of the balance between raw material cost and performance, 0.05 mg / cm 2 ~0.35mg / cm 2 In particular, in the catalyst layer of this embodiment, in order to reduce the amount of catalyst used and to achieve high output, the content of the catalyst in the catalyst layer per unit area may be 0.20 mg / cm 2 the following.

[0066] The specific surface area of ​​the catalyst-supported carbon as a whole is preferably 200 m2 from the viewpoint of achieving both reduction in the amount of catalyst used and high output. 2 / g catalyst or more, more preferably 250m 2It should be noted that the specific surface area of ​​the entire catalyst-supported carbon refers to the total surface area per unit mass of the catalyst-supported carbon in a state where the ionomer is not attached.

[0067] In addition, the specific surface area of ​​the catalyst-supported carbon can be 700 m 2 / g catalyst or less, can be 500m 2 / g catalyst or less, and may be 350m 2 / g catalyst or less.

[0068] The specific surface area of ​​the entire catalyst-supported carbon is measured by nitrogen adsorption on the carbon surface using a BET specific surface area device.

[0069] The specific surface area of ​​mesopores in the catalyst-supported carbon is preferably 200 m2, for example, from the viewpoint of achieving both reduction in the amount of catalyst used and high output. 2 / g catalyst or more, more preferably 250m 2 It should be noted that the specific surface area of ​​the mesopores in the catalyst-supported carbon refers to the total pore surface area of ​​the mesopores in the catalyst-supported carbon per unit mass in a state where the ionomer is not attached. In addition, the specific surface area of ​​the catalyst-supported carbon as a whole can be 700 m 2 / g catalyst or less, can be 500m 2 / g catalyst or less, and may be 350m 2 / g catalyst or less.

[0070] The specific surface area of ​​the specific mesopores in the catalyst-supported carbon is more preferably 200 m 2 It should be noted that the specific surface area of ​​the specific mesopores in the catalyst-supported carbon refers to the total pore surface area of ​​the specific mesopores in the catalyst-supported carbon per unit mass in a state where the ionomer is not attached.

[0071] The total pore volume of specific mesopores per unit mass in the catalyst-supported carbon in a state where the ionomer is not attached is, for example, 0.1 cm 3 / g catalyst~0.8cm 3 The range of / g catalyst is preferably 0.15 cm / g from the viewpoint of gas diffusibility and power generation performance. 3 / g catalyst~0.7cm 3 / g catalyst, more preferably 0.2 cm 3 / g catalyst~0.6cm 3 / g catalyst range.

[0072] The ratio of the total pore volume of specific mesopores in the catalyst-loaded carbon in the state where the ionomer is not attached to the total pore volume of the mesopores and macropores as a whole can be, for example, in the range of 20% to 90%. From the viewpoint of the drainage of the generated water and the power generation performance, the range of 25% to 80% is preferred, and the range of 30% to 70% is more preferred.

[0073] The total pore volume of the macropores in the catalyst-supported carbon per unit mass in a state where the ionomer is not attached is, for example, 0.05 cm 3 / g catalyst, preferably 0.07 cm 3 / g catalyst~0.50cm 3 / g catalyst, more preferably 0.1cm 3 / g catalyst~0.4cm 3 / g catalyst range.

[0074] <Ionomer>

[0075] The ionomer is not particularly limited as long as it is a polymer compound having an ion exchange group, and a polymer compound having proton conductivity is preferred. Hereinafter, a polymer compound having an ion exchange group is also referred to as an "ion exchange resin". "Ion exchange group" refers to a polymer having H + , monovalent metal cations, ammonium ions, etc.

[0076] Examples of the ion exchange group include sulfonic acid group, sulfonylimide group, sulfonamide group, sulfonemethide group, carboxyl group, phosphoric acid group, etc. Among them, sulfonic acid group having excellent proton conductivity is preferred. The ion exchange group may be used alone or in combination of two or more.

[0077] As the ionomer, from the viewpoint of durability, a fluorine-containing ion exchange resin is preferred, and a perfluorocarbon polymer having an ion exchange group is more preferred. It should be noted that the perfluorocarbon polymer may contain etheric oxygen atoms.

[0078] Examples of the perfluorocarbon polymer include the polymer (H) described below, the polymer (Q) described below, and known polymers such as polymers having an ion exchange group and a structural unit derived from a perfluoromonomer having a 5-membered ring as described in International Publication No. 2011 / 013577, etc. The ionomer preferably contains at least one selected from the group consisting of the polymer (H) and the polymer (Q) from the perspective of ease of availability and ease of manufacture.

[0079] It should be noted that "polymer" refers to a compound having a structure composed of a plurality of structural units. In addition, "structural unit" refers to a unit derived from a monomer formed by polymerization of the monomer. The structural unit may be a unit directly formed by the polymerization reaction of the monomer, or may be a unit in which a part of the unit is converted into another structure by treating the polymer. "Monomer" refers to a compound having a polymerization-reactive carbon-carbon double bond.

[0080] Polymer (H):

[0081] The polymer (H) is a polymer having the following unit (U1) (however, excluding the polymer (Q)).

[0082]

[0083] Among them, in the above unit (U1), Q 3 is a single bond or a perfluoroalkylene group which may have an ethereal oxygen atom, R f2 is a perfluoroalkyl group which may have an ethereal oxygen atom, X 2 is an oxygen atom, a nitrogen atom, or a carbon atom, and b is 2 When it is an oxygen atom, it is 0, X 2 When it is a nitrogen atom, it is 1, X 2 For carbon atoms, it is 2, Y 2 is a fluorine atom or a monovalent perfluorinated organic group, and t is 0 or 1. A single bond refers to CFY 2 The carbon atom of SO2 is directly bonded to the sulfur atom of SO2. The organic group refers to a group containing one or more carbon atoms.

[0084] Q in the above unit (U1) 3 When the perfluoroalkylene group has an etheric oxygen atom, the number of the oxygen atom may be 1 or 2 or more. In addition, the oxygen atom may be inserted between carbon-carbon bonds of the perfluoroalkylene group or may be inserted at the end of a carbon bond.

[0085] The perfluoroalkylene group may be linear or branched.

[0086] The perfluoroalkylene group preferably has 1 to 6 carbon atoms, more preferably 1 to 4 carbon atoms.

[0087] R in the above unit (U1) f2 The perfluoroalkyl group shown may be linear or branched, but is preferably linear.

[0088] The carbon number of the perfluoroalkyl group is preferably 1 to 6, more preferably 1 to 4. As the perfluoroalkyl group, a perfluoromethyl group, a perfluoroethyl group, etc. are preferred.

[0089] In the above unit (U1), -(SO2X 2 (SO2Rf2 ) b ) - H + The group is an ion exchange group.

[0090] As the -(SO2X 2 (SO2R f2 ) b ) - H + The groups include sulfonic acid groups (-SO3 - H + sulfonimide (-SO2N(SO2R f2 ) - H + yl), or sulfonylmethylene (-SO2C(SO2R f2 )2) - H + base).

[0091] As Y in the above unit (U1) 2 , preferably a fluorine atom or a trifluoromethyl group.

[0092] The unit (U1) is preferably the following unit (U1-1), and is more preferably the following unit (U1-11), unit (U1-12), unit (U1-13), or unit (U1-14) from the viewpoint of easy production of the polymer (H) and easy industrial implementation.

[0093]

[0094] In the above unit (U1-1), Z is a fluorine atom or a trifluoromethyl group, t is 0 or 1, m is an integer from 0 to 3, n is an integer from 1 to 12, p is 0 or 1, and m+p>0.

[0095] The polymer (H) may further have a structural unit derived from other monomers (hereinafter referred to as other units). The ratio of the other units can be appropriately adjusted so that the ion exchange capacity of the polymer (H) is within the preferred range described below.

[0096] As the other unit, from the viewpoint of mechanical strength and chemical durability, a structural unit derived from a perfluoromonomer is preferred, and a structural unit derived from tetrafluoroethylene (hereinafter referred to as TFE) is more preferred.

[0097] The polymer (H) can be produced by polymerizing the following compound (M1) and other monomers as needed to obtain a precursor polymer, and then converting the -SO2F groups in the precursor polymer into sulfonic acid groups. The conversion of the sulfonic acid groups into -SO2F groups is carried out by hydrolysis and acidification.

[0098] CF2=CF-(CF2) t OCF2-CFY 2 -Q 3 -SO2F···(M1).

[0099] It should be noted that t and Y in the above compound (M1) 2 , and Q 3 Respectively with t, Y in the above unit (U1) 2 , and Q 3 Same meaning.

[0100] Polymer (Q):

[0101] The polymer (Q) is a polymer having at least one of the following units (U2) and the following units (U3).

[0102]

[0103] Among them, in the above unit (U2), Q 1 is a perfluoroalkylene group which may have an ethereal oxygen atom, Q 2 is a single bond or a perfluoroalkylene group which may have an ethereal oxygen atom, R f1 is a perfluoroalkyl group which may have an ethereal oxygen atom, X 1 is an oxygen atom, a nitrogen atom, or a carbon atom, and a is 1 When it is an oxygen atom, it is 0. 1 When it is a nitrogen atom, it is 1. 1 For carbon atoms, it is 2, Y 1 is a fluorine atom or a monovalent perfluorinated organic group, and s is 0 or 1. A single bond refers to CY 1 The carbon atom of SO2 is directly bonded to the sulfur atom of SO2. An organic group is a group containing one or more carbon atoms.

[0104] In the above unit (U2), Q 1 , Q 2 When the perfluoroalkylene group has an etheric oxygen atom, the oxygen atom may be 1 or 2 or more. In addition, the oxygen atom may be inserted between carbon atom-carbon atom bonds of the perfluoroalkylene group or may be inserted at the end of the carbon atom bond.

[0105] The perfluoroalkylene group may be linear or branched, but is preferably linear.

[0106] The carbon number of the perfluoroalkylene group is preferably 1 to 6, more preferably 1 to 4. When the carbon number is 6 or less, the boiling point of the fluorinated monomer as a raw material becomes low, and purification by distillation becomes easy.

[0107] Q in the above unit (U2) 2It is preferably a perfluoroalkylene group having 1 to 6 carbon atoms which may have an ethereal oxygen atom. 2 When it is a perfluoroalkylene group having 1 to 6 carbon atoms which may have an ethereal oxygen atom, 2 Compared with the case of a single bond, the stability of power generation performance is excellent when the solid polymer fuel cell is operated for a long period of time.

[0108] In the above unit (U2), Q 1 , Q 2 At least one of them is a C1-6 perfluoroalkylene group having an etheric oxygen atom. The fluorinated monomer containing a C1-6 perfluoroalkylene group having an etheric oxygen atom can be synthesized without a fluorination reaction using fluorine gas, and thus has a good yield and is easy to produce.

[0109] In the above unit (U2), R f1 The perfluoroalkyl group may be linear or branched, but is preferably linear.

[0110] The carbon number of the perfluoroalkyl group is preferably 1 to 6, more preferably 1 to 4. As the perfluoroalkyl group, a perfluoromethyl group, a perfluoroethyl group, etc. are preferred.

[0111] Unit (U2) has 2 or more R f1 In the case of R f1 They may be the same group or different groups.

[0112] In the above unit (U2), -(SO2X 1 (SO2R f1 ) a ) - H + The group is an ion exchange group.

[0113] As the -(SO2X 1 (SO2R f1 ) a ) - H + The groups include sulfonic acid groups (-SO3 - H + sulfonimide (-SO2N(SO2R f1 ) - H + yl), or sulfonylmethylene (-SO2C(SO2R f1 )2) - H + base).

[0114] As Y in the above unit (U2) 1 , preferably a fluorine atom or a linear perfluoroalkyl group having 1 to 6 carbon atoms which may have an ethereal oxygen atom.

[0115] The unit (U2) is preferably the following unit (U2-1), and is more preferably the following unit (U2-11), unit (U2-12), or unit (U2-13) from the viewpoint of easy production of the polymer (Q) and easy industrial implementation.

[0116]

[0117] Among them, in the above unit (U2-1), R F11 is a single bond or a linear perfluoroalkylene group having 1 to 6 carbon atoms which may have an ethereal oxygen atom, R F12 It is a linear perfluoroalkylene group having 1 to 6 carbon atoms, and s is 0 or 1.

[0118]

[0119] Among them, in the above unit (U3), R F1 and R F2 Each is independently a perfluoroalkylene group having 1 to 3 carbon atoms.

[0120] As R F1 and R F2 Specific examples include -CF2-, -CF2CF2-, -CF(CF3)-, -CF2CF2CF2-, -CF(CF2CF3)-, -CF(CF3)CF2-, -CF2CF(CF3)-, and -C(CF3)(CF3)-.

[0121] From the perspectives of low-cost raw materials, easy production, and the ability to further increase the ion exchange capacity of the polymer (Q), R F1 and R F2 Each independently is preferably a perfluoroalkylene group having 1 or 2 carbon atoms. A straight chain is preferred when the carbon number is 2. Specifically, -CF2-, -CF2CF2- or -CF(CF3)- is preferred, -CF2- or -CF2CF2- is more preferred, and -CF2- is particularly preferred.

[0122] As the unit (U3), the following unit (U3-1) is preferred.

[0123]

[0124] The polymer (Q) may further have other units. The ratio of other units can be appropriately adjusted so that the ion exchange capacity of the polymer (Q) is within the preferred range described below.

[0125] As the other unit, from the viewpoint of mechanical strength and chemical durability, a structural unit derived from a perfluoromonomer is preferred, and a structural unit derived from TFE is more preferred.

[0126] The polymer (Q) can be produced by the methods described in, for example, International Publication No. 2007 / 013533, International Publication No. 2020 / 116651, and the like.

[0127] The ion exchange capacity of the ionomer is preferably 0.5 to 2.0 milliequivalents / g dry resin, particularly preferably 0.8 to 1.5 milliequivalents / g dry resin, from the viewpoint of electrical conductivity and gas permeability.

[0128] The content of the ionomer is 100 parts by mass or more relative to 100 parts by mass of the carbon carrier. From the viewpoint of achieving both reduction in the amount of catalyst used and high output, it is preferably 100 parts by mass to 240 parts by mass, more preferably 110 parts by mass to 200 parts by mass, and further preferably 120 parts by mass to 180 parts by mass.

[0129] <Characteristics of Catalyst Layer>

[0130] The ionomer occupancy is 50% by volume or less, and preferably 10% by volume to 50% by volume from the viewpoint of achieving both reduction in the amount of catalyst used and high output. In addition, from the viewpoint of achieving both reduction in the amount of catalyst used and high output in a low humidity environment (e.g., an environment with a humidity of 30%), the ionomer occupancy is more preferably 15% by volume to 40% by volume, and further preferably 20% by volume to 35% by volume.

[0131] Examples of methods for increasing the ionomer content and reducing the ionomer occupancy include adjusting the mixing conditions in the process of preparing the catalyst layer-forming coating liquid and adjusting the properties of the materials used in preparing the catalyst layer-forming coating liquid. These methods may be used in combination.

[0132] Examples of a method for adjusting the mixing treatment conditions include a method of reducing the shear stress applied during the mixing treatment and a method of shortening the treatment time of the mixing treatment.

[0133] Methods for adjusting the properties of the material include using a thickening ionomer (for example, an ionomer having a viscosity increased by adding a fluorine-based solvent), using an ionomer having a large molecular weight, and using a hydrophilized catalyst-loaded carbon (for example, a catalyst-loaded carbon having an increased amount of hydrophilic functional groups on the surface by acid treatment).

[0134] The catalyst-supported carbon in the catalyst layer preferably has a diameter of 0.03 cm 3 / g catalyst or more macropores, wherein the pore diameter of the macropores in the pore distribution obtained by a nitrogen adsorption method is 50 nm or more.

[0135] The total pore volume of the macropores per unit mass of the catalyst-supported carbon in the state where the ionomer is attached is, for example, 0.03 cm 3 / g catalyst~0.3cm 3 / g catalyst, from the viewpoint of both reducing the amount of catalyst used and increasing output, preferably 0.05 cm 3 / g catalyst~0.25cm 3 / g catalyst, more preferably 0.07cm 3 / g catalyst~0.20cm 3 / g catalyst range.

[0136] The thickness of the catalyst layer is not particularly limited, and is, for example, in the range of 0.5 μm to 10 μm, preferably in the range of 1 μm to 8 μm, and more preferably in the range of 2 μm to 6 μm.

[0137] The thickness of the catalyst layer can be measured by observing the cross section of the catalyst layer using a scanning electron microscope or the like.

[0138] <Method for producing catalyst layer>

[0139] The method for manufacturing a catalyst layer, for example, includes the following steps: a preparation step of preparing a coating liquid for forming a catalyst layer; and a catalyst layer forming step of coating the coating liquid for forming a catalyst layer on the surface of a layer in contact with the catalyst layer in a membrane electrode assembly (gas diffusion layer, polymer electrolyte membrane, etc.) or on the surface of a substrate film, and drying the coating liquid to thereby form a catalyst layer.

[0140] When the coating liquid for forming a catalyst layer is applied to the surface of the substrate film, a transfer step of transferring the formed catalyst layer to the surface of a layer in contact with the catalyst layer in the membrane electrode assembly may be further performed.

[0141] In the preparation process, for example, catalyst-supported carbon, ionomer, and a solvent as required are mixed to prepare a coating liquid for catalyst layer formation. The catalyst-supported carbon and ionomer may each be pre-dispersed in a solvent. That is, a dispersion liquid in which the catalyst-supported carbon is dispersed and a dispersion liquid in which the ionomer is dispersed may be mixed.

[0142] Examples of the solvent include aqueous solvents such as water, alcohol, and mixtures thereof, and organic solvents. Among them, aqueous solvents are preferred from the viewpoint of safety during coating and drying.

[0143] The mixing method is not particularly limited, and examples thereof include known mixing methods such as mixing with a bead mill, mixing with a ball mill, mixing with an ultrasonic disperser, and a jet mill. Among them, mixing with a bead mill is preferred from the viewpoint of reducing the ionomer content.

[0144] The solid content concentration of the catalyst layer-forming coating liquid is not particularly limited, and is, for example, in the range of 5% by mass to 30% by mass.

[0145] The substrate film used in the catalyst layer forming step may include, in addition to the PET film, an ETFE film, an olefin resin film, etc. The above-mentioned "ETFE" refers to a tetrafluoroethylene-ethylene copolymer resin.

[0146] The method of applying the catalyst layer-forming coating liquid is not particularly limited, and examples thereof include known methods such as a die coating method.

[0147] The method of drying the layer of the applied catalyst layer-forming coating liquid can be a known method. The drying temperature is, for example, in the range of 40° C. to 130° C., preferably in the range of 45° C. to 80° C. The drying time is, for example, in the range of 0.5 minutes to 10 minutes, preferably in the range of 1 minute to 7 minutes.

[0148] [Membrane electrode assembly for polymer electrolyte fuel cells]

[0149] The membrane electrode assembly for a solid polymer fuel cell of the present embodiment (hereinafter also referred to as a "membrane electrode assembly") comprises: an anode having a first gas diffusion layer and a first catalyst layer arranged on one side of the first gas diffusion layer; a cathode having a second gas diffusion layer and a second catalyst layer arranged on one side of the second gas diffusion layer; and a polymer electrolyte membrane arranged between the first catalyst layer and the second catalyst layer, and at least one of the first catalyst layer and the second catalyst layer is the aforementioned catalyst layer.

[0150] Hereinafter, the membrane electrode assembly according to the present embodiment will be described with reference to the drawings.

[0151] Figure 1 2 is a schematic cross-sectional view showing an example of a mode in which the above-mentioned catalyst layer is used as the second catalyst layer as the cathode catalyst layer in the membrane electrode assembly of the present embodiment.

[0152] Figure 1 The membrane electrode assembly 10 shown includes: an anode 13 having a catalyst layer 11 and a gas diffusion layer 12, a cathode 14 having a catalyst layer 21 and a gas diffusion layer 22, and a polymer electrolyte membrane 15 arranged between the anode 13 and the cathode 14 in contact with the catalyst layer 11 and the catalyst layer 21.

[0153] Furthermore, the catalyst layer 21 is the aforementioned catalyst layer.

[0154] The catalyst layer 21 and the catalyst layer 11 may be layers having the same components, composition, thickness, etc., or may be different layers.

[0155] The catalyst layer 11 may include, for example, a layer containing catalyst-supported carbon and an ionomer. The catalyst layer 11 may be the catalyst layer of the aforementioned embodiment, or may be a catalyst layer other than the catalyst layer of the aforementioned embodiment. It should be noted that, as the catalyst-supported carbon and the ionomer in the catalyst layer 11, the same examples as those of the catalyst-supported carbon and the ionomer in the catalyst layer of the aforementioned embodiment may be used.

[0156] The gas diffusion layer 12 and the gas diffusion layer 22 have the function of uniformly diffusing the gas in the catalyst layer 11 and the catalyst layer 21, respectively, and the function of being a collector. The gas diffusion layer 12 and the gas diffusion layer 22, for example, include a gas diffusion substrate. As the gas diffusion layer 12 and the gas diffusion layer 22, carbon paper, carbon cloth, carbon felt, etc. can be cited. The gas diffusion layer 12 and the gas diffusion layer 22 are preferably treated with water repellency using polytetrafluoroethylene or the like. It should be noted that the gas diffusion layer 12 and the gas diffusion layer 22 can be layers with the same composition, composition, thickness, etc., or they can be different layers.

[0157] The anode 13 may have a carbon layer (not shown) as an intermediate layer between the catalyst layer 11 and the gas diffusion layer 12. In addition, the cathode 14 may also have a carbon layer (not shown) as an intermediate layer between the catalyst layer 21 and the gas diffusion layer 22. By having the carbon layer, the gas diffusion property of the surface of the catalyst layer is improved, and the power generation performance of the solid polymer fuel cell is greatly improved.

[0158] As the carbon layer, for example, a layer containing carbon and a nonionic fluorine-containing polymer can be cited. As the carbon used in the carbon layer, for example, a carbon nanofiber having a fiber diameter of 1 nm to 1000 nm and a fiber length of 1000 μm or less can be cited. As the nonionic fluorine-containing polymer, for example, polytetrafluoroethylene can be cited.

[0159] The polymer electrolyte membrane 15 is a membrane containing an ion exchange resin. As the ion exchange resin, from the aspect of durability, a fluorine-containing ion exchange resin is preferred, a perfluorocarbon polymer having an ion exchange group is more preferred, the above-mentioned polymer (H) or polymer (Q) is further preferred, and polymer (H) is particularly preferred. It should be noted that the above-mentioned perfluorocarbon polymer may contain etheric oxygen atoms.

[0160] The ion exchange capacity of the fluorine-containing ion exchange resin is preferably 0.5 to 2.0 milliequivalents / g of dry resin, particularly preferably 0.8 to 1.5 milliequivalents / g of dry resin.

[0161] It should be noted that the ion exchange capacity of the fluorinated ion exchange resin can be measured by the same method as that for the ion exchange capacity of the ionomer.

[0162] The polymer electrolyte membrane 15 can be reinforced with a reinforcing material. Examples of the reinforcing material include porous bodies, fibers, woven fabrics, nonwoven fabrics, etc. Examples of the reinforcing material include polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymers, tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymers, polyethylene, polypropylene, polyphenylene sulfide, etc.

[0163] In order to further improve durability, the polymer electrolyte membrane 15 may contain one or more atoms selected from the group consisting of cerium and manganese. Cerium and manganese decompose hydrogen peroxide, which is a causative substance for deterioration of the polymer electrolyte membrane 15. Cerium and manganese are preferably present in the polymer electrolyte membrane 15 in the form of ions.

[0164] The polymer electrolyte membrane 15 may contain silicon dioxide, a heteropoly acid (zirconium phosphate, phosphomolybdic acid, phosphotungstic acid, etc.) or the like as a moisture retaining agent for preventing drying.

[0165] The thickness of the polymer electrolyte membrane is preferably 10 μm to 30 μm, more preferably 15 μm to 25 μm. When the thickness of the polymer electrolyte membrane is below the upper limit of the aforementioned range, the reduction in the power generation performance of the solid polymer fuel cell under low humidification conditions is suppressed. In addition, by setting the thickness of the polymer electrolyte membrane to be above the lower limit of the aforementioned range, gas leakage and electrical short circuit can be suppressed.

[0166] The thickness of the polymer electrolyte membrane can be measured by observing a cross section of the polymer electrolyte membrane using a scanning electron microscope or the like.

[0167] <Method for Manufacturing Membrane Electrode Assembly>

[0168] The membrane electrode assembly 10 is produced, for example, by the following method.

[0169] (α) A method in which the catalyst layer 11 and the catalyst layer 21 are formed on the polymer electrolyte membrane 15 to produce a membrane-catalyst layer assembly, and the membrane-catalyst layer assembly is sandwiched between the gas diffusion layers 12 and the gas diffusion layers 22 .

[0170] (β) A method in which the catalyst layer 11 is formed on the gas diffusion layer 12 to form the anode 13 , the catalyst layer 21 is formed on the gas diffusion layer 22 to form the cathode 14 , and the polymer electrolyte membrane 15 is sandwiched between the anode 13 and the cathode 14 .

[0171] When the membrane electrode assembly 10 has a carbon layer, the membrane electrode assembly 10 is produced, for example, by the following method.

[0172] (γ) A dispersion containing carbon and a nonionic fluorine-containing polymer is coated on a substrate film and dried to form a carbon layer, a catalyst layer 11 is formed on the carbon layer, and a laminate having a carbon layer and a catalyst layer 21 sequentially formed on a substrate film is prepared by the same method, the catalyst layer 11 and the polymer electrolyte membrane 15 are laminated, and the catalyst layer 21 and the polymer electrolyte membrane 15 are laminated, respectively, and each substrate film is peeled off to prepare a membrane-catalyst layer assembly having a carbon layer, and the membrane-catalyst layer assembly is clamped by a gas diffusion layer 12 and a gas diffusion layer 22.

[0173] (δ) A method in which a dispersion containing carbon and a nonionic fluorine-containing polymer is coated on a gas diffusion layer 12 and a gas diffusion layer 22, respectively, and the dispersion is dried to form a carbon layer, and a membrane-catalyst layer assembly having a catalyst layer 11 and a catalyst layer 21 is formed on a polymer electrolyte membrane 15 by sandwiching the gas diffusion layer 12 having the carbon layer and the gas diffusion layer 22 having the carbon layer.

[0174] The polymer electrolyte membrane 15 can be formed, for example, by a method (casting method) in which a liquid composition containing an ion exchange resin is applied onto a substrate film or a catalyst layer (catalyst layer 11 or catalyst layer 21) and then dried.

[0175] When the polymer electrolyte membrane 15 is formed, for example, a liquid composition containing a liquid medium, a fluorine-containing polymer having a sulfonic acid group, and trivalent or tetravalent cerium ions can be used.

[0176] When the above-mentioned liquid composition is used, it is preferred to perform heat treatment in order to stabilize the polymer electrolyte membrane 15. The temperature of the heat treatment varies depending on the type of ion exchange resin, and is preferably 130°C to 200°C. When the temperature of the heat treatment is 130°C or higher, the ion exchange resin will not contain excessive water. When the temperature of the heat treatment is 200°C or lower, the thermal decomposition of the sulfonic acid group can be suppressed, and the reduction in the proton conductivity of the polymer electrolyte membrane 15 can be suppressed. The polymer electrolyte membrane 15 can be treated with hydrogen peroxide water as needed.

[0177] [Solid polymer fuel cell]

[0178] The polymer electrolyte fuel cell of the present embodiment includes the above-mentioned membrane electrode assembly.

[0179] A polymer electrolyte fuel cell is produced, for example, by sandwiching a membrane electrode assembly between two separators to form a cell and stacking a plurality of cells.

[0180] Examples of the separator include a conductive carbon plate having grooves formed therein as passages for a fuel gas or an oxidant gas containing oxygen (air, oxygen, etc.).

[0181] Examples of the types of polymer electrolyte fuel cells include hydrogen / oxygen fuel cells, direct methanol fuel cells (DMFC), etc. Methanol or methanol aqueous solution used as fuel for DMFC may be supplied as a liquid or gaseous feed.

[0182] Example

[0183] Hereinafter, the present disclosure will be described in detail with reference to examples and reference examples, but the present disclosure is not limited to the following examples.

[0184] [Catalyst supported carbon]

[0185] As the catalyst-supported carbon, the following catalyst-supported carbon (1), catalyst-supported carbon (2), and catalyst-supported carbon (3) were prepared.

[0186] Catalyst-supported carbon (1): Catalyst: Catalyst content of the entire catalyst-supported carbon relative to platinum particles: 60 mass %, number average particle size of platinum particles: 4.8 nm

[0187] Catalyst-supported carbon (2): Catalyst: Catalyst content of the entire catalyst-supported carbon relative to platinum particles: 50% by mass, number average particle size of platinum particles: 3.3 nm

[0188] Catalyst-supported carbon (3): Catalyst: Catalyst content of the entire catalyst-supported carbon relative to platinum particles: 20 mass %, number average particle size of platinum particles: 2.5 nm

[0189] It should be noted that as the catalyst-supported carbon (3), a common platinum-supported carbon catalyst having a platinum supporting rate of 20% was used.

[0190] The characteristics of the catalyst-supported carbon (1) are as follows.

[0191] Overall specific surface area: 283m 2 / g catalyst

[0192] Total pore volume of specific mesopores: 0.15 cm 3 / g catalyst

[0193] The proportion of the total pore volume of specific mesopores to the total volume of mesopores and macropores: 28%

[0194] Total pore volume of macropores: 0.25 cm 3 / g catalyst

[0195] The characteristics of the catalyst-supported carbon (2) are as follows.

[0196] Overall specific surface area: 410m 2 / g catalyst

[0197] Total pore volume of specific mesopores: 0.15 cm 3 / g catalyst

[0198] The ratio of the total pore volume of specific mesopores to the total volume of mesopores and macropores: 50%

[0199] Total pore volume of macropores: 0.25 cm 3 / g catalyst

[0200] [Ionomer dispersion]

[0201] As an ionomer, a polymer (H1) having a structural unit derived from TFE and the above-mentioned unit (U1-11) (ion exchange capacity: 1.1 milliequivalent / g dry resin) was prepared.

[0202] The polymer (H1) was dispersed in a dispersion medium of ethanol / water = 6 / 4 (mass ratio) to prepare a polymer (H1) dispersion (A) having a solid content concentration of 25.0 mass %.

[0203] [Preparation of coating liquid for forming catalyst layer]

[0204] <Coating liquid (a1)>

[0205] 50.0 g of catalyst-supported carbon (1) was added to 363 g of distilled water and stirred thoroughly. 177 g of ethanol and 65 g of 2-propanol were further added and stirred thoroughly. 56.0 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using 1 mm zirconium oxide beads at a peripheral speed of 6 m / s and a residence time of 1.1 minutes to prepare a coating solution (a1).

[0206] <Coating liquid (a2)>

[0207] 50.0 g of catalyst-supported carbon (1) was added to 389 g of distilled water and stirred thoroughly. 188 g of ethanol and 71 g of 2-propanol were further added and stirred thoroughly. 80.0 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using 1 mm zirconium oxide beads at a peripheral speed of 6 m / s and a residence time of 1.1 minutes to prepare a coating liquid (a2).

[0208] <Coating liquid (a3)>

[0209] 50.0 g of catalyst-supported carbon (1) was added to 431 g of distilled water and stirred thoroughly. 207 g of ethanol and 81 g of 2-propanol were further added and stirred thoroughly. 120 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using 1 mm zirconium oxide beads at a peripheral speed of 6 m / s and a residence time of 1.1 minutes to prepare a coating liquid (a3).

[0210] <Coating liquid (a4)>

[0211] 50.0 g of catalyst-supported carbon (1) was added to 363 g of distilled water and stirred thoroughly. 177 g of ethanol and 65 g of 2-propanol were further added and stirred thoroughly. 56.0 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using 0.5 mm zirconium oxide beads at a peripheral speed of 8 m / s and a residence time of 5.5 minutes to prepare a coating liquid (a4).

[0212] <Coating liquid (a5)>

[0213] 50.0 g of catalyst-supported carbon (1) was added to 389 g of distilled water and stirred thoroughly. 188 g of ethanol and 71 g of 2-propanol were further added and stirred thoroughly. 80.0 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using 0.5 mm zirconium oxide beads at a peripheral speed of 8 m / s and a residence time of 5.5 minutes to prepare a coating liquid (a5).

[0214] <Coating liquid (a6)>

[0215] 50.0 g of catalyst-supported carbon (1) was added to 431 g of distilled water and stirred thoroughly. 207 g of ethanol and 81 g of 2-propanol were further added and stirred thoroughly. 120 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using 0.5 mm zirconium oxide beads at a peripheral speed of 8 m / s and a residence time of 5.5 minutes to prepare a coating liquid (a6).

[0216] <Coating liquid (a7)>

[0217] 50.0 g of catalyst-supported carbon (3) was added to 357 g of distilled water and stirred thoroughly. 376 g of ethanol was further added and stirred thoroughly. 128 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using zirconia beads of 1.0 mm to a peripheral speed of 6 m / s and a residence time of 4.3 minutes to prepare a coating liquid (a7).

[0218] <Coating liquid (a8)>

[0219] 50.0 g of catalyst-supported carbon (2) was added to 375 g of distilled water and stirred thoroughly. 397 g of ethanol was further added and stirred thoroughly. 150 g of polymer (H1) dispersion (A) was added thereto and dispersed in a bead mill (LZ015 manufactured by Ashizawa Finetech Ltd.) using zirconia beads of 1.0 mm at a peripheral speed of 6 m / s and a residence time of 1.1 minutes to prepare a coating solution (a8).

[0220] [Preparation of coating liquid for forming intermediate layer (carbon layer)]

[0221] <Coating liquid (c1)>

[0222] 21.0 g of ethanol and 24.0 g of distilled water were added to 10.0 g of vapor-grown carbon fiber (manufactured by Showa Denko K.K., trade name: VGCF-H, average fiber diameter: about 150 nm, fiber length: 10 to 20 μm), and the mixture was stirred thoroughly. 20.0 g of the polymer (H1) dispersion (A) was added thereto, stirred thoroughly, and then mixed and pulverized with a homogenizer to prepare a coating liquid (c1).

[0223] [Formation of Catalyst Layer]

[0224] <Example C1>

[0225] A gas diffusion layer substrate (H2315 T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) with a platinum content of 0.20 mg / cm 2 The coating liquid (a1) is applied in a manner and dried to obtain a cathode (gc1). It should be noted that the above-mentioned "amount of platinum" refers to the content of the catalyst in the catalyst layer per unit area.

[0226] A gas diffusion layer substrate with a barrier layer (25BC manufactured by SGL Carbon Co., Ltd.) was coated with platinum in an amount of 0.05 mg / cm using a die coater. 2The coating liquid (a7) is applied in a manner and dried to obtain an anode (ga1).

[0227] As the polymer electrolyte membrane, a 20 μm thick ion exchange membrane made of a perfluorocarbon polymer having a sulfonic acid group (manufactured by Asahi Glass Co., Ltd., trade name: FLEMION, ion exchange capacity: 1.1 milliequivalent / g dry resin) was prepared.

[0228] The polymer electrolyte membrane was sandwiched between the anode (ga1) and the cathode (gc1), and the catalyst layers of the anode (ga1) and the cathode (gc1) were pressed onto the polymer electrolyte membrane by hot pressing to obtain a membrane electrode assembly (electrode area: 25 cm 2 ).

[0229] <Example 1>

[0230] A gas diffusion layer substrate (H2315 T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) with a platinum content of 0.20 mg / cm 2 The coating liquid (a2) is applied in a manner and dried to obtain a cathode (gc2).

[0231] A membrane electrode assembly was obtained in the same manner as in Example C1 except that the cathode (gc2) was used instead of the cathode (gc1).

[0232] <Example 2>

[0233] A gas diffusion layer substrate (H2315 T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) with a platinum content of 0.20 mg / cm 2 The coating liquid (a3) ​​is applied in a manner and dried to obtain a cathode (gc3).

[0234] A membrane electrode assembly was obtained in the same manner as in Example C1 except that the cathode (gc3) was used instead of the cathode (gc1).

[0235] <Example C2>

[0236] A gas diffusion layer substrate (H2315 T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) with a platinum content of 0.20 mg / cm 2The coating liquid (a4) is applied in a manner and dried to obtain a cathode (gc4).

[0237] A membrane electrode assembly was obtained in the same manner as in Example C1 except that the cathode (gc4) was used instead of the cathode (gc1).

[0238] <Example 3>

[0239] A gas diffusion layer substrate (H2315T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) with a platinum content of 0.20 mg / cm 2 The coating liquid (a5) is applied in a manner and dried to obtain a cathode (gc5).

[0240] A membrane electrode assembly was obtained in the same manner as in Example C1 except that the cathode (gc5) was used instead of the cathode (gc1).

[0241] <Example C3>

[0242] A gas diffusion layer substrate (H2315 T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) with a platinum content of 0.20 mg / cm 2 The coating liquid (a6) is applied in a manner and dried to obtain a cathode (gc6).

[0243] A membrane electrode assembly was obtained in the same manner as in Example C1 except that the cathode (gc6) was used instead of the cathode (gc1).

[0244] <Example 4>

[0245] A gas diffusion layer substrate (H2315 T10X6 manufactured by NOK) without a barrier layer was coated with a die coater to give a solid content of 3.0 mg / cm 2 The coating liquid (c1) was applied and dried, and a die coater was used to coat the coating liquid (c1) in an amount of 0.10 mg / cm 2 The coating liquid (a8) is applied in a manner and dried to obtain a cathode (gc7).

[0246] A membrane electrode assembly was obtained in the same manner as in Example C1 except that the cathode (gc7) was used instead of the cathode (gc1).

[0247] [Measurement and evaluation]

[0248] <Content of ionomer relative to 100 parts by mass of carbon support>

[0249] The contents (parts by mass) of the ionomer in the cathodes of the above examples relative to 100 parts by mass of the carbon support are shown in Table 1 (“ionomer content” in Table 1).

[0250] <Ionomer Occupancy Ratio>

[0251] The coating liquid used in forming the cathode of the above example was applied on a PET film and dried, and the coating layer was scraped off, and the resulting powder was used as a "sample of catalyst-supported carbon with ionomer attached". In addition, a coating liquid not containing ionomer (i.e., a mixed solution of catalyst-supported carbon and a solvent) was applied on a PET film and dried, and the coating layer was scraped off, and the resulting powder was used as a "sample of catalyst-supported carbon without ionomer attached". Using these samples, the pore distribution was determined by the above-mentioned method, and the ionomer occupancy (%) of each example was calculated. The results are shown in Table 1.

[0252] <Macropore and fine pore capacity after ionomer attachment>

[0253] Based on the pore distribution of the above-mentioned "catalyst-supported carbon sample with ionomer attached" of each example, the total pore volume (cm2) of the macropores per unit mass of the catalyst-supported carbon in the state where the ionomer is attached was determined. 3 / g catalyst). The results are shown in Table 1 ("Macropore capacity" in Table 1).

[0254] <Power Generation Performance (1)>

[0255] The membrane electrode assembly obtained in the above example was assembled into a power generation cell, and hydrogen (utilization rate 70%) / air (utilization rate 50%) were supplied under normal pressure. The current density was measured at a cell temperature of 80°C at 1.0 A / cm 2 The battery cell voltage (V) at the initial stage of operation under . It should be noted that hydrogen with a dew point of 80°C was supplied to the anode side of the battery cell, and air with a dew point of 80°C was supplied to the cathode side (relative humidity in the battery cell: 100% RH). The results are shown in Table 1 ("100% RH battery cell voltage" in Table 1).

[0256] <Power Generation Performance (2)>

[0257] The membrane electrode assembly obtained in the above example was assembled into a power generation cell, and hydrogen (utilization rate 70%) / air (utilization rate 50%) was supplied under normal pressure. The current density was measured at a cell temperature of 80°C at 1.0 A / cm 2The battery cell voltage (V) at the initial stage of operation under . It should be noted that hydrogen with a dew point of 53°C was supplied to the anode side of the battery cell, and air with a dew point of 53°C was supplied to the cathode side (relative humidity in the battery cell: 30% RH). The results are shown in Table 1 ("30% RH battery cell voltage" in Table 1).

[0258] [Table 1]

[0259]

[0260] From the results shown in Table 1, it can be seen that in Examples 1 to 4, the amount of catalyst used was reduced and the output of the fuel cell was increased as compared to Examples C1 to C3.

[0261] The disclosure of Japanese Patent Application No. 2019-232523 filed on December 24, 2019 is incorporated into this specification by reference in its entirety.

[0262] All documents, patent applications, and technical standards described in this specification are incorporated into this specification to the same extent as if each document, patent application, and technical standard was specifically and individually described and incorporated by reference.

[0263] Description of Reference Numerals

[0264] 10 membrane electrode assembly, 11 catalyst layer, 12 gas diffusion layer, 13 anode, 14 cathode, 21 catalyst layer, 22 gas diffusion layer.

Claims

1. A catalyst layer comprising: a catalyst-supported carbon having a catalyst containing platinum supported on a carbon carrier, and an ionomer, The catalyst-supported carbon has mesopores having a pore diameter of 2 nm or more and less than 10 nm in a pore distribution obtained by a nitrogen adsorption method, At least a part of the ionomer is present in the mesopores having a pore diameter of 2 nm or more and less than 10 nm. The content of the ionomer is 100 parts by mass or more relative to 100 parts by mass of the carbon support. The ionomer has an occupancy rate of 10 to 50% by volume in the total volume of the mesopores having a pore diameter of 2 nm or more and less than 10 nm.

2. The catalyst layer according to claim 1, wherein The catalyst-supported carbon in the catalyst layer has a thickness of 0.03 cm 3 / g catalyst or more macropores, wherein the pore diameter of the macropores in the pore distribution obtained by a nitrogen adsorption method is 50 nm or more.

3. The catalyst layer according to claim 1 or 2, wherein: The content of the catalyst in the catalyst layer per unit area is 0.2 mg / cm 2 the following.

4. The catalyst layer according to claim 1 or 2, wherein The catalyst includes at least one selected from the group consisting of platinum particles and platinum alloy particles.

5. The catalyst layer according to claim 4, wherein The number average particle size of the catalyst is 1 nm to 20 nm.

6. The catalyst layer according to claim 1 or 2, wherein The content of the catalyst with respect to the entire catalyst-supported carbon is 10% by mass to 70% by mass.

7. A membrane electrode assembly for a solid polymer fuel cell, comprising: an anode having a first gas diffusion layer and a first catalyst layer provided on one side of the first gas diffusion layer; a cathode having a second gas diffusion layer and a second catalyst layer provided on one side of the second gas diffusion layer; and a polymer electrolyte membrane disposed between the first catalyst layer and the second catalyst layer, At least one of the first catalyst layer and the second catalyst layer is the catalyst layer according to any one of claims 1 to 6. 8 . A polymer electrolyte fuel cell comprising the membrane electrode assembly for a polymer electrolyte fuel cell according to claim 7 .

Citation Information

Patent Citations

  • Catalyst and catalytic layer for fuel cell

    JP2010167379A

  • Catalyst layer for fuel cell

    JP2010186678A

  • Catalyst layer for fuel cell

    JP2011081977A

  • Electrolyte material for solid polymer fuel cell, electrolyte membrane and membrane-electrode assembly

    WO2007013533A1

  • Electrolyte material, liquid composition, and membrane electrode assembly for solid polymer fuel cells

    WO2011013577A1