Method for preparing super-hydrophobic polyolefin porous membrane by combining impregnation polymerization and stretching

By introducing fluorine-containing olefin monomers and initiators into the polyolefin dense membrane, performing heat treatment and graft polymerization, and combining stretching and heat setting, a polyolefin porous membrane with superhydrophobic properties was prepared, which solved the problem of polyolefin porous membranes. The problem of pore clogging after water contact improves the performance and applicability of the membrane.

CN114917772BActive Publication Date: 2024-10-11HENAN MINA PURIFICATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210513449.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-11
Publication Date
2024-10-11
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

After existing polyolefin porous membranes are in contact with water for a long time, the membrane surface and pores are easily infiltrated by water, resulting in clogging of the pores and reducing membrane performance. In addition, the existing hydrophobic modification methods have expensive equipment, easy damage to the pore structure, and reduced mechanical strength. etc. questions.

Method used

Using a technology that combines impregnation polymerization and stretching, fluorine-containing olefin monomers and initiators are introduced into the polyolefin dense film, and heat treatment and graft polymerization are performed to form a fluoropolymer-polyolefin interpenetrating network structure, and Stretching and heat setting were performed to prepare a polyolefin porous membrane with superhydrophobic properties.

Benefits of technology

It achieves good superhydrophobic properties on both the inner and outer surfaces of the membrane pores, and is suitable for membrane contactors, gas-water separation and other fields. It improves the performance and mechanical strength of the membrane, avoids the defect of grafts blocking the pore channels, and is suitable for large-scale preparation. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114917772B_ABST
    Figure CN114917772B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a super-hydrophobic polyolefin porous membrane by combining impregnation polymerization with stretching. The preparation method is achieved by combining impregnation polymerization with stretching, and the steps are: 1. impregnating a fluorine-containing olefin monomer and an initiator into the amorphous region of a dense membrane at low temperature; 2. initiating in-situ polymerization of the fluorine-containing olefin monomer in the dense membrane in 1 by heating, and forming an interpenetrating network structure in the amorphous region; 3. stretching the dense membrane in 2, so that the wafers are pulled apart, the amorphous region is microfibrillated to form micropores, and the fluorine-containing polymer on the surface of the microfiber makes the membrane hydrophobic; 4. heat-setting the microporous membrane in 3 to eliminate stress, and obtain a super-hydrophobic polyolefin porous membrane with a stable pore structure. The preparation method is suitable for large-scale preparation of flat microporous membranes; the prepared microporous membrane has good super-hydrophobic properties both in the membrane pores and on both surfaces of the membrane, and can be used in membrane contactors, gas-water separation and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of super-hydrophobic polyolefin porous film preparation, and specifically relates to a method for preparing a super-hydrophobic polyolefin porous film by combining impregnation polymerization with stretching. Background Art

[0002] Polyethylene and polypropylene are a kind of general polymer materials, which are non-toxic, odorless, transparent, diverse, low-priced, and stable in physical and chemical properties. Based on their melting and crystallization characteristics, they can be prepared into excellent filtration and separation membrane materials, which are widely used in the fields of petroleum, chemical industry, agriculture, industry, medicine, environmental protection, etc. Among them, the hydrophobic properties of polyethylene and polypropylene are used to make membranes for gas-liquid separation, membrane distillation, membrane contactors, etc. However, as general hydrophobic materials, after long-term contact with water, the membrane surface and the surrounding and pores of the membrane are still inevitably wetted by water, blocking the membrane pores, greatly reducing the performance of the membrane. In order to improve the performance of the membrane, the membrane material needs to be further hydrophobized. Generally, the hydrophobicity of the membrane material can be improved by changing the microscopic morphology of the material surface to increase the surface roughness and introducing low surface energy components (fluorine-containing and silicon-containing compounds) on the surface of the material.

[0003] Patents have provided many methods for preparing super-hydrophobic polyethylene and polypropylene surfaces by changing or constructing the microscopic morphology of the material surface. For example, Chinese patent CN101531764B provides "a super-hydrophobic polypropylene film and a preparation method thereof", which adds acetone of 20% to 60% of the volume of the polypropylene solution to a polypropylene solution, and utilizes the induction effect of acetone to cause the polypropylene solution to produce microphase separation to form an irregular structure, thereby obtaining a super-hydrophobic surface. The surface of the polypropylene film obtained is a network-like bird's nest structure of porous crystals, with a contact angle between 152° and 174°, and a water rolling angle of less than 4°; Chinese patent CN102850572B provides "a preparation method of a super-hydrophobic polypropylene film", which dissolves polypropylene in benzene, toluene or ethylbenzene, and then performs phase conversion in an environment with a certain humidity and ethanol vapor concentration, to prepare a super-hydrophobic polypropylene film with a honeycomb surface and a contact angle between 150° and 170°; There are many means to prepare super-hydrophobic materials by introducing low surface energy components on the surface of the material, such as initiating a graft polymerization reaction of monomers containing unsaturated double bonds on the surface of the material by high-energy electron beams, UV, plasma, γ-rays and other technologies. The low surface energy materials that have been studied and reported more are fluorinated monomers, among which the polymers grafted with perfluorocarbon side chains have the best performance. Since the F atom has an extremely low polarizability, and the fluorinated carbon side chains are oriented and crystallized outward, forming a shielding and protective effect on the main chain and internal molecules, only a small amount of such polymers is needed to give the material an extremely low surface energy, thereby achieving excellent hydrophobic properties. For example, Chinese patent CN102688704A provides "a method for preparing a polypropylene hollow fiber membrane with durable super-hydrophobic modification", which uses plasma and ultraviolet radiation to initiate monomer technology containing unsaturated double bonds to graft polymers containing fluorine and long-chain alkyl on the surface of the polypropylene hollow fiber membrane, and prepares a polypropylene hollow fiber membrane with durable super-hydrophobic properties. When the material surface is grafted and modified with the help of special equipment such as energy electron beams, UV, plasma, and γ-rays, there are problems such as expensive equipment, easy destruction of pore structure, decreased mechanical strength, and clogging of membrane pores by grafted materials. For example, Chinese patent CN102627799B provides "a super-hydrophobic low-density polyethylene film material and its preparation method", which mixes low-density polyethylene and nano zinc oxide particles to form a film, then dissolves the zinc oxide particles by acetic acid, and finally obtains a super-hydrophobic low-density polyethylene film. Chinese patent CN101157768B provides "a super-hydrophobic high-density polyethylene film preparation method", which dissolves high-density polyethylene in xylene at high temperature, adds ethanol, and then obtains a super-hydrophobic high-density polyethylene film by casting. The super-hydrophobic film materials prepared by the above two methods are all non-porous films without filtering and separation functions.

[0004] Different from the above reports, the present invention targets the problems and inapplicability of existing technologies for hydrophobic modification of polyolefin porous membranes, combines the heat treatment-stretching process in the preparation process of polyolefin membranes, uses solvents to impregnate initiators and hydrophobic monomers into the non-crystalline region of the dense membrane, and then performs heat treatment and grafting polymerization reaction, and finally performs stretching and heat setting processes to obtain a super-hydrophobic modified polyolefin membrane. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a super-hydrophobic polyolefin porous membrane. The preparation method is suitable for large-scale preparation of flat microporous membranes; the prepared microporous membrane has good super-hydrophobic properties inside the membrane pores and on both surfaces of the membrane, and can be used in the fields of membrane contactors, gas-water separation, etc.

[0006] The technical solution of the present invention is as follows:

[0007] The present invention first provides a method for preparing a super-hydrophobic polyolefin porous membrane, which comprises the following steps:

[0008] 1) The polyolefin dense film is swollen with a non-polar solvent at 20-40° C., and then fully contacted and immersed in a mixed solution consisting of the non-polar solvent, a fluorine-containing olefin monomer, and an initiator. Under the action of swelling, the fluorine-containing olefin monomer and the initiator are impregnated into the amorphous region of the polyolefin dense film;

[0009] 2) in the step 1), the dense polyolefin film impregnated with the fluorine-containing olefin monomer and the initiator is subjected to in-situ polymerization of the fluorine-containing olefin monomer at 60-100° C. to form a fluorine-containing polymer-polyolefin interpenetrating network structure in the amorphous region;

[0010] 3) The dense membrane obtained in step 2) is stretched so that the crystals are pulled apart, the amorphous regions are microfibrillated to form micropores, and the fluorine-containing polymer on the surface of the microfibrils makes the membrane hydrophobic;

[0011] 4) The membrane obtained in step 3) is subjected to heat setting to eliminate stress, thereby obtaining a super hydrophobic polyolefin porous membrane with a stable pore structure.

[0012] As a preferred embodiment of the present invention, the dense polyolefin film in step 1) refers to a nonporous polyethylene film or a nonporous polypropylene film after melt molding. Polyethylene and polypropylene are both crystalline thermoplastic resins, and the dense polyolefin film contains crystals and microcrystalline micro-regions.

[0013] As a preferred embodiment of the present invention, when the dense polyolefin film is a polyethylene film, the heat setting temperature in step 4) is 100-130°C; when the dense polyolefin film is a polypropylene film, the heat setting temperature in step 4) is 100-150°C.

[0014] As a preferred embodiment of the present invention, the non-polar solvent is one or more of cyclohexane, decahydronaphthalene, benzene, toluene and xylene.

[0015] As a preferred embodiment of the present invention, the initiator is a thermal initiator, and the thermal initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, tert-amyl peroxide 2-ethylhexanoate, diisopropylbenzene peroxide, and di-tert-butyl peroxide.

[0016] As a preferred embodiment of the present invention, the fluorine-containing olefin monomer has a structural formula as shown in Formula I or Formula II below:

[0017] C n F 2n+1 SO2N(CH3)CH2CH2OCOCH=CH2

[0018] Formula I

[0019] C m F 2m+1 CH2CH2OCOCH=CH2

[0020] Formula II

[0021] In the formula, n and m are integers greater than 1.

[0022] As a preferred embodiment of the present invention, in the mixed solution described in step 1), the mass percentage ranges of the non-polar solvent, the fluorinated olefin monomer, and the initiator are: 85-95: 2-10: 0.3-1.0 respectively.

[0023] As a preferred embodiment of the present invention, as a preferred embodiment of the present invention, the total stretching ratio (elongation compared to the unstretched polyolefin dense film) of step 3) is 20% to 400%, preferably 20% to 80%, that is, the length of the stretched film is 1.2-1.8 compared to the unstretched polyolefin dense film.

[0024] The present invention also provides a super-hydrophobic polyolefin porous membrane prepared by the above method, wherein the surface of the super-hydrophobic polyolefin porous membrane and the pores contain super-hydrophobic fluorine-containing groups, and the surface of the polyolefin porous membrane and the pores form a fluorine-containing polymer-polyolefin interpenetrating network structure.

[0025] As a preferred embodiment of the present invention, the pore size of the outer surface layer of the super hydrophobic polyolefin porous membrane is 0.01-2.0 μm, the pore size ratio of the inner surface layer to the outer surface layer is 2:1-10:1, and the porosity is 40-50%.

[0026] The present invention has the following advantages:

[0027] The present invention selects a dense polyolefin film to ensure that the initiator and the reaction monomer can be evenly diffused into the amorphous region at the interface of the film matrix, thereby improving the penetration efficiency, the grafting rate and the uniformity of the distribution.

[0028] The present invention fixes the initiator and the grafted monomer in the amorphous region at the membrane interface by impregnation and penetration, which can improve the subsequent initiation and grafting polymerization efficiency and better avoid the initiator from ineffectively initiating self-polymerization in the active monomer reaction solution. Since the reaction occurs in the amorphous region, the crystalline region is not destroyed, which ensures the mechanical strength of the membrane and the formation of micropores during subsequent stretching.

[0029] The present invention combines the preparation process of polypropylene and polyethylene membranes, and the subsequent heat treatment process can improve the preparation efficiency, achieving the purpose of one-step multi-effects, and bringing the following benefits: (1) it can promote the decomposition and reaction of residual initiators and monomers; (2) it can provide the heat energy required for membrane drying, which is more energy-saving; (3) during the heat treatment process, the fluorocarbon side chains can be enriched on the membrane surface and membrane pore wall, thereby improving the hydrophobicity of the membrane. Therefore, it is different from the previously reported method that requires additional heat energy required for the reaction and solvent-induced enrichment.

[0030] The subsequent stretching process of the present invention is also a process of forming membrane pores, which increases the porosity and pore size of the membrane, thereby effectively offsetting the blocking effect of the grafted polymer on the membrane pores, and is particularly suitable for the case of a high grafting rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the surface electron micrograph of the unmodified polypropylene film in Example 1;

[0032] Figure 2 This is a surface electron micrograph of the super-hydrophobic polypropylene film prepared after modification in Example 1;

[0033] Figure 3 is the water contact angle on the surface of the super-hydrophobic polypropylene film prepared in Example 1;

[0034] Figure 4 is the water contact angle on the surface of the super-hydrophobic polypropylene film prepared in Example 2;

[0035] Figure 5 It is a schematic diagram of the preparation process combining impregnation polymerization and stretching of the present invention. DETAILED DESCRIPTION

[0036] The present invention is described in detail below in conjunction with the embodiments and drawings, but this should not be understood as the scope of the subject matter involved in the present invention being limited to the following embodiments, and all technologies implemented based on the following contents belong to the scope of protection of the present invention.

[0037] like Figure 5The schematic diagram of the preparation process of the present invention combining impregnation polymerization and stretching is shown. The steps of the method of the present invention are as follows:

[0038] (1) swelling the polyolefin dense film with a non-polar solvent at 20-40° C., and then fully contacting and immersing the film in a mixed solution consisting of the non-polar solvent, a fluorine-containing olefin monomer, and an initiator, so that the fluorine-containing olefin monomer and the initiator are impregnated into the amorphous region of the polyolefin dense film under the swelling effect;

[0039] The dense polyolefin film refers to a nonporous polyethylene film or nonporous polypropylene film after melt molding, the impregnation time is 1 to 5 hours, the mass concentration of the initiator is 5 to 10%, and the mass concentration of the grafted monomer is 5 to 20%;

[0040] The solvent is one of cyclohexane, decahydronaphthalene, benzene, toluene, xylene and decahydronaphthalene. According to the solubility parameter principle of polymer and solvent, cyclohexane is preferred for polyethylene material, and benzene, toluene, xylene and decahydronaphthalene are preferred for polypropylene.

[0041] The initiator is a thermal initiator, including: azobisisobutyronitrile, benzoyl peroxide, tert-amyl peroxide 2-ethylhexanoate, diisopropylbenzene peroxide, and di-tert-butyl peroxide.

[0042] The fluoroester containing unsaturated double bonds is ethyl acrylate (N-methyl perfluorosulfonamide) C n F 2n+1 SO2N(CH3)CH2CH2OCOCH=CH2, perfluoroalkylethyl acrylate C m F 2m+1 CH2CH2OCOCH=CH2, wherein n and m are integers greater than 1.

[0043] In the mixed solution, the mass percentage ranges of the non-polar solvent, the fluorine-containing olefin monomer and the initiator are respectively: 85-95:2-10:0.3-1.0.

[0044] (2) heating the dense film impregnated with fluorine-containing olefin monomer and initiator in (1) to initiate in-situ polymerization of the fluorine-containing olefin monomer, thereby forming a fluorine-containing polymer-polyolefin interpenetrating network structure in the amorphous region and achieving growth of the crystalline region;

[0045] (3) stretching the dense film in (2) so that the crystals are pulled apart and the amorphous regions are microfibrillated to form micropores, and the fluorine-containing polymer on the surface of the microfibrils makes the film hydrophobic;

[0046] The total stretching ratio (elongation compared to the unstretched polyolefin dense film) of step 3) is 20% to 400%, preferably 20% to 80%, that is, the length of the stretched film is 1.2-1.8 compared to the unstretched polyolefin dense film.

[0047] (4) The microporous membrane of (3) is subjected to heat setting to eliminate stress, thereby obtaining a hydrophobic polyolefin porous membrane with a stable pore structure.

[0048] When the dense polyolefin film is a polyethylene film, the heat setting temperature is 100 to 130° C.; when the dense polyolefin film is a polypropylene film, the heat setting temperature is 100 to 150° C. The heat setting time is 12 to 36 hours.

[0049] The present invention is further illustrated by examples below. The specific steps of the examples are the same as the above-mentioned implementation steps, but the present invention is not limited by the examples.

[0050] Example 1

[0051] 1) Place 100 g of polyethylene film in 50°C benzene to swell for 2 hours, then place in a 10°C hot water bath containing 5 g of azobisisobutyronitrile and 10 g of C6F 13 SO2N(CH3)CH2CH2OCOCH=CH2 and 85g of benzene were soaked for 5 hours and then taken out;

[0052] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 80°C for 3 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 100%, the heat-setting temperature was 100°C, and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25°C to be 150°, which has super-hydrophobic characteristics. Figure 2 is an electron microscopic image of the surface of the super-hydrophobic polypropylene film prepared after modification in Example 1; compared with Figure 1 From the electron microscope image of the surface of the unmodified polypropylene film, it can be seen that the surface porosity of the superhydrophobic polypropylene film obtained in Example 1 is larger than that of the unmodified polypropylene film. Figure 3 Schematic diagram of the water contact angle on the surface of the super-hydrophobic polypropylene film prepared in Example 1.

[0053] Example 2

[0054] 1) Place 100 g of polyethylene film in cyclohexane at 50°C for swelling for 1 hour, then place in a 10°C cyclohexane containing 5 g of azobisisobutyronitrile and 10 g of C6F 13 SO2N(CH3)CH2CH2OCOCH=CH2 and 85g of cyclohexane were soaked for 5 hours and then taken out;

[0055] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 80°C for 4 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 100%, the heat-setting temperature was 110°C, and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25°C to be 151°, which has super-hydrophobic characteristics. Figure 4 is the water contact angle on the surface of the super hydrophobic polypropylene film prepared in Example 2.

[0056] Example 3

[0057] 1) Place 100 g of polyethylene film in 60°C cyclohexane for swelling for 2 hours, then place in 20°C cyclohexane containing 8 g of benzoyl peroxide and 15 g of C8F 17 SO2N(CH3)CH2CH2OCOCH=CH2 and 77g of cyclohexane were soaked for 5 hours and then taken out;

[0058] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 90°C for 5 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 400%, the heat setting temperature was 120°C, and the heat setting time was 24 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25°C to be 158°, which has super-hydrophobic characteristics.

[0059] Example 4

[0060] 1) Place 100 g of polypropylene film in 80°C xylene to swell for 2 hours, then place in a 30°C flask containing 10 g benzoyl peroxide, 20 g C8F 17 SO2N(CH3)CH2CH2OCOCH=CH2 and 70g of xylene were soaked for 4.5 hours and then taken out;

[0061] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 90° C. for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 400%, the heat-setting temperature was 120° C., and the heat-setting time was 36 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25° C. to be 160°, which has super-hydrophobic characteristics.

[0062] Example 5

[0063] 1) A polypropylene film with a mass of 100 g was placed in a decahydronaphthalene solvent at 80°C for swelling for 1 hour, and then taken out and placed in a 30°C solution containing 5 g of tert-amyl peroxy 2-ethylhexanoate, 5 g of C6F 13 Soak in CH2CH2OCOCH=CH2 and 90g of decahydronaphthalene solution for 3.5 hours and take it out;

[0064] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 120° C. for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 300%, the heat-setting temperature was 150° C., and the heat-setting time was 36 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25° C. to be 150°, which has super-hydrophobic characteristics.

[0065] Example 6

[0066] 1) A polyethylene film with a mass of 100 g was placed in 80°C decahydronaphthalene for swelling for 1.5 hours, and then placed in a 30°C solution containing 5 g of tert-amyl peroxy 2-ethylhexanoate, 5 g of C 10 F 21 Soak in CH2CH2OCOCH=CH2 and 90g of decahydronaphthalene for 4 hours and then take it out;

[0067] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 120°C for 12 hours, and then stretched and heat-set to obtain a highly hydrophobic polyethylene porous film, wherein the total stretching ratio was 300%, the heat setting temperature was 100°C, and the heat setting time was 36 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25°C to be 155°, which has super hydrophobic characteristics.

[0068] Example 7

[0069] 1) Place 100 g of polypropylene film in 70°C toluene to swell for 1.5 hours, then place in a 30°C toluene containing 8 g of di-tert-butyl peroxide, 15 g of C 10 F 21 Soak in CH2CH2OCOCH=CH2 and 77g of toluene for 3 hours and then take it out;

[0070] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 120° C. for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 200%, the heat-setting temperature was 130° C., and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25° C. to be 159°, which has super-hydrophobic characteristics.

[0071] Example 8

[0072] 1) Place 100 g of polypropylene film in 80°C xylene to swell for 0.5 hours, then place in a 30°C flask containing 8 g of di-tert-butyl peroxide, 15 g of C 12 F 25 Soak in CH2CH2OCOCH=CH2 and 77g of xylene for 2.5 hours and then take it out;

[0073] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 120° C. for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 300%, the heat-setting temperature was 130° C., and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25° C. to be 161°, which has super-hydrophobic characteristics.

[0074] Example 9

[0075] 1) Place 100 g of polyethylene film in xylene at 70°C for swelling for 2 hours, then place in a 30°C flask containing 8 g of diisopropylbenzene peroxide, 15 g of C 12 F 25 SO2N(CH3)CH2CH2OCOCH=CH2 and 77g of xylene were soaked for 3.5 hours and then taken out;

[0076] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 120° C. for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 400%, the heat-setting temperature was 130° C., and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25° C. to be 158°, which has super-hydrophobic characteristics.

[0077] Example 10

[0078] 1) Place 100 g of polyethylene film in cyclohexane at 50°C for swelling for 1.5 hours, then place in a 30°C cyclohexane containing 8 g of diisopropylbenzene peroxide, 15 g of C 12 F 25 SO2N(CH3)CH2CH2OCOCH=CH2 and 77g of cyclohexane were soaked for 3.5 hours and then taken out;

[0079] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 120° C. for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 300%, the heat-setting temperature was 100° C., and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25° C. to be 155°, which has super-hydrophobic characteristics.

[0080] Embodiment 11

[0081] 1) Place 100 g of polypropylene film in 80°C decahydronaphthalene to swell for 1 hour, then place in a 30°C flask containing 8 g of diisopropylbenzene peroxide, 16 g of C 10 F 21 SO2N(CH3)CH2CH2OCOCH=CH2 and 76g of decahydronaphthalene were soaked for 2.5 hours and then taken out;

[0082] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 90°C for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 400%, the heat-setting temperature was 120°C, and the heat-setting time was 36 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25°C to be 157°, which has super-hydrophobic characteristics.

[0083] Example 12

[0084] 1) Place 100 g of polyethylene film in 70°C cyclohexane to swell for 1 hour, then place in a 25°C cyclohexane containing 8 g of diisopropylbenzene peroxide, 10 g of C8F 17 Soak in CH2CH2OCOCH=CH2 and 85g of cyclohexane for 1 hour and take it out;

[0085] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 110° C. for 24 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 400%, the heat-setting temperature was 120° C., and the heat-setting time was 24 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25° C. to be 163°, which has super-hydrophobic characteristics.

[0086] Embodiment 13

[0087] 1) Place 100 g of polypropylene film in 75°C xylene to swell for 1.5 hours, then place in a 20°C flask containing 6 g of azobisisobutyronitrile, 10 g of C 12 F 25 SO2N(CH3)CH2CH2OCOCH=CH2 and 84g of xylene were soaked for 1.5 hours and then taken out;

[0088] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 90°C for 12 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 400%, the heat-setting temperature was 130°C, and the heat-setting time was 36 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25°C to be 163°, which has super-hydrophobic characteristics.

[0089] Embodiment 14

[0090] 1) Place 100 g of polyethylene film in 60°C benzene to swell for 2 hours, then place in a 30°C hot water bath containing 8 g of benzoyl peroxide and 15 g of C6F 13 Soak in CH2CH2OCOCH=CH2 and 77g of benzene for 2 hours and then take it out;

[0091] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 90°C for 20 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 80%, the heat setting temperature was 120°C, and the heat setting time was 18 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25°C to be 153°, which has super-hydrophobic characteristics.

[0092] Embodiment 15

[0093] 1) Place 100 g of polyethylene film in cyclohexane at 50°C to swell for 1 hour, then place in a 15°C cyclohexane containing 7 g of azobisisobutyronitrile and 14 g of C 10 F 21 Soak in CH2CH2OCOCH=CH2 and 79g of cyclohexane for 5 hours and then take it out;

[0094] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 90°C for 3 hours, and then stretched and heat-set to obtain a super-hydrophobic polyethylene porous film, wherein the total stretching ratio was 200%, the heat-setting temperature was 130°C, and the heat-setting time was 20 hours. The water contact angle of the surface of the hydrophobically modified polyethylene film was measured at 25°C to be 156°, which has super-hydrophobic characteristics.

[0095] Example 16

[0096] 1) Place 100 g of polypropylene film in 65°C benzene to swell for 1 hour, then place in a 25°C flask containing 5 g of di-tert-butyl peroxide, 20 g of C 12 F 25 Soak in CH2CH2OCOCH=CH2 and 75g of benzene for 5 hours and then take it out;

[0097] 2) The film impregnated with the initiator and the grafted monomer was reacted in a nitrogen atmosphere at 110° C. for 8 hours, and then stretched and heat-set to obtain a super-hydrophobic polypropylene porous film, wherein the total stretching ratio was 20%, the heat-setting temperature was 150° C., and the heat-setting time was 12 hours. The water contact angle of the surface of the hydrophobically modified polypropylene film was measured at 25° C. to be 162°, which has super-hydrophobic characteristics.

Claims

1. A method for preparing a super-hydrophobic polyolefin porous membrane by combining impregnation polymerization and stretching, characterized in that The steps include: 1) Swelling a polyolefin dense film with a non-polar solvent at 20-40° C., and then fully contacting and immersing the film in a mixed solution consisting of a non-polar solvent, a fluorine-containing olefin monomer, and an initiator, and impregnating the fluorine-containing olefin monomer and the initiator into the amorphous region of the polyolefin dense film under the action of swelling; the polyolefin dense film is a non-porous polyethylene film or a non-porous polypropylene film after melt molding; The structural formula of the fluorinated olefin monomer is shown in Formula I or Formula II below: C n F 2n+1 SO2N(CH3)CH2CH2OCOCH=CH2 Formula I C m F 2m+1 CH2CH2OCOCH=CH2 Formula II Wherein, n and m are integers greater than 1; 2) In the step 1), the dense polyolefin film is impregnated with a fluorine-containing olefin monomer and an initiator, and the fluorine-containing olefin monomer is in situ polymerized at 60-100° C. to form a fluorine-containing polymer-polyolefin interpenetrating network structure in the amorphous region; 3) The dense membrane obtained in step 2) is stretched so that the crystals are pulled apart, the amorphous regions are microfibrillated to form micropores, and the fluorine-containing polymer on the surface of the microfibrils makes the membrane hydrophobic; 4) The membrane obtained in step 3) is heat-set to eliminate stress, thereby obtaining a super-hydrophobic polyolefin porous membrane with a stable pore structure.

2. The method for preparing a super hydrophobic polyolefin porous membrane according to claim 1, wherein When the dense polyolefin film is a polyethylene film, the heat setting temperature in step 4) is 100-130°C; when the dense polyolefin film is a polypropylene film, the heat setting temperature in step 4) is 100-150°C.

3. The method for preparing a super hydrophobic polyolefin porous membrane according to claim 1, wherein The non-polar solvent is one or more of cyclohexane, decahydronaphthalene, benzene, toluene and xylene.

4. The method for preparing a super hydrophobic polyolefin porous membrane according to claim 1, wherein The initiator is a thermal initiator, and the thermal initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, tert-amyl peroxide 2-ethylhexanoate, diisopropylbenzene peroxide, and di-tert-butyl peroxide.

5. The method for preparing a super hydrophobic polyolefin porous membrane according to claim 1, wherein The total stretching ratio of step 3) is 20%-400%.

6. A super-hydrophobic polyolefin porous membrane prepared by the method according to any one of claims 1 to 5, characterized in that: The super-hydrophobic polyolefin porous membrane and the surface of the holes contain super-hydrophobic fluorine-containing groups, and the polyolefin porous membrane and the surface of the holes form a fluorine-containing polymer-polyolefin interpenetrating network structure.

7. A super hydrophobic polyolefin porous membrane as claimed in claim 6, characterized in that: The pore size of the outer surface layer of the super hydrophobic polyolefin porous membrane is 0.01-2.0 μm, the pore size ratio of the inner surface layer to the outer surface layer is 2:1-10:1, and the porosity is 40-50%.