A method for preparing a gas diffusion layer for a fuel cell

High-carbon slurry is prepared through mechanical mixing and high-speed stirring, combined with multi-stage heat roller pressing and high-temperature carbonization, and the problem of uneven thickness and pore distribution of fuel cell gas diffusion layer material is solved, significantly reducing contact resistance and improving fuel cell performance .

CN114927704BActive Publication Date: 2024-11-15SHANGHAI TANJI IND GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210520489.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-12
Publication Date
2024-11-15
Estimated Expiration
2042-05-12

AI Technical Summary

Technical Problem

The existing fuel cell gas diffusion layer materials have uneven thicknesses and unevenness, resulting in uneven slurry filling, which affects the performance of fuel cells, especially the uneven pores and thickness distribution and large contact resistance.

Method used

High-carbon slurries A, B and C were prepared by mechanical mixing and high-speed stirring, soaking and drying carbon fiber felts respectively, and undergoing multi-stage hot rolling and high-temperature carbonization, followed by soaking B and coating, and controlling the solid-liquid ratio and Dry temperature to ensure uniform material thickness and pore distribution.

Benefits of technology

The uniformity and flatness of the gas diffusion layer are achieved, the contact resistance is reduced, and the performance of the fuel cell is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114927704B_ABST
    Figure CN114927704B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a gas diffusion layer for a fuel cell, which belongs to the technical field of fuel cells and comprises the following steps: (1) slurrying A; (2) slurrying B; (3) slurrying C; (4) slurrying A; (5) hot rolling; (6) high temperature carbonization; (7) slurrying B; (8) coating. In the present invention, the solid components of slurry A are evenly distributed on the surface and inside of the carbon fiber felt by slurrying A, and then hot rolling is performed to make the material thickness evenly distributed, and then high temperature carbonization, slurrying B and coating are performed to make the pore distribution even, thereby reducing the contact resistance to ensure the performance of the fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a method for preparing a gas diffusion layer for a fuel cell. Background Art

[0002] The gas diffusion layer is a key material for preparing the membrane electrode of fuel cells. Therefore, the uniformity and flatness of the gas diffusion layer directly affect the performance of the fuel cell. The current gas diffusion layer material is limited by the uneven thickness and unevenness of the carbon fiber felt used in the production process, which makes it more uneven after the slurry is filled, making the pores and thickness distribution of the prepared gas diffusion layer uneven, and the contact resistance is large, thus affecting the performance of the fuel cell. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a gas diffusion layer for a fuel cell in view of the existing problems.

[0004] The present invention is achieved through the following technical solutions:

[0005] A method for preparing a gas diffusion layer for a fuel cell comprises the following steps:

[0006] (1) Pulping A:

[0007] The high carbon powder, surfactant, resin and stabilizer are mechanically mixed and transferred to a high-speed mixer, and water is added to stir and disperse to obtain a high carbon slurry A;

[0008] (2) Pulping B:

[0009] The hydrophobic agent and the stabilizer are mixed with water and then transferred to a high-speed mixer for dispersion to obtain slurry B;

[0010] (3) Pulping C:

[0011] The high carbon powder, surfactant and stabilizer are mechanically mixed and then transferred to a high-speed mixer, and water and a hydrophobic agent are added and stirred for dispersion to obtain a high carbon slurry C;

[0012] (4) Slurry A:

[0013] The carbon fiber felt is impregnated with high carbon slurry A and dried to obtain a reinforced carbon fiber felt;

[0014] (5) Hot roller pressing:

[0015] The reinforced carbon fiber felt is subjected to multi-stage controllable hot roller pressing to obtain a calendered reinforced carbon fiber felt;

[0016] (6) High temperature carbonization:

[0017] The calendered reinforced carbon fiber felt is carbonized in a high-temperature carbonization furnace to obtain calendered low-resistance carbon fiber paper;

[0018] (7) Slurry B:

[0019] The calendered low-resistance carbon fiber paper is impregnated with slurry B and dried to obtain calendered hydrophobic carbon fiber paper;

[0020] (8) Coating:

[0021] The high carbon slurry C is coated on one side of the calendered hydrophobic carbon fiber paper and subjected to multi-stage drying to obtain a gas diffusion layer.

[0022] Furthermore, the solid-liquid ratio of the high carbon slurry A described in step (1) is 1 / 4 to 1 / 10, the surfactant accounts for 20% to 30% of the solid content, the stabilizer accounts for 3% to 10% of the solid content, and the resin accounts for 20% to 50% of the solid content.

[0023] Furthermore, the solid-liquid ratio of the slurry B in step (2) is 1 / 10 to 1 / 99, and the hydrophobic agent accounts for 70% to 95% of the solid content.

[0024] Furthermore, the solid-liquid ratio in the high carbon slurry C described in step (3) is 1 / 4 to 1 / 10, the surfactant accounts for 10% to 20% of the solid content, the stabilizer accounts for 3% to 10% of the solid content, and the hydrophobic agent accounts for 20% to 50% of the solid content.

[0025] Furthermore, the drying temperature of the slurry A in step (4) is 70 to 120° C., and the drying time is 10 to 30 minutes.

[0026] Furthermore, the multi-stage controllable hot rolling in step (5) includes a controllable pressure range of 0.5 to 10 bar, a temperature of 250 to 400° C., and a gap of 0 to 250 um.

[0027] Furthermore, the high temperature carbonization in step (6) is carried out at a temperature of 1200 to 2200° C. and a carbonization time of 3 to 50 min.

[0028] Furthermore, the wet film thickness of the high carbon slurry C applied in step (8) is 100-400um, and the multi-stage drying is 40-70°C baking for 1-15min, 70-100°C baking for 1-15min, 100-250°C baking for 1-15min, and 250-400°C baking for 1-15min.

[0029] Furthermore, the high carbon powder is one or more of carbon black, acetylene black, activated carbon, graphite, carbon nanotubes, carbon nanowires, graphene oxide, graphene, and fullerene; the surfactant is Triton or a nonionic surfactant; the resin is one or more of acrylic resin, epoxy resin, phenolic resin, polyacrylamide, polyvinyl pyrrolidone, polyurethane, and polyvinyl alcohol; the stabilizer is one or more of polyethylene glycol, hydroxyethyl cellulose, hydroxypropyl cellulose, cellulose hydroxypropyl methyl ether, carboxymethyl cellulose, lignin, and xanthan gum; the hydrophobic agent is one or more of polytetrafluoroethylene, polyvinylidene fluoride, and fluorinated ethylene-propylene copolymer.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] The present application uses slurry A to evenly distribute the solid components of slurry A on the surface and inside of the carbon fiber felt, then performs hot rolling to evenly distribute the material thickness, and then performs high-temperature carbonization, slurry B and coating to evenly distribute the pores, thereby reducing the contact resistance to ensure the performance of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a flow chart of the preparation process of the gas diffusion layer for fuel cells in this application. DETAILED DESCRIPTION

[0033] In order to further explain the present invention, it is described below in conjunction with the accompanying drawings and specific embodiments.

[0034] Embodiment 1:

[0035] A method for preparing a gas diffusion layer for a fuel cell, wherein 25 g of graphite, 10 g of Triton, 20 g of epoxy resin and 5 g of polyethylene glycol are weighed, mechanically mixed and transferred to a high-speed mixer, 440 g of water is added, and stirred and dispersed uniformly to obtain a high-carbon slurry A;

[0036] Weigh 41 g of 60% polytetrafluoroethylene dispersion, 7 g of polyethylene glycol, mix with 452 g of water, and transfer to a high-speed mixer for dispersion to obtain slurry B;

[0037] Weigh 30 g of acetylene black, 7 g of polyoxyethylene ether and 10 g of polyethylene glycol, mix mechanically and transfer to a high-speed mixer, add 423 g of water and 30 g of a polytetrafluoroethylene dispersion having a mass fraction of 60% and stir to disperse, to obtain a high carbon slurry C;

[0038] The carbon fiber felt was impregnated with the high carbon slurry A and placed in a 90° C. blast oven for 20 min to obtain a reinforced carbon fiber felt;

[0039] The reinforced carbon fiber felt is subjected to multi-stage controllable hot rolling, and the rolling conditions should be set in advance, for example, the first-stage rolling pressure is 0.5 bar, the temperature is 300°C, and the gap is 160um; the second-stage rolling pressure is 0.8 bar, the temperature is 320°C, and the gap is 160um; the third-stage rolling pressure is 1 bar, the temperature is 340°C, and the gap is 150um; the fourth-stage rolling pressure is 2 bar, the temperature is 350°C, and the gap is 150um, to obtain a calendered reinforced carbon fiber felt;

[0040] The calendered reinforced carbon fiber felt is carbonized in a high temperature carbonization furnace, the carbonization temperature is set to 1800° C., the carbonization time is 15 min, and a calendered low-resistance carbon fiber paper is obtained;

[0041] The calendered low-resistance carbon fiber paper is impregnated with slurry B and dried at 90°C to obtain calendered hydrophobic carbon fiber paper;

[0042] High carbon slurry C was coated on one side of the calendered hydrophobic carbon fiber paper, and the wet film thickness was controlled to be 300um. After multi-stage drying, the first stage was dried at 50℃ for 10min, the second stage was dried at 80℃ for 10min, the third stage was dried at 150℃ for 10min, and the fourth stage was dried at 350℃ for 10min to obtain a gas diffusion layer.

[0043] Example 2

[0044] A method for preparing a gas diffusion layer for a fuel cell, wherein 40 g of graphite, 10 g of polyvinyl pyrrolidone, 20 g of epoxy resin and 5 g of polyethylene glycol are weighed, mechanically mixed and transferred to a high-speed mixer, 425 g of water is added, and stirred and dispersed uniformly to obtain a high-carbon slurry A;

[0045] Weigh 30 g of 50% by mass fluorinated ethylene-propylene copolymer dispersion, 5 g of polyethylene glycol, and 465 g of water, then transfer to a high-speed mixer for dispersion to obtain slurry B;

[0046] Weigh 35 g of acetylene black, 10 g of polyoxyethylene ether and 10 g of polyethylene glycol, mix mechanically and transfer to a high-speed mixer, add 410 g of water and 35 g of a 50% by mass fluorinated ethylene-propylene copolymer dispersion, stir and disperse to obtain a high carbon slurry C;

[0047] The carbon fiber felt was impregnated with the high carbon slurry A and placed in a 110° C. forced air oven for 15 min to obtain a reinforced carbon fiber felt;

[0048] The reinforced carbon fiber felt is subjected to multi-stage controllable hot rolling, and the rolling conditions should be set in advance, for example, the first-stage rolling pressure is 0.6 bar, the temperature is 250°C, and the gap is 170um; the second-stage rolling pressure is 0.9 bar, the temperature is 300°C, and the gap is 160um; the third-stage rolling pressure is 1.3 bar, the temperature is 315°C, and the gap is 150um; the fourth-stage rolling pressure is 2.3 bar, the temperature is 330°C, and the gap is 150um, to obtain a calendered reinforced carbon fiber felt;

[0049] The calendered reinforced carbon fiber felt is carbonized in a high temperature carbonization furnace, the carbonization temperature is set to 2100° C., the carbonization time is 15 min, and a calendered low-resistance carbon fiber paper is obtained;

[0050] The calendered low-resistance carbon fiber paper is impregnated with slurry B and dried at 110° C. to obtain calendered hydrophobic carbon fiber paper;

[0051] High carbon slurry C was coated on one side of the calendered hydrophobic carbon fiber paper, and the wet film thickness was controlled to be 300um. After multi-stage drying, the first stage was dried at 70℃ for 10min, the second stage was dried at 100℃ for 10min, the third stage was dried at 250℃ for 10min, and the fourth stage was dried at 330℃ for 10min to obtain a gas diffusion layer.

[0052] The present application uses slurry A to evenly distribute the solid components of slurry A on the surface and inside of the carbon fiber felt, then performs hot rolling to evenly distribute the material thickness, and then performs high-temperature carbonization, slurry B and coating to evenly distribute the pores, thereby reducing the contact resistance to ensure the performance of the fuel cell.

[0053] The specific embodiment described above is only one of the preferred embodiments of the present invention, and is not limited to the above specific implementation mode, and does not limit the scope of the claims of the present invention. All changes or modifications made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a gas diffusion layer for a fuel cell, characterized in that: The following steps are involved: (1) Pulping A: The high carbon powder, which is one or more of carbon black, acetylene black, activated carbon, graphite, carbon nanotubes, carbon nanowires, graphene oxide, graphene, and fullerene, as well as a surfactant, a resin, and a stabilizer are mechanically mixed and transferred to a high-speed mixer, and water is added to stir and disperse to obtain a high carbon slurry A; (2) Pulping B: The hydrophobic agent and the stabilizer are mixed with water and then transferred to a high-speed mixer for dispersion to obtain slurry B; (3) Pulping C: The high carbon powder, surfactant and stabilizer are mechanically mixed and then transferred to a high-speed mixer, and water and a hydrophobic agent are added and stirred for dispersion to obtain a high carbon slurry C; (4) Slurry A: The carbon fiber felt is impregnated with high carbon slurry A and dried to obtain a reinforced carbon fiber felt; (5) Hot roller pressing: The reinforced carbon fiber felt is subjected to multi-stage controllable hot roller pressing to obtain a calendered reinforced carbon fiber felt; (6) High temperature carbonization: The calendered reinforced carbon fiber felt is carbonized in a high-temperature carbonization furnace to obtain calendered low-resistance carbon fiber paper; (7) Slurry B: The calendered low-resistance carbon fiber paper is impregnated with slurry B and dried to obtain calendered hydrophobic carbon fiber paper; (8) Coating: The high carbon slurry C is coated on one side of the calendered hydrophobic carbon fiber paper and subjected to multi-stage drying to obtain a gas diffusion layer.

2. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: The solid-liquid ratio of the high carbon slurry A in step (1) is 1 / 4 to 1 / 10, the surfactant accounts for 20% to 30% of the solid content, and the The stabilizer accounts for 3% to 10% of the solid content, and the resin accounts for 20% to 50% of the solid content.

3. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: Step (2) The solid-liquid ratio in the slurry B is 1 / 10 to 1 / 99, and the hydrophobic agent accounts for 70% to 95% of the solid content.

4. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: In step (3) The solid-liquid ratio in the high carbon slurry C is 1 / 4 to 1 / 10, the surfactant accounts for 10% to 20% of the solid content, and the The stabilizer accounts for 3% to 10% of the solid content, and the hydrophobic agent accounts for 20% to 50% of the solid content.

5. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: Step (4) The drying temperature in the slurry A is 70-120° C. and the drying time is 10-30 minutes.

6. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: In step (5) The multi-stage controllable hot roller pressing includes a controllable pressure range of 0.5 to 10 bar, a temperature of 250 to 400° C., and a gap of 0 to 250 um.

7. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: Step (6) High temperature carbonization, the temperature is 1200-2200℃, and the carbonization time is 3-50min.

8. The method for preparing a gas diffusion layer for a fuel cell according to claim 1, characterized in that: In the coating step (8) The wet film thickness of the high carbon slurry C is 100-400um, and the multi-stage drying is 40-70℃ baking for 1-15min, 70- Bake at 100℃ for 1 to 15 min, bake at 100-250℃ for 1 to 15 min, bake at 250-400℃ for 1 to 15 min.