High temperature resistant B-stageable epoxy adhesive and products made therefrom

By using a specific proportion of epoxy resin and polyester in the epoxy adhesive and introducing a crosslinking agent containing aniridine group to form a crosslinking network, the heat resistance of existing epoxy adhesives is solved. and the problem of insufficient balance of adhesion strength achieves good performance at high temperatures.

CN114929827BActive Publication Date: 2024-11-293M CHINA

Patent Information

Application Number
CN201980103301.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-27
Publication Date
2024-11-29
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

The existing B-stage epoxy adhesives have insufficient balance in terms of heat resistance and adhesion strength, especially at high temperatures, which is difficult to meet the high performance needs of electrical devices and equipment for insulating materials.

Method used

Two different epoxy resins in a specific proportion, two polyesters and crosslinking agents containing 2 or more aziridine groups are used to form a crosslinking network to improve the heat resistance and adhesion strength of the adhesive , balance improvement.

Benefits of technology

The balance between good bonding strength and heat resistance at high temperatures is achieved, the overall performance of epoxy adhesive is improved, and it is suitable for insulation protection of electrical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003710510990000101
    Figure BDA0003710510990000101
  • Figure BDA0003710510990000102
    Figure BDA0003710510990000102
  • Figure BDA0003710510990000171
    Figure BDA0003710510990000171
Patent Text Reader

Abstract

The present disclosure relates to a B-stageable epoxy adhesive composition and articles made therefrom. The B-stageable epoxy adhesive composition comprises: (A) 20 wt% to 50 wt% of a first epoxy resin having an epoxide equivalent of 5000 g / eq or more; (B) 5 wt% to 20 wt% of a second epoxy resin having an epoxide equivalent of 800 g / eq or less and having 2 to 4 epoxy functional groups; (C) 5 wt% to 30 wt% of a carboxyl-terminated polyester; (D) 5 wt% to 15 wt% of a polyisocyanate-modified polyester; and (E) 0.1 wt% to 0.5 wt% of a crosslinker containing 2 or more aziridine groups, all percentages of which are based on the total weight of the B-stageable epoxy adhesive composition. The B-stageable epoxy adhesive composition and related products can be widely used as insulation protection for battery management, busbars, transformers and other markets, with a good balance between high bond strength and high temperature resistance and other properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to the field of adhesive applications. More specifically, the present disclosure relates to a high temperature resistant B-stageable epoxy adhesive and articles made therefrom. Background Art

[0002] With new market and industrial trends, electrical devices and equipment are becoming smaller, thinner, lighter and high-power density, better heat-resistant insulation materials with good thermal conductivity are becoming more and more important for insulation protection in the electrical market. Rubber-based PSA or acrylic PSA insulation tapes are a key type of insulation material for electrical devices and equipment. Generally speaking, the temperature rating of these materials is Class B or below, and thermal degradation of these known materials at higher temperatures will lead to loss of adhesion and other properties.

[0003] EP1275673 relates to epoxy resin compositions, cured products thereof, novel epoxy resins used therein, polyphenol compounds suitable for use as intermediates thereof, and methods for preparing the same. One of the purposes to be achieved by the present invention is to impart heat resistance, moisture resistance, dielectric properties, and flame retardant effects required for electrical or electronic materials (such as semiconductor packaging materials and varnishes for circuit boards) to epoxy resin compositions.

[0004] CN100336841C discloses epoxy resin roughening and curing agent. The epoxy resin roughening and curing agent is composed of 10% to 60% by weight of a dendritic polyamide-amine polymer, 10% to 70% by weight of a saturated fatty polyamine and 10% to 45% by weight of an aromatic polyamine, and is prepared by mixing a dendritic polyamide-amine polymer, a saturated fatty polyamine and an aromatic polyamine. The preparation process has low cost. Compared with epoxy resins with saturated fatty polyamines and aromatic polyamines, the epoxy resin with the epoxy resin roughening and curing agent has an impact toughness increased by 180%, and other important properties are maintained. In addition, the epoxy resin roughening and curing agent has a wide curing temperature range from room temperature to 120 degrees Celsius (℃) and an adjustable curing cycle, and therefore enables the epoxy resin to have a widened application range and an improved application value. A thermally conductive epoxy resin is produced by mixing 20 wt% of magnesium oxide frit powder as a filler with 80 wt% of a polymer material comprising an epoxy resin, a curing agent, a curing accelerator and a pigment. The magnesium oxide frit powder is obtained by calcining magnesite at 1700° C. to 1800° C. to produce periclase crystalline particles.

[0005] CN103897643 discloses a high heat-proof epoxy adhesive of room temperature curing, which comprises components A and B. Component A comprises the following components in parts by weight: 80 to 100 parts of epoxy resins, 0 to 3 parts of coupling agents, 0 to 30 parts of diluents, 0 to 20 parts of softeners, 80 to 120 parts of heat-proof fillers, 0 to 5 parts of nanofillers and 0 to 3 parts of thixotropic agents. Component B comprises the following components in parts by weight: 50 to 100 parts of curing agents, 0 to 3 parts of accelerators, 80 to 120 parts of heat-proof fillers, 0 to 5 parts of nanofillers and 0 to 3 parts of thixotropic agents. Epoxy adhesive meets the requirements of adhesive in adhesive shear strength and room temperature shear strength, and is good in toughness. Since raw materials are common products on the market, adhesive is simple and easy to obtain and has low cost.

[0006] CN1079922813A discloses a B-staged epoxy adhesive composition and a coating film prepared therefrom, and the composition imparts the coating film with very high adhesion, excellent high temperature resistance, chemical resistance and flame retardancy.

[0007] CN108026424A discloses a B-staged epoxy adhesive composition for use in areas where good bond strength, toughness, shelf life and aging properties as well as functional properties such as heat resistance and flame retardancy are required. However, the peel strength and heat resistance of this adhesive composition / film are still relatively low and therefore need to be further improved.

[0008] CN108291129A discloses a novel B-staged adhesive composition which can be achieved when epoxy resin, carboxyl terminated butadiene-acrylonitrile copolymer and polyfluorene modified phenolic resin are mixed in a specific ratio.

[0009] Therefore, there is a need to develop a novel B-stageable epoxy adhesive composition to provide a better bonding solution in the field requiring good functions in terms of heat resistance and adhesion strength. Summary of the invention

[0010] With the purpose of developing a B-stageable epoxy adhesive composition having good heat resistance, good adhesion strength, etc., especially a balance between these properties, in the present disclosure, a novel B-staged epoxy adhesive composition and articles made therefrom are developed.

[0011] In one aspect, the present disclosure provides a B-stageable epoxy adhesive composition, the B-stageable epoxy adhesive composition comprising: (A) 20 wt % to 50 wt % of a first epoxy resin having an epoxide equivalent weight of 5000 g / eq or more; (B) 5 wt % to 20 wt % of a second epoxy resin having an epoxide equivalent weight of 800 g / eq or less and having 2 to 4 epoxy functional groups; (C) 5 wt % to 30 wt % of a carboxyl-terminated polyester; (D) 5 wt % to 15 wt % of a polyisocyanate-modified polyester having a glass transition temperature Tg of -13°C to 30°C; and (E) 0.1 wt % to 0.5 wt % of a crosslinker containing 2 or more aziridine groups, wherein all content percentages are based on the total weight of the B-stageable epoxy adhesive composition.

[0012] In some preferred embodiments, the first epoxy resin has a weight average molecular weight Mw of 10,000 g / mol or greater.

[0013] In some preferred embodiments, the first epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, glycidyl ether epoxy resin, and combinations thereof.

[0014] In some preferred embodiments, the first epoxy resin is present in the B-stageable adhesive composition in an amount of 35 wt % to 45 wt %, based on the total weight of the B-stageable adhesive composition.

[0015] In some preferred embodiments, the second epoxy resin has a weight average molecular weight Mw of 200 to 2,000 g / mol.

[0016] In some preferred embodiments, the second epoxy resin is selected from the group consisting of polyurethane-modified bisphenol A epoxy resin, polyurethane-modified bisphenol F epoxy resin, polyurethane-modified novolac epoxy resin, polyurethane-modified trisphenol methane epoxy resin, polyurethane-modified glycidylamine epoxy resin, polyurethane-modified aminophenol epoxy resin, polyurethane-modified naphthalene epoxy resin, and combinations thereof.

[0017] In some preferred embodiments, the second epoxy resin is present in the B-stageable adhesive composition in an amount of 6 wt % to 10 wt %, based on the total weight of the B-stageable adhesive composition.

[0018] In some preferred embodiments, the carboxyl terminated polyester has an acid value of 20 mg KOH / g to 80 mg KOH / g.

[0019] In some preferred embodiments, the polyisocyanate-modified polyester has a weight average molecular weight Mw of 20,000 g / mol or greater.

[0020] In some preferred embodiments, the carboxyl-terminated polyester or polyisocyanate-modified polyester comprises dicarboxylic acid units and diol units, wherein the dicarboxylic acid units include one or more of succinic acid, adipic acid, cyclohexane dicarboxylic acid, suberic acid, phthalic acid, naphthylic acid (naphthalene dicarboxylic acid), trimellitic acid, or pyromellitic acid, and the diol units include one or more of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, decanediol, diethylene glycol, dipropylene glycol, dimethylolpropane, or dimethylolethane.

[0021] In some preferred embodiments, the carboxyl terminated polyester is selected from a carboxyl terminated phthalate polyester, a carboxyl terminated adipate polyester, or a combination thereof.

[0022] In some preferred embodiments, the polyisocyanate-modified polyester is a phthalate polyester, a polyisocyanate-modified adipate polyester, or a combination thereof, which is modified by a polyisocyanate selected from toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, or a combination thereof.

[0023] In some preferred embodiments, the polyisocyanate-modified polyester has a glass transition temperature Tg of -11°C to 16°C.

[0024] In some preferred embodiments, the crosslinking agent is 1,1′-isophthaloylbis(2-methylaziridine), trimethylolpropane tris(2-methyl-1-aziridine propionate), 2-((3-aziridine-1-ylpropionyl)methyl)-2-ethylpropane-1,3-diylbis(aziridine-1-propionate), or a combination thereof.

[0025] In some preferred embodiments, the B-stageable adhesive composition further comprises a solvent. Preferably, the solvent is selected from N,N-dimethylformamide, methyl ethyl ketone (MEK), hexane, heptane, cyclohexane, toluene, xylene, or a combination thereof. Preferably, the solvent is present in the B-stageable adhesive composition in an amount of 30 wt % to 70 wt % based on the total weight of the B-stageable adhesive composition.

[0026] In some preferred embodiments, the B-stageable adhesive composition further comprises a toughening agent, a flame retardant, or a combination thereof.

[0027] In some preferred embodiments, the toughening agent is present in the B-stageable adhesive composition in an amount of 0.5 wt % to 2.0 wt %, based on the total weight of the B-stageable adhesive composition.

[0028] In some preferred embodiments, the flame retardant is present in the B-stageable adhesive composition in an amount of 1.0 wt % to 30.0 wt %, based on the total weight of the B-stageable adhesive composition.

[0029] In another aspect, the present disclosure provides an article including a substrate and a coating formed of the above-mentioned adhesive composition on a surface of the substrate.

[0030] In some preferred embodiments, the article is in the form of a plate, sheet, belt, roll, film, or tube.

[0031] In the present disclosure, by specifically selecting two different epoxy resins, two different polyesters and using a specific crosslinking agent in a specific weight ratio, a B-stageable epoxy adhesive composition having good heat resistance, good adhesion strength, etc., and especially a balance between these properties, and articles made therefrom are obtained.

[0032] In addition, the crosslinking agent containing 2 or more aziridine groups in the B-stageable epoxy adhesive composition of the present disclosure, such as 1,1′-phthaloylbis(2-methylaziridine), can react with the carboxyl groups in the epoxy resin and the polyester to form a crosslinked network in the B-stageable epoxy adhesive composition, which can significantly improve both its heat resistance and adhesion strength.

[0033] Furthermore, the B-stageable epoxy adhesive compositions and related products of the present disclosure can be widely used as insulation protection in battery management, busbars, transformers, and other markets, with a good balance between high bond strength and high temperature resistance, as well as other properties such as chemical resistance. DETAILED DESCRIPTION

[0034] The present inventors have conducted intensive and extensive research to develop a novel B-stageable epoxy adhesive composition having a good balance between high adhesive strength and high heat resistance or high temperature resistance. The present inventors surprisingly found that when two different epoxy resins, two different polyesters and a specific crosslinking agent containing 2 or more aziridine groups (such as 1,1′-isophthaloylbis(2-methylaziridine)) are mixed in a specific weight ratio, a B-stageable epoxy adhesive composition having good heat resistance, good adhesive strength, etc., and especially a balance between these properties can be achieved.

[0035] One aspect of the present disclosure provides a B-stageable epoxy adhesive composition, which includes: (A) 20 wt % to 50 wt % of a first epoxy resin, the first epoxy resin having an epoxide equivalent weight of 5000 g / eq or more; (B) 5 wt % to 20 wt % of a second epoxy resin, the second epoxy resin having an epoxide equivalent weight of 800 g / eq or less and having 2 to 4 epoxy functional groups; (C) 5 wt % to 30 wt % of a carboxyl-terminated polyester; (D) 5 wt % to 15 wt % of a polyisocyanate-modified polyester; and (E) 0.1 wt % to 0.5 wt % of a crosslinker containing 2 or more aziridine groups, wherein all percentages are based on the total weight of the B-stageable epoxy adhesive composition.

[0036] As used herein, the term "B-stageable epoxy adhesive composition" has the conventional meaning, i.e., an epoxy resin-based adhesive composition that can be subjected to a B-staging process as known to those skilled in the art, unless otherwise specified. B-staging is the process of using heat to remove a large portion of the solvent from the adhesive composition to allow for "staging" of the construction. Between the processes of coating, assembling, and curing the adhesive composition, the adhesive composition can be maintained for a period of time without sacrificing its relevant properties.

[0037] The components used in the B-stageable epoxy adhesive composition according to the present disclosure will be described in detail below.

[0038] (A) First Epoxy Resin

[0039] In the present disclosure, a first epoxy resin having a higher epoxide equivalent weight is contained in the adhesive composition. In the present disclosure, the first epoxy resin has an epoxide equivalent weight of 5000 g / eq or more, preferably 5000 g / eq to 10000 g / eq.

[0040] The first epoxy resin is present in the B-stageable adhesive composition in an amount of 20 wt % to 50 wt %, preferably 35 wt % to 45 wt %, based on the total weight of the B-stageable epoxy adhesive composition.

[0041] In the present disclosure, preferably, the first epoxy resin may have a weight average molecular weight Mw of 10,000 g / mol or more, advantageously 12,000 g / mol or more, advantageously 15,000 g / mol or more, advantageously 20,000 g / mol or more, and advantageously 25,000 g / mol or more. As the present inventors have found, if the weight average molecular weight Mw is less than 10,000 g / mol, it may reduce the peel strength of the adhesive composition at room temperature.

[0042] In the present disclosure, the specific type of the first epoxy resin to be used in the present invention is not particularly limited, as long as it meets the relevant requirements. Preferably, the first epoxy resin can be selected from the group consisting of the following items: bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, glycidyl ether epoxy resin, and combinations thereof. Such epoxy resins are commercially available, and a specific example of the first epoxy resin is 40AXM40 (trade name) from Shandong Shengquan New Materials Chemical Co., Ltd., which is a bisphenol A epoxy resin having an epoxide equivalent of 5000 g / eq to 10000 g / eq (with a weight average molecular weight of about 38,000 g / mol) and in the form of a solution having a solid content of 40% by weight.

[0043] As the present inventors have found, when the first epoxy resin is used in the above amount range, the B-stageable adhesive composition has good tack, and its cured product has a good balance of adhesive strength and heat resistance.

[0044] (B) Second epoxy resin

[0045] In the present disclosure, a second epoxy resin having a lower epoxide equivalent weight is contained in the adhesive composition. In the present disclosure, the second epoxy resin is a multifunctional epoxy resin having an epoxide equivalent weight of 800 g / eq or less, advantageously 100 g / eq to 700 g / eq, and advantageously 100 g / eq to 500 g / eq, such as about 180 g / eq, and having 2 to 4, such as 2.5, 3.3 or 4 epoxy functional groups.

[0046] The second epoxy resin is present in the B-stageable adhesive composition in an amount of 5 wt % to 20 wt %, preferably 6 wt % to 10 wt %, based on the total weight of the B-stageable epoxy adhesive composition.

[0047] In the present disclosure, preferably, the second epoxy resin may have a weight average molecular weight Mw of 200 to 2,000 g / mol, advantageously 250 to 1,500 g / mol, advantageously 250 to 1,200 g / mol, and advantageously 300 to 1,000 g / mol.

[0048] In the present disclosure, the specific type of the second epoxy resin to be used in the present invention is not particularly limited, as long as it meets the relevant requirements. Preferably, the second epoxy resin can be selected from modified epoxy resins, such as polyurethane (PU) modified epoxy resins. Preferably, the second epoxy resin is selected from the group consisting of the following items: polyurethane-modified bisphenol A epoxy resin, polyurethane-modified bisphenol F epoxy resin, polyurethane-modified novolac epoxy resin, polyurethane-modified trisphenol methane epoxy resin, polyurethane-modified glycidylamine epoxy resin, polyurethane-modified aminophenol epoxy resin, polyurethane-modified naphthalene epoxy resin, and combinations thereof. Such second epoxy resins can be commercially available, and specific examples thereof are EPN1179 (trade name) and EPN1183 (trade name) from Huntsman International LLC.; and NPPN638S (trade name) from Nanya Epoxy Co., Ltd.

[0049] As discovered by the present inventors, when the second epoxy resin having the above epoxide equivalent weight and 2 to 4 epoxy functional groups is used within the above amount range, the B-stageable adhesive composition has good adhesion, and the coating formed from the adhesive composition can be effectively cured with good adhesion strength and high heat resistance.

[0050] The combination of components (A) and (B) is also referred to as a two-component epoxy resin system according to the present disclosure. According to certain embodiments, the adhesive composition of the present invention preferably comprises a combination of a bisphenol epoxy resin having a higher epoxide equivalent and a lower weight average molecular weight and a polyurethane-modified bisphenol epoxy resin having a lower epoxide equivalent and a lower weight average molecular weight as a two-component epoxy resin system. If the content of the first epoxy resin and the content of the second epoxy resin are both within the above range, a better balance of adhesion strength and heat resistance can be provided.

[0051] (C) Carboxyl-terminated polyester and (D) polyisocyanate-modified polyester

[0052] In the present disclosure, carboxyl terminated polyesters and polyisocyanate modified (hydroxyl terminated) polyesters are contained in the adhesive composition of the present disclosure. Without wishing to be bound by a particular theory, it is believed that such carboxyl terminated polyesters and polyisocyanate modified polyesters act as toughening agents to further balance the adhesion strength and heat resistance of the coating obtained by the adhesive composition after curing. Such toughening agents have functional groups that can react with the above-mentioned epoxy resin and the crosslinking agent described below under curing reaction conditions, particularly at high temperatures, so as to improve the adhesion strength and heat resistance of the coating formed by curing.

[0053] The carboxyl terminated polyester is present in the B-stageable adhesive composition in an amount of 5 wt % to 30 wt % and the polyisocyanate modified polyester is present in the B-stageable adhesive composition in an amount of 5 wt % to 15 wt % based on the total weight of the B-stageable epoxy adhesive composition.

[0054] In the present disclosure, preferably, the carboxyl terminated polyester has an acid value of 20 to 80 mg KOH / g, advantageously 20 to 60 mg KOH / g, advantageously 20 to 50 mg KOH / g, and advantageously 29 to 35 mg KOH / g.

[0055] In the present disclosure, preferably, the polyisocyanate-modified polyester has a weight average molecular weight Mw of 20,000 g / mol or more, advantageously 25,000 g / mol or more, advantageously 30,000 g / mol or more, and advantageously 35,000 g / mol or more.

[0056] In the present disclosure, preferably, the carboxyl-terminated polyester or polyisocyanate-modified polyester comprises dicarboxylic acid units and diol units, wherein the dicarboxylic acid units include one or more of succinic acid, adipic acid, cyclohexane dicarboxylic acid, suberic acid, phthalic acid, naphthoic acid, trimellitic acid or pyromellitic acid, and the diol units include one or more of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, decanediol, diethylene glycol, dipropylene glycol, dimethylolpropane or dimethylolethane.

[0057] In the present disclosure, preferably, the carboxyl-terminated polyester is selected from a carboxyl-terminated phthalate polyester, a carboxyl-terminated adipate polyester, or a combination thereof. Such carboxyl-terminated polyesters are commercially available, and a specific example thereof is SJ4866 (trade name) obtained from Anhui Shenjian New Materials Co., Ltd.

[0058] In the present disclosure, the polyisocyanate-modified polyester has a glass transition temperature Tg of -13°C to 30°C, preferably -11°C to 16°C.

[0059] In the present disclosure, preferably, the polyisocyanate-modified polyester is a phthalate polyester, a polyisocyanate-modified adipate polyester, or a combination thereof, which is modified by a polyisocyanate selected from toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, or a combination thereof. Such polyisocyanate-modified polyesters can be obtained, for example, by modifying V3300, V3650, and V1801 (trade names) obtained from Bostik Inc. with a polyisocyanate before use.

[0060] As the present inventors have found, when the carboxyl-terminated polyester and the polyisocyanate-modified polyester are used within the above-mentioned amount range, an improvement in toughness can be achieved and a balance between toughness and adhesive strength will be established.

[0061] (E) Cross-linking agent

[0062] In the present disclosure, a crosslinking agent containing 2 or more, for example, 2 or 3 aziridine groups is included in the adhesive composition of the present disclosure.

[0063] The crosslinker is present in the B-stageable adhesive composition in an amount of 0.1 wt % to 0.5 wt %, based on the total weight of the B-stageable epoxy adhesive composition.

[0064] In the present disclosure, preferably, the cross-linking agent containing 2 or more aziridine groups may be 1,1′-isophthaloylbis(2-methylaziridine), trimethylolpropane tris(2-methyl-1-aziridine propionate), 2-((3-aziridine-1-ylpropionyl)methyl)-2-ethylpropane-1,3-diylbis(aziridine-1-propionate), or a combination thereof. Such cross-linking agents are commercially available, and specific examples thereof are HX-752 (trade name) from Shenzhen Hongyuan Chemical New Material Technology Ltd. and Sac-100 (trade name) from Shanghai UN Chemical Co., Ltd.

[0065] Typically, 1,1′-isophthaloylbis(2-methylaziridine) or other aziridine crosslinking agents are commonly used in acrylic pressure-sensitive adhesive (PSA) systems, and the main function is to form a linear crosslinking structure of the linear polymer of the acrylic polymer in the pressure-sensitive adhesive system, thereby providing cohesive strength of the polymer molecules, making it usable as a pressure-sensitive adhesive, and in theory, it also has a specific effect of improving heat resistance, but this is not its fundamental purpose;

[0066] Typically, the crosslinking agent of a general epoxy resin system is a crosslinking agent that can directly react with epoxy groups (such as amines or anhydrides). The crosslinking agent used in the present disclosure does not directly react with epoxy groups, so epoxy adhesives generally do not use such crosslinking agents;

[0067] The inventors were surprised to find that a crosslinking agent containing 2 or more aziridine groups can improve the heat resistance of the B-stageable epoxy adhesive composition disclosed herein. The improvement in heat resistance can be explained from two aspects. On the one hand, it is the use of a crosslinking agent in an epoxy adhesive. This crosslinking agent acts as a bridge in the original glue reaction system, which adds a reaction connection point to obtain a larger crosslinking system, reduces the ability of molecular movement, and thus improves heat resistance. On the other hand, it is a specific modified polyester used as the above-mentioned toughening agent. Such modified polyester resins are used as toughening agents. The multifunctional isocyanate is treated for a period of time, so that its addition ratio is greatly reduced (5% to 15%), and a good toughening effect is ensured without significantly affecting the heat resistance of the glue.

[0068] Table 1 below shows the chemical structures of some typical aziridine cross-linking agents.

[0069] Table 1

[0070]

[0071] Without being bound by a particular theory, the estimated reaction mechanism between aziridine and carboxyl group is shown below.

[0072] On the one hand, such a crosslinking agent reacts with a carboxyl terminated polyester resin in a B-stageable epoxy adhesive composition to increase the crosslink density, which will contribute to significantly improving heat resistance.

[0073]

[0074] On the other hand, polyisocyanate-modified polyester resins are also innovative for B-stageable epoxy adhesive compositions. Typically, epoxy-based adhesives are difficult to coat on PET films, and polyester resins with low Tg can be used as tougheners to increase adhesion to film backings. However, the addition rate of polyester tougheners will be high, typically 30% by weight, and even more. It will reduce heat resistance and the Tg of the adhesive system, which will be inconvenient in applications where initial viscosity is not required or low initial viscosity is required. By using polyisocyanate-modified polyesters, the addition rate can be reduced to 5% to 15% by weight, and this will reduce the impact on adhesive Tg and heat resistance. And in addition, compared with conventional polyester resins, the adhesion to PET film is significantly improved.

[0075] By incorporating isocyanate-modified polyesters and multifunctional aziridine crosslinkers into epoxy-based adhesive compositions, a well-balanced system is created that exhibits good heat resistance and bond strength at room temperature, and in particular, has much higher heat resistance than existing solutions.

[0076] In particular, a crosslinking agent such as 1,1′-isophthaloylbis(2-methylaziridine) is added to the adhesive composition, and upon thermal activation, the epoxy groups of the epoxy resin and the carboxyl groups of the polyester will react with the crosslinking agent and thereby form a crosslinked network, which will help to significantly improve the heat resistance performance of the cured coating.

[0077] Other optional components

[0078] In addition to the above components, the B-stageable adhesive composition of the present disclosure may include one or more of the following components: such as solvents, toughening agents, flame retardants, antioxidants, defoamers, pigments, fillers, surfactants, and the like.

[0079] According to certain preferred embodiments, the adhesive composition may contain a solvent to dissolve related components, such as epoxy resins, polyesters, crosslinking agents and other components. In the present disclosure, the solvent may be selected from the group consisting of the following items: N, N-dimethylformamide, methyl ethyl ketone (MEK), hexane, heptane, cyclohexane, toluene, xylene or a combination thereof. Such solvents are commercially available, and a specific example thereof is MEK (trade name) obtained from Shanghai Xiangshun Fine Chemical Co., Ltd. In the present disclosure, preferably, based on the total weight of the B-stage adhesive composition, the solvent is present in the B-stage adhesive composition in an amount of 30% by weight to 70% by weight.

[0080] According to certain preferred embodiments, a toughening agent may be included in the adhesive composition to impart more toughness to the cured product. Such toughening agents are known in the art and are commercially available, such as Fortegra 100 (trade name) from Dow Chemical Company.

[0081] In the present disclosure, if necessary, a flame retardant may be contained in the adhesive composition to impart excellent fire resistance to the product obtained by the adhesive composition. Taking environmental issues into consideration, preferably, the flame retardant is a halogen-free flame retardant. The flame retardant that can be used in the present disclosure can be selected from organic flame retardants and inorganic flame retardants, such as aluminum hydroxide, magnesium hydroxide, MgO, ZnO, organic phosphorus salts, phosphates, phosphorus-containing polymers, nitrogen-containing polymers, or combinations thereof. According to certain embodiments, the content of the flame retardant is 1.0 wt % to 30.0 wt %, based on the total weight of the adhesive composition.

[0082] In the present disclosure, if necessary, an antioxidant may be contained in the adhesive composition to provide the advantage of better aging performance. According to certain embodiments, the antioxidant may be selected from the group consisting of: tea polyphenols, vitamin E, flavonoids, butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone. According to certain embodiments, based on the total weight of the adhesive composition, the content of the antioxidant is 0.1 wt % to 5 wt %.

[0083] In the present disclosure, if necessary, defoamer may be contained in the adhesive composition to provide the advantage of a good coating surface. According to certain embodiments, the defoamer may be selected from the group consisting of insoluble oil, polydimethylsiloxane and other organosilicones, certain alcohols, stearates, glycols or their combination. According to certain embodiments, based on the gross weight of the adhesive composition, the content of the defoamer is 0.01 wt % to 1 wt %.

[0084] In the present disclosure, if necessary, a pigment may be contained in the adhesive composition to provide the advantage of coating color. According to certain embodiments, the pigment may be selected from the group consisting of carbon black, ivory black, cadmium pigment, chromium, cobalt pigment, copper, iron oxide, lead pigment, manganese pigment, mercury pigment, titanium pigment, zinc pigment. According to certain embodiments, the content of the pigment is 0.1 wt % to 30 wt % based on the total weight of the adhesive composition.

[0085] In the present disclosure, fillers may be contained in the adhesive composition, if necessary, to change or improve the properties of the adhesive composition, wherein the fillers may be selected from: conductive fillers, such as carbon black, nickel powder, copper powder, gold powder, silver powder; thermal conductive fillers, such as boron nitride (BN), aluminum hydride (ATH); or other fillers, such as CaCO3, SiO2, clay, chalk, glass fiber, etc. According to certain embodiments, the content of the filler is 0.1 wt% to 30 wt% based on the total weight of the adhesive composition.

[0086] In the present disclosure, if necessary, a surfactant may also be contained in the adhesive composition to provide the advantage of a good coating surface. According to certain embodiments, the surfactant may be selected from the group consisting of sulfates, sulfonates, phosphates, ammonium lauryl sulfate, sodium lauryl sulfate (SDS, sodium dodecyl sulfate) and related alkyl ether sulfates sodium lauryl polyoxyethylene ether sulfate, also known as sodium lauryl ether sulfate (SLES), sodium myristyl alcohol polyether sulfate, etc. According to certain embodiments, the content of the surfactant is 0.01% by weight to 5% by weight based on the total weight of the adhesive composition.

[0087] For example, when one or more of these components are present in the adhesive in suitable ratios, a coating formed from the B-stageable adhesive composition of the present disclosure can be imparted with very high adhesion to substrates such as copper plates at high temperatures (>0.7 N / mm at 105° C.), together with good flame retardancy and other properties.

[0088] In the present disclosure, there is no limitation on the method for preparing a B-stageable adhesive composition. According to certain embodiments, the method for preparing a B-stageable adhesive composition includes a step of uniformly mixing all components thereof. According to certain embodiments, the temperature of the mixing step may be 5° C. to 60° C., and the pressure of the mixing step may be 0.5 atm to 2 atm.

[0089] In the present disclosure, the above components can be mixed with a solvent to form a single-component package. And, the obtained adhesive composition can be applied to the surface of a device such as an electronic device by a known coating method, and then cured to provide effective adhesion. Alternatively, the adhesive composition can be applied to the surface of a substrate such as a plate, a film, a plate, a belt, and then dried to provide a B-staged product, such as an adhesive tape. The B-staged product can be stored in the form of a package or a roll under normal conditions. When applied, the B-staged product can be applied to the device and further cured at a relatively high temperature and optional pressure to provide a fully cured product with heat resistance and flame retardancy.

[0090] Therefore, the present disclosure also relates to an article comprising a coating formed by the adhesive composition after curing. Preferably, such an article may be in the form of a plate, a plate, a belt, a roller, a film or a tube. According to certain embodiments, the article may have the following structure: a coating obtained by the adhesive composition of the present disclosure disposed on a liner; a coating obtained by the adhesive composition of the present disclosure disposed between the liner and the backing; a first coating obtained by the adhesive composition of the present disclosure disposed on the liner, and then a backing disposed in sequence and a second coating obtained by the adhesive composition of the present disclosure; and a backing interposed between the first coating and the second coating.

[0091] According to certain embodiments, the article of the present disclosure may be manufactured by mixing the components of the adhesive composition to obtain a mixture; and applying the mixture to a substrate, and then drying the coated substrate. According to certain embodiments, the substrate may be a PET film. According to certain embodiments, the coated substrate may be dried at a temperature of 120° C. or less for a period of time that allows the article to be formed, such as several minutes to several hours. According to certain embodiments, the coating may be applied to the surface of the substrate at a temperature below 25° C. and below atmospheric pressure.

[0092] The present disclosure also relates to the use of the adhesive composition or article according to the present disclosure in insulation applications for electrical devices including batteries, current collectors, PCBs, bus bars, transformers, and the like.

[0093] Implementation plan list

[0094] Embodiment 1 provides a B-stageable epoxy adhesive composition, the B-stageable epoxy adhesive composition comprising: (A) 20 wt % to 50 wt % of a first epoxy resin, the first epoxy resin having an epoxide equivalent weight of 5000 g / eq or more; (B) 5 wt % to 20 wt % of a second epoxy resin, the second epoxy resin having an epoxide equivalent weight of 800 g / eq or less and having 2 to 4 epoxy functional groups; (C) 5 wt % to 30 wt % of a carboxyl-terminated polyester; (D) 5 wt % to 15 wt % of a polyisocyanate-modified polyester, the polyisocyanate-modified polyester having a glass transition temperature Tg of -13°C to 30°C; (E) 0.1 wt % to 0.5 wt % of a crosslinker containing 2 or more aziridine groups, wherein all content percentages are based on the total weight of the B-stageable epoxy adhesive composition.

[0095] Embodiment 2 provides the B-stageable adhesive composition according to embodiment 1, wherein the first epoxy resin has a weight average molecular weight Mw of 10,000 g / mol or greater.

[0096] Embodiment 3 provides a B-stageable adhesive composition according to embodiment 1 or 2, wherein the first epoxy resin is selected from the group consisting of: bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, glycidyl ether epoxy resin, and combinations thereof.

[0097] Embodiment 4 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 3, wherein the first epoxy resin is present in the B-stageable adhesive composition in an amount of 35 wt % to 45 wt % based on the total weight of the B-stageable adhesive composition.

[0098] Embodiment 5 provides the B-stageable adhesive composition of any one of Embodiments 1 to 4, wherein the second epoxy resin has a weight average molecular weight Mw of 200 g / mol to 2,000 g / mol.

[0099] Embodiment 6 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 5, wherein the second epoxy resin is selected from the group consisting of: polyurethane-modified bisphenol A epoxy resin, polyurethane-modified bisphenol F epoxy resin, polyurethane-modified novolac epoxy resin, polyurethane-modified trisphenol methane epoxy resin, polyurethane-modified glycidylamine epoxy resin, polyurethane-modified aminophenol epoxy resin, polyurethane-modified naphthalene epoxy resin, and combinations thereof.

[0100] Embodiment 7 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 6, wherein the second epoxy resin is present in the B-stageable adhesive composition in an amount of 6 wt % to 10 wt % based on the total weight of the B-stageable adhesive composition.

[0101] Embodiment 8 provides the B-stageable adhesive composition of any one of Embodiments 1 to 7, wherein the carboxyl terminated polyester has an acid value of 20 mg KOH / g to 80 mg KOH / g.

[0102] Embodiment 9 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 8, wherein the carboxyl-terminated polyester or the polyisocyanate-modified polyester comprises dicarboxylic acid units and diol units, wherein the dicarboxylic acid units include one or more of succinic acid, adipic acid, cyclohexane dicarboxylic acid, suberic acid, phthalic acid, naphthoic acid, trimellitic acid, or pyromellitic acid, and the diol units include one or more of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, decanediol, diethylene glycol, dipropylene glycol, dimethylolpropane, or dimethylolethane.

[0103] Embodiment 10 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 9, wherein the carboxyl terminated polyester is selected from a carboxyl terminated phthalate polyester, a carboxyl terminated adipate polyester, or a combination thereof.

[0104] Embodiment 11 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 10, wherein the polyisocyanate-modified polyester is a phthalate polyester, a polyisocyanate-modified adipate polyester, or a combination thereof, which is modified by a polyisocyanate selected from toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, or a combination thereof.

[0105] Embodiment 12 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 11, wherein the polyisocyanate-modified (hydroxyl-terminated) polyester has a weight average molecular weight of 20,000 g / mol or greater.

[0106] Embodiment 13 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 12, wherein the polyisocyanate-modified polyester has a glass transition temperature Tg of -11°C to 16°C.

[0107] Embodiment 14 provides a B-stageable adhesive composition according to any one of Embodiments 1 to 13, wherein the crosslinker is 1,1′-isophthaloylbis(2-methylaziridine), trimethylolpropane tris(2-methyl-1-aziridine propionate), 2-((3-aziridine-1-ylpropionyl)methyl)-2-ethylpropane-1,3-diylbis(aziridine-1-propionate), or a combination thereof.

[0108] Embodiment 15 provides the B-stageable adhesive composition of any one of Embodiments 1 to 14, further comprising a solvent.

[0109] Embodiment 16 provides a B-stageable adhesive composition according to embodiment 15, wherein the solvent is selected from N,N-dimethylformamide, methyl ethyl ketone (MEK), hexane, heptane, cyclohexane, toluene, xylene, or a combination thereof.

[0110] Embodiment 17 provides a B-stageable adhesive composition according to Embodiment 15 or 16, wherein the solvent is present in the B-stageable adhesive composition in an amount of 30 wt % to 70 wt % based on the total weight of the B-stageable adhesive composition.

[0111] Embodiment 18 provides the B-stageable adhesive composition of any one of Embodiments 1 to 17, further comprising a toughening agent, a flame retardant, or a combination thereof.

[0112] Embodiment 19 provides a B-stageable adhesive composition according to Embodiment 18, wherein the toughening agent is present in the B-stageable adhesive composition in an amount of 0.5 wt % to 2.0 wt %, based on the total weight of the B-stageable adhesive composition.

[0113] Embodiment 20 provides a B-stageable adhesive composition according to Embodiment 18, wherein the flame retardant is present in the B-stageable adhesive composition in an amount of 1.0 wt % to 30.0 wt %, based on the total weight of the B-stageable adhesive composition.

[0114] Embodiment 21 provides an article including a substrate and a coating formed of the adhesive composition according to any one of Embodiments 1 to 20 on a surface of the substrate.

[0115] Embodiment 22 provides an article according to embodiment 21, wherein the article is in the form of a plate, sheet, belt, roll, film or tube.

[0116] Example

[0117] Hereinafter, the present disclosure is further described with reference to the following Examples and Comparative Examples, which are provided in the present disclosure for illustrative purposes only and are not intended to limit the scope of the present disclosure.

[0118] It should be understood that those skilled in the art can conceive of other various embodiments and modify them according to the teachings of the specification without departing from the scope or spirit of the present disclosure. Therefore, the following embodiments are not intended to be limiting in any sense.

[0119] Unless otherwise indicated, it should be understood that all numbers used to represent feature sizes, quantities and physicochemical characteristics in the specification and claims are modified by the term "about" in all cases. Therefore, unless otherwise stated to the contrary, the numerical parameters listed in this specification and claims are approximate values. Those skilled in the art can appropriately change these approximate values ​​according to the teachings disclosed herein to obtain the desired characteristics. The numerical range represented by using the endpoint should include all numbers and any range therein. For example, the range 1-5 includes 1, 1.1, 1.3, 1.5, 2, 1.75, 3, 3.80, 4 and 5, etc.

[0120] Unless otherwise indicated, all percentages used herein refer to weight percentages based on the total weight of the adhesive composition.

[0121] raw materials

[0122] The raw materials used in the following illustrative examples of the present disclosure are commercially available and are listed in Table 2 below by trade name, chemical name and supplier.

[0123] Table 2: Raw materials list

[0124]

[0125]

[0126]

[0127] Test Method

[0128] The adhesion strength of the coating was evaluated by the “peel strength test” (180° peel strength at 25°C), the heat resistance of the coating was evaluated by adhesive oozing out in the “adhesive flow test” (i.e., 180° peel strength at 105°C or 130°C), and a bending simulation test was performed to evaluate the toughness of the coating.

[0129] Initial viscosity

[0130] Initial tack is an important property of a B-stage adhesive composition and will affect the application operation. The present invention is intended to disclose a B-stage adhesive film with good initial tack at room temperature (about 25°C), and will be very suitable for die cutting and easy to assemble into a multilayer film. According to ASTM D1000, after the heat aging test, the tack during application is evaluated by measuring the 180° peel force at room temperature. Specifically, a sample of the adhesive film is formed by coating the B-stage adhesive composition on a 0.175mm white PET film (BP, Foshan Dupont Company). The adhesive film is then cut into a size of 150mm long and 25.4mm wide, and a 10-layer adhesive film sample is prepared by stacking ten adhesive films arranged in the same direction, and then 70g / cm 2 A pressure of 100° C. was applied to the 10-layer adhesive film sample, which was kept at 65° C. for heat aging for 1 week. After the heat aging test, the 10-layer adhesive film sample could be stuck together, and the adhesion for separating the samples was measured by 180° peeling at room temperature.

[0131] The initial tack of the adhesive film at 25° C. was evaluated according to the result criteria shown in Table 3-1.

[0132] Table 3-1

[0133]

[0134]

[0135] Peel strength test

[0136] In order to study the bonding strength of the final cured product formed by the B-stageable adhesive composition, the sample of the adhesive film formed by the B-stageable adhesive composition of the present disclosure was tested for 180° peel strength according to ASTM D1000. Specifically, the sample of the B-stageable adhesive film obtained by the B-stageable adhesive composition of the present disclosure was adhered to a copper plate having a thickness of 0.3 mm using manual pressure, and then placed in a hot press to perform heat lamination at 160°C and 0.7MPa for 20 minutes, so that the adhesive film adhered to the copper plate. After 30 minutes, the 180° peel strength was tested on a tensile machine under the following test conditions:

[0137] (1) Peel strength test at room temperature (25°C)

[0138] Air temperature: 25℃;

[0139] Substrate: copper plate;

[0140] Speed: 100mm / min;

[0141] Sample size: 150mm long, 12.7mm wide;

[0142] Number of samples: 5.

[0143] The 180° peel strength of the coating at 25° C. was evaluated according to the result criteria shown in Table 3-2.

[0144] Table 3-2

[0145] 180° peel strength at 25°C Results Criteria <1.0N / mm Unacceptable 1.0N / mm to 1.5N / mm Acceptable >1.5N / mm Excellent

[0146] (2) Peel strength test at 105°C (i.e. heat resistance)

[0147] Atmospheric temperature and time: 105°C, after 15 minutes;

[0148] Substrate: copper plate;

[0149] Speed: 50mm / min;

[0150] Sample size: 150mm long, 12.7mm wide;

[0151] Number of samples: 5.

[0152] The 180° peel strength of the coating at 105° C. was evaluated according to the result criteria shown in Table 3-3.

[0153] Table 3-3

[0154] 180° peel strength at 105°C Results Criteria <0.4N / mm Unacceptable 0.4N / mm to 0.6N / mm Acceptable >0.6N / mm Excellent

[0155] (3) Peel strength test at 130°C (i.e. heat resistance)

[0156] Atmospheric temperature and time: 130°C, after 15 minutes;

[0157] Substrate: copper plate;

[0158] Speed: 50mm / min;

[0159] Sample size: 150mm long, 12.7mm wide;

[0160] Number of samples: 5.

[0161] The 180° peel strength of the coatings at 105°C was evaluated according to the results criteria shown in Tables 3-4.

[0162] Table 3-4

[0163] 180° peel strength at 130°C Results Criteria <0.2N / mm Unacceptable 0.2N / mm to 0.3N / mm Acceptable >0.3N / mm Excellent

[0164] 90° bending simulation test

[0165] In order to study the balance between the room temperature flexibility and heat resistance of the final cured product formed by the B-stage adhesive composition, the sample of the adhesive film formed by the B-stage adhesive composition of the present invention was tested for a 90° bending simulation test. Specifically, the sample of the B-stage adhesive film obtained by the B-stage adhesive composition of the present invention was adhered to a copper plate with a size of 50 mm wide, 150 mm long and 2 mm thick, and then placed in a hot press to be thermally laminated at 160°C and 0.7MPa for 20 minutes, so that the adhesive film is adhered to the copper plate with a 2mm adhesive film edge width and the excess edge is removed. Then, the copper plate with the adhesive film is bent at 90° in a bending machine and the height of the bent copper plate is 20 mm. After the sample is prepared, it is placed in an oven at 105°C for 1 week.

[0166] The heat resistance of the coatings was evaluated according to the result criteria shown in Tables 3-6.

[0167] Table 3-6

[0168] Heat resistance at 105°C Results Criteria Cracking Unacceptable Uncracked good

[0169] Examples E1-E9

[0170] An adhesive film was prepared using the components and amounts listed in Table 4-1 by the following steps:

[0171] Step 1: In a 100 ml flask and at room temperature, polyester V1801, V2700, V3300 or V3650 was dissolved in MEK solvent to obtain a solution having a solid content of 34%, and then polyisocyanate N100 and catalyst D80 were added in a suitable ratio, cured for 1 day to obtain a polyisocyanate-modified polyester.

[0172] Step 2: In a 100 ml flask, the first epoxy resin and the second epoxy resin, the carboxyl-terminated polyester and the polyisocyanate-modified polyester were dissolved in methyl ethyl ketone (MEK) at room temperature to obtain a solution, and then a crosslinking agent was added and uniformly mixed;

[0173] Step 3: If necessary, add other optional components such as toughening agent, etc., and stir at room temperature to obtain an adhesive mixture.

[0174] The adhesive film was prepared by the following steps:

[0175] Step 1: applying the above adhesive mixture onto the surface of a 175 μm PET film by knife coating, wherein the coating thickness is about 35 μm to 40 μm;

[0176] Step 2: Dry the coated PET film in an oven at a temperature of 105° C. for 5 minutes, and then cut the dried adhesive film into a sample size of 150 mm long and 12.7 mm wide;

[0177] Step 3: Laminating the adhesive film onto the copper plate at a temperature of 160°C and a pressure of 0.7 MPa for 20 minutes;

[0178] Step 4: Cool the sample to room temperature (25°C).

[0179] The adhesion strength (ie, 180° peel strength at 25° C., 105° C., and 130° C.), heat resistance, and toughness of the coating were measured according to the test methods described above. The test results are shown in Table 4-2.

[0180] Comparative Examples C1-C9

[0181] Adhesive film samples of Comparative Examples C1 to C11 were prepared by the same method as above using the components and amounts listed in Table 4-1. The test results are shown in Table 4-2.

[0182]

[0183]

[0184] From the experimental data of Table 4-1 and Table 4-2, the adhesive films of Examples E1 to E7 that satisfy the composition of the adhesive composition in terms of the types and amounts of the components required by the present disclosure show a good balance between peel strength (at 25°C) and peel strength (at 105°C or 130°C, i.e., heat resistance), together with initial tack and toughness. On the contrary, the adhesive films of Comparative Examples C1 to C11 that do not satisfy the composition of the adhesive composition in terms of one or more of the types and amounts of the components required by the present disclosure do not show a good balance between peel strength (at 25°C) and peel strength (at 105°C or 130°C, i.e., heat resistance), together with initial tack.

[0185] Although the present disclosure has been described with reference to a number of illustrative embodiments as explained above, it will be appreciated that those skilled in the art may devise many other modifications and embodiments that fall within the scope of the principles of the present disclosure. More specifically, within the scope of the present disclosure, the drawings and the appended claims, various variations and modifications may be made in the component parts and / or arrangements of the subject combination arrangement. In addition to variations and modifications of the component parts and / or arrangements, alternative uses will also be apparent to those skilled in the art.

Claims

1. A B-stageable epoxy adhesive composition, comprising: (A) 20 to 50 wt % of a first epoxy resin having an epoxide equivalent weight of 5000 g / eq or more; (B) 5 to 20 wt % of a second epoxy resin having an epoxide equivalent weight of 800 g / eq or less and having 2 to 4 epoxy functional groups; (C) 5 to 30 wt % of a carboxyl terminated polyester; (D) 5 to 15 wt% of a polyisocyanate-modified polyester having a glass transition temperature Tg of -13°C to 30°C; (E) 0.1 wt % to 0.5 wt % of a crosslinking agent containing 2 or more aziridine groups, wherein all percentages are based on the total weight of the B-stageable epoxy adhesive composition.

2. The B-stageable adhesive composition of claim 1, wherein the first epoxy resin has a weight average molecular weight (Mw) of 10,000 g / mol or greater, wherein the first epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, and combinations thereof. 3 . The B-stageable adhesive composition of claim 1 , wherein the first epoxy resin has a weight average molecular weight (Mw) of 10,000 g / mol or greater, wherein the first epoxy resin is a glycidyl ether epoxy resin.

4. The B-stageable adhesive composition of claim 1, wherein the first epoxy resin is present in the B-stageable adhesive composition in an amount of 35 wt% to 45 wt%, based on the total weight of the B-stageable adhesive composition. 5 . The B-stageable adhesive composition of claim 1 , wherein the second epoxy resin has a weight average molecular weight (Mw) of 200 to 2,000 g / mol.

6. The B-stageable adhesive composition of claim 5, wherein the second epoxy resin is selected from the group consisting of polyurethane-modified bisphenol A epoxy resin, polyurethane-modified bisphenol F epoxy resin, polyurethane-modified novolac epoxy resin, polyurethane-modified trisphenol methane epoxy resin, polyurethane-modified glycidylamine epoxy resin, polyurethane-modified aminophenol epoxy resin, polyurethane-modified naphthalene epoxy resin, and combinations thereof.

7. The B-stageable adhesive composition of claim 1, wherein the second epoxy resin is present in the B-stageable adhesive composition in an amount of 6 wt% to 10 wt%, based on the total weight of the B-stageable adhesive composition. 8 . The adhesive composition of claim 1 , wherein the carboxyl-terminated polyester has an acid value of 20 to 80 mg KOH / g.

9. The adhesive composition according to claim 1, wherein the carboxyl-terminated polyester or the polyisocyanate-modified polyester comprises dicarboxylic acid units and diol units, wherein the dicarboxylic acid units include one or more of succinic acid, adipic acid, cyclohexane dicarboxylic acid, suberic acid, phthalic acid, or naphthalene dicarboxylic acid, and the diol units include one or more of ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, decanediol, diethylene glycol, dipropylene glycol, dimethylolpropane, or dimethylolethane.

10. The B-stageable adhesive composition of claim 1, wherein the carboxyl terminated polyester is selected from the group consisting of a carboxyl terminated phthalate polyester, a carboxyl terminated adipate polyester, or a combination thereof.

11. The B-stageable adhesive composition of claim 1 , wherein the polyisocyanate-modified polyester is a phthalate polyester, an adipate polyester, or a combination thereof, which is modified by a polyisocyanate selected from toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, or a combination thereof. 12 . The adhesive composition according to claim 1 , wherein the polyisocyanate-modified polyester has a weight average molecular weight of 20,000 g / mol or more.

13. The B-stageable adhesive composition of claim 1, wherein the polyisocyanate-modified polyester has a glass transition temperature Tg of -11°C to 16°C.

14. The B-stageable adhesive composition of claim 1, wherein the crosslinker is 1,1'-isophthaloylbis(2-methylaziridine), trimethylolpropane tris(2-methyl-1-aziridine propionate), 2-((3-aziridine-1-ylpropionyl)methyl)-2-ethylpropane-1,3-diylbis(aziridine-1-propionate), or a combination thereof.

15. The B-stageable adhesive composition of claim 1 further comprising a solvent.

16. The B-stageable adhesive composition of claim 15, wherein the solvent is selected from N,N-dimethylformamide, methyl ethyl ketone, hexane, heptane, cyclohexane, toluene, xylene, or combinations thereof.

17. The B-stageable adhesive composition of claim 15, wherein the solvent is present in the B-stageable adhesive composition in an amount of 30 wt% to 70 wt%, based on the total weight of the B-stageable adhesive composition.

18. The B-stageable adhesive composition of claim 1, further comprising a toughening agent, a flame retardant, or a combination thereof.

19. The B-stageable adhesive composition of claim 18, wherein the toughening agent is present in the B-stageable adhesive composition in an amount of 0.5 wt% to 2.0 wt%, based on the total weight of the B-stageable adhesive composition.

20. The B-stageable adhesive composition of claim 18, wherein the flame retardant is present in the B-stageable adhesive composition in an amount of 1.0 wt% to 30.0 wt%, based on the total weight of the B-stageable adhesive composition.

21. An article comprising a substrate and a coating formed of the adhesive composition according to claim 1 on a surface of the substrate, wherein the article is in the form of a plate, a belt, a roll, a film or a tube.

Citation Information

Patent Citations

  • Epoxy resin roughening and curing agent

    CN100336841C

  • An adhesive composition and an article manufactured therefrom

    CN108026424A

  • B-stageable adhesive composition

    CN108291129A

  • Epoxy resin composition, cured article thereof, novel epoxy resin, novel phenol compound, and process for preparing the same

    EP1275673A2

  • Adhesive composition and articlemanufactured therefrom

    CN107922813A

Cited By

  • One-component adhesive composition, process for the production thereof, b-staged resin film and use thereof

    CN123083472A