Decorative sheet, decorative board and method for manufacturing decorative sheet
By using ionizing radiation-curable resin in the surface protective layer of the decorative sheet and forming concave-convex ridges, the problem of reduced oleophobicity caused by gloss modifiers is solved and the fingerprint resistance and contamination resistance of the decorative sheet are improved.
Patent Information
- Application Number
- CN202180008332.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-01-05
AI Technical Summary
The use of gloss modifiers in existing decorative sheets results in reduced surface oleophobicity and easy attachment of fingerprints.
Ionizing radiation-curable resin is used as the surface protective layer. By irradiating the surface with ionizing radiation of a specific wavelength, it shrinks to form uneven ridges, thereby improving the surface's oleophobicity and fingerprint resistance.
A decorative sheet with a matte surface and fingerprint resistance is realized, which reduces fingerprint adhesion and oil adsorption, and improves the wear resistance and pollution resistance of the surface.
Smart Images

Figure CN114945463B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a decorative sheet, a decorative board and a method for manufacturing the decorative sheet. Background Art
[0002] Conventionally, for decorative sheets, a gloss adjuster (matting additive) is added to the surface protective layer of the decorative sheet to adjust the matte feeling of the decorative sheet surface from the viewpoint of design etc. (for example, see Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-129959 Summary of the invention
[0006] Problems to be Solved by the Invention
[0007] However, the gloss adjuster reduces the oleophobicity of the layer formed of the resin material. Therefore, the decorative sheet having the surface protection layer containing the gloss adjuster has a problem that fingerprints are easily attached.
[0008] The present disclosure has been made in view of such a problem, and an object of the present invention is to provide a decorative sheet having excellent anti-fingerprint properties on the surface of the decorative sheet, a decorative board, and a method for producing the decorative sheet.
[0009] Solutions to Solve Problems
[0010] In order to solve the above-mentioned problems, a decorative sheet involved in one embodiment of the present invention is characterized in that it comprises: a raw material layer, a colored pattern layer arranged on one surface of the raw material layer, and a first surface protection layer, which is arranged on the surface of the colored pattern layer on the opposite side of the raw material layer, has a core portion and a ridge portion protruding from one surface of the core portion in a ridge shape, and has a concave-convex shape formed on the surface.
[0011] Furthermore, a decorative board according to another aspect of the present disclosure is characterized by comprising: the decorative sheet described above; and a base material layer provided on a surface of the raw material layer on the opposite side to the colored pattern layer.
[0012] In addition, the manufacturing method of the decorative sheet involved in other embodiments of the present invention is characterized in that a first ionizing radiation having energy capable of cutting the polymer chain of the ionizing radiation curing resin is irradiated onto a surface coated with an ionizing radiation curing resin to shrink the surface of the ionizing radiation curing resin and form a concave-convex shape on the surface of the ionizing radiation curing resin, and the ionizing radiation curing resin is cured by irradiating the shrunken ionizing radiation curing resin with a second ionizing radiation for curing the ionizing radiation curing resin, thereby forming a first surface protective layer having a core portion and a ridge portion protruding in a ridge shape from one surface of the core portion.
[0013] Effects of the Invention
[0014] According to the aspects of the present disclosure, a decorative sheet, a decorative board, and a method for manufacturing a decorative sheet that can achieve both a matte feeling and fingerprint resistance on the surface of the decorative sheet can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] [ Figure 1 ] is a cross-sectional view showing a structural example of a decorative sheet involved in the first embodiment of the present disclosure.
[0016] [ Figure 2 ] is a plan photograph showing a configuration example of the surface of the first surface protection layer of the decorative sheet involved in the first embodiment of the present disclosure.
[0017] [ Figure 3 ] is a cross-sectional photograph showing a configuration example of the first surface protection layer of the decorative sheet involved in the first embodiment of the present disclosure.
[0018] [ Figure 4 ] is an enlarged cross-sectional view showing a structural example of a decorative sheet involved in the first embodiment of the present disclosure.
[0019] [ Figure 5 ] is an enlarged cross-sectional view showing the surface shape of the surface protection layer when a concavo-convex shape is formed on the surface of the surface protection layer by mechanical processing such as embossing.
[0020] [ Figure 6 ] is a cross-sectional view showing a modified example of the decorative sheet involved in the first embodiment of the present disclosure.
[0021] [ Figure 7 ] is a cross-sectional view showing a modified example of the decorative sheet involved in the first embodiment of the present disclosure.
[0022] [ Figure 8 ] is a cross-sectional view showing a modified example of the decorative sheet involved in the first embodiment of the present disclosure.
[0023] [ Fig. 9] is a cross-sectional view showing a structural example of a decorative sheet involved in the second embodiment of the present disclosure.
[0024] [ Fig.10 ] is a cross-sectional view showing a structural example of a decorative panel involved in the third embodiment of the present disclosure. DETAILED DESCRIPTION
[0025] The present disclosure is described below through embodiments, but the following embodiments do not limit the invention involved in the claims. In addition, not all combinations of the features described in the embodiments are necessary for the solution of the invention. In addition, the drawings schematically illustrate the invention involved in the claims, and the dimensions such as the width and thickness of each part are different from the actual situation, and their ratios are also different from the actual situation.
[0026] The decorative sheet of the present disclosure is described. The decorative sheet involved in the present disclosure is, for example, a decorative sheet applied to a wall surface, a door or window, a piece of furniture, etc. It should be noted that in the following description, the side of the decorative sheet in contact with the substrate is sometimes referred to as "lower" and the side (surface) opposite to the side in contact with the substrate is sometimes referred to as "upper".
[0027] Below, refer to Figures 1 to 8 Each mode of each embodiment of the present disclosure will be described.
[0028] 1. First Implementation
[0029] (1.1) Basic composition of decorative sheets
[0030] use Figure 1 A basic configuration of a decorative sheet according to a first embodiment of the present disclosure will be described. Figure 1 1 is a cross-sectional view for explaining a configuration example of a decorative sheet 1 according to an embodiment of the present disclosure. Figure 1 As shown, the decorative sheet 1 comprises: a raw material layer 11, a colored pattern layer 12, and a first surface protection layer 13. The decorative sheet 1 is formed by laminating the raw material layer 11, the colored pattern layer 12, and the first surface protection layer 13 in sequence.
[0031] The raw material layer 11 is a layer that becomes the base material of the decorative sheet 1, and is a layer used to absorb the unevenness or step difference of the pasting surface to complete the construction of the decorative sheet 1 well and conceal the color / pattern of the pasting surface. The colored pattern layer 12 is a layer that gives at least one of color and pattern to the decorative sheet 1. The first surface protection layer 13 is a layer used to protect the raw material layer 11 and the colored pattern layer 12 from damage.
[0032] Hereinafter, each of the raw material layer 11 , the colored pattern layer 12 , and the first surface protection layer 13 will be described in detail.
[0033] <Raw material layer>
[0034] The raw material layer 11 is a layer (sheet) serving as a base material of the decorative sheet 1 .
[0035] The raw material layer 11 is, for example, a paper material mainly composed of pulp or cellulose fibers, or a resin layer or a resin sheet formed of a resin material.
[0036] When the raw material layer 11 is a paper material, additives such as a paper strength enhancer, an additive for improving concealment, cellulose nanofibers, and a colorant may be added.
[0037] In addition, when the raw material layer 11 is a resin material, it is preferable to use a thermoplastic resin represented by polypropylene, polyethylene, and polyester as the resin material. The thermoplastic resin may contain, for example, an inorganic material such as titanium oxide and calcium carbonate as an additive. By using at least one of polypropylene, polyethylene, and polyester as the thermoplastic resin, the dispersibility of the inorganic material is improved. In addition, by using polypropylene as the thermoplastic resin, the dispersibility of the inorganic material is further improved.
[0038] In addition, when the raw material layer 11 is a resin film, as the resin film, a film material mainly composed of polyethylene terephthalate is preferred. The resin film may contain the above-mentioned inorganic material as an additive. In addition, when the raw material layer 11 is a resin film, the raw material layer 11 may be a resin film formed by uniaxial or biaxial stretching. The raw material layer 11 formed by the resin film formed by uniaxial or biaxial stretching may contain voids inside.
[0039] When the raw material layer 11 is a resin material or a resin film, the content of the inorganic material relative to the raw material layer 11 is preferably in the range of 1 mass % to 90 mass %, more preferably in the range of 5 mass % to 80 mass %, and further preferably in the range of 20 mass % to 80 mass %. By making the content of the inorganic material within the above range, sufficient non-combustibility or sufficient flame retardancy can be reliably obtained, while the printability and lamination suitability can be reliably improved, and cracks generated in the curved portion of the sheet can be reliably reduced.
[0040] The thickness of the raw material layer 11 is preferably within a range of 20 μm to 250 μm, more preferably within a range of 25 μm to 250 μm, and further preferably within a range of 70 μm to 200 μm. When the thickness of the raw material layer 11 is within the above range, lamination suitability can be improved and cracks generated in the bent portion of the sheet can be reduced.
[0041] The surface of the raw material layer 11 may be subjected to a surface treatment such as a corona treatment or a plasma treatment. This improves the adhesion (closeness) between the raw material layer 11 and the colored pattern layer 12.
[0042] <Coloring pattern layer>
[0043] The colored pattern layer 12 is provided on one surface of the raw material layer 11. The colored pattern layer 12 includes, for example, a colored layer 12A provided on the raw material layer 11 and a pattern layer 12B provided on the colored layer 12A. It should be noted that the colored pattern layer 12 may include at least one of the colored layer 12A and the pattern layer 12B according to the desired design.
[0044] The colored layer 12A is a layer for imparting a desired color design to the decorative sheet 1 and concealing the color and pattern of the base material to which the decorative sheet 1 is attached. The colored layer 12A is formed by, for example, solid application of ink.
[0045] The pattern layer 12B is provided on the surface side of the decorative sheet 1 more than the colored layer 12A and provides the decorative sheet 1 with a desired design. The pattern layer 12B is formed on the colored layer 12A and is printed with patterns such as wood grain patterns, stone grain patterns, sand grain patterns, tile patterns, brick stack patterns, cloth grain patterns, leather grain patterns, geometric patterns, etc.
[0046] The coloring layer 12A and the pattern layer 12B are formed by, for example, screen printing using ink. As the ink used to form the coloring layer 12A and the pattern layer 12B, for example, any one of isoindolinone yellow, polyazo red, phthalocyanine blue, carbon black, iron oxide, and titanium oxide can be used alone or as a mixture thereof. In addition, these inks may be aqueous solvents or organic solvents. As the organic solvent, for example, ethyl acetate, n-butyl acetate, isobutyl alcohol, methyl isobutyl ketone, etc. can be used.
[0047] The thickness of the colored layer 12A and the pattern layer 12B of the colored pattern layer 12 can be any thickness that fully expresses the desired degree of design. The thickness of the colored layer 12A is preferably in the range of 2 μm to 20 μm, for example. By making the thickness of the colored layer 12A within the above range, for example, even when colored in white or light colors, the color and stains of the original material layer 11 can be sufficiently concealed, and the reduction in the adhesion strength between the ink layers constituting the colored layer 12A can be prevented, so that sufficient durability can be obtained. In addition, the thickness of the pattern layer 12B is preferably in the range of 0.1 μm to 10 μm, for example. Here, the "thickness of the pattern layer 12B" refers to the thickness of the portion printed with ink. The pattern layer 12B may not be provided on the entire surface of the colored layer 12A, and the colored layer 12A may be exposed from the pattern layer 12B. By making the thickness of the pattern layer 12B within the above range, the pattern can be clearly expressed, or the design can be improved by adding gradations to the pattern. In addition, when multiple colors are printed in an overlapping manner, the color of the upper layer overlaps with the color of the lower layer, thereby increasing the color width that can be expressed by limited colors.
[0048] <First surface protective layer>
[0049] The first surface protection layer 13 is arranged on the surface of the colored pattern layer 12 on the opposite side of the raw material layer 11. The first surface protection layer 13 includes a core 13A as a lower layer (back side) area in the layer, and a ridge 13B as an upper layer (surface side) area in the layer. The first surface protection layer 13 has a core 13A and a ridge 13B that is arranged to protrude from one surface of the core 13A in a ridge shape. Thus, a concavo-convex shape is formed on the surface of the first surface protection layer 13.
[0050] Here, in the decorative sheet 1 involved in the present embodiment, "ridge" refers to a shape that is slenderly raised and connected in a linear shape in a plan view. The ridge portion 13B may be curved or straight in a plan view, but is preferably curved from the viewpoint of the anti-fingerprint property of the surface of the decorative sheet 1. In addition, in the present disclosure, the ridge portion 13B is, for example, a portion from the lowest part to the top of the concave-convex shape provided on the surface of the first surface protection layer 13, and the core portion 13A refers to the portion of the first surface protection layer 13 other than the ridge portion 13B.
[0051] Figure 2 This is a plan view showing the structure of the surface (upper surface) of the first surface protection layer 13. Figure 3 : is a cross-sectional photograph showing the structure of the surface (upper surface) of the first surface protection layer 13. Figure 4 It is a cross-sectional view schematically showing the structure of the surface (upper surface) of the first surface protection layer 13 . Figure 3 and Figure 413B is a cross-sectional photograph and a cross-sectional view showing a cross section in the width direction of the ridge portion 13B. Figure 2 and Figure 3 These are plan and cross-sectional photographs obtained using an optical microscope (digital microscope, VHX-6000 manufactured by KEYENCE).
[0052] like Figure 2 and Figure 3 As shown in the plan view and cross-sectional view, the ridge 13B is a shape that is slenderly raised and connected in a linear shape in a plan view. As described later, the ridge 13B is formed by irradiating the surface of the ionizing radiation curing resin with ionizing radiation of a specific wavelength to shrink the surface of the ionizing radiation curing resin. The ridge 13B formed by the shrinkage of the ionizing radiation curing resin has a different composition from the core 13A that has not shrunk. Specifically, the ridge 13B formed by the shrinkage of the ionizing radiation curing resin has a composition in which the ratio of the carbonyl bond (C=O) and the carbon-carbon bond (double bond (C=C) and triple bond (C≡C) of carbon to carbon) contained in the resin is reduced compared to the core 13A in the deep layer. For example, the ratio of the carbonyl bond and the carbon-carbon bond contained in the resin in the ridge 13B is preferably reduced by 10% or more, and more preferably reduced by 20% or more, compared to the core 13A in the deep layer. This is because, by irradiating the ionizing radiation curing resin with high energy ionizing radiation, the polymer chains (carbonyl bonds and carbon-carbon bonds (double bonds, triple bonds)) contained in the resin are broken. In the ionizing radiation curing resin irradiated with high energy ionizing radiation, new bonds (rebonding, re-crosslinking) are generated at the broken bond portions, so that the surface of the ionizing radiation curing resin shrinks to form the ridge 13B. Such a difference in composition between the core 13A and the ridge 13B is a feature when the surface of the first surface protective layer 13 is formed with unevenness by irradiating ionizing radiation.
[0053] In addition, by irradiating the ionizing radiation curing resin with high energy ionizing radiation, the polymer chains contained in the resin are cut, and rebonding and re-crosslinking are performed in a state where hydrogen atoms are abstracted. Therefore, compared with the core 13A in the deep layer, the ridge 13B formed by the cutting, rebonding and re-crosslinking of the polymer chains has a high crosslinking density. Therefore, the porosity in the resin of the surface part of the first surface protection layer 13 as the outermost layer of the decorative sheet 1, that is, the ridge 13B, is reduced, and the surface hardness of the first surface protection layer 13 is increased, thereby improving the scratch resistance of the decorative sheet 1.
[0054] like Figure 4As shown, the surface of such a ridge 13B is curved in the cross-sectional view. The ridge 13B shrinks due to the ablation of the ionizing radiation curing resin after irradiation with ionizing radiation of a specific wavelength. That is, by irradiating the surface of the ionizing radiation curing resin with a strong laser, the ionizing radiation curing resin on the surface that has become locally hot evaporates, and atoms, molecules, plasma, and their clusters fly away, thereby forming the ridge 13B. In this way, the ridge 13B that is curved in the cross-sectional view has a concave-convex shape formed on the surface of the surface protection layer by mechanical processing such as embossing (see Figure 5 ) are of distinctly different shapes.
[0055] Therefore, a smooth ridge 13B is formed on the surface of the ionizing radiation curing resin due to surface tension. Specifically, the free radicals of the ionizing radiation directly cut the carbonyl bond and the double or triple bond between carbon and carbon in the resin constituting the first surface protection layer 13. In addition, by irradiation with high-energy ionizing radiation such as vacuum ultraviolet light, ozone or oxygen free radicals are generated from oxygen molecules, and the free radicals generated in this way may cut the carbonyl bond and the double or triple bond between carbon and carbon. In this case, ozone or oxygen free radicals are generated from oxygen molecules whose concentration (for example) is limited to 2000ppm, preferably 1000ppm or less, and more preferably 400ppm or less in a vacuum atmosphere. The cut bonds are rebonded with adjacent atoms such as carbon, oxygen, nitrogen, or free radicals present in the atmosphere, causing the surface of the ionizing radiation curing resin to shrink, thereby forming a gentle curve shape. The gentle shape of such a ridge 13B is also a feature when the surface of the first surface protection layer 13 is formed with unevenness by irradiating ionizing radiation.
[0056] The height of such a ridge 13B is, for example, preferably less than 15 μm, more preferably less than 8 μm. In addition, the period p of adjacent ridges 13B (for example, the interval between the vertices of the ridges 13B) is preferably less than 50 μm, preferably less than 10 μm, and more preferably less than 6.5 μm. Compared with the concave-convex shape formed on the surface of the surface protection layer by mechanical processing such as embossing, the ridge 13B formed by irradiating high-energy ionizing radiation to the ionizing radiation-curing resin has a fine structure. By forming such a fine concave-convex shape on the surface of the first surface protection layer 13, the fingerprint resistance can be improved while maintaining the matte feeling of the surface of the decorative sheet 1.
[0057] The following describes in more detail the mechanism by which the ridge portion 13B is formed by irradiation with the first ionizing radiation.
[0058] Vacuum ultraviolet light (VUV) can use photon energy to cut bond energy that is less than the photon energy. Therefore, by irradiating the surface of the ionizing radiation curing resin with vacuum ultraviolet light, the molecular bonds of the organic matter in the ionizing radiation curing resin are cut, and the bonding state of the polymer on the surface of the ionizing radiation curing resin changes, thereby modifying (shrinking) the surface.
[0059] When a rare gas, a halogen gas and mercury are combined as the medium of the first ionizing radiation, a light source close to monochromatic light can be obtained with a wavelength interval of 20nm to 30nm within a wavelength range of 100nm to 500nm. As the first ionizing radiation for forming the ridge 13B, any of these light sources can be used. However, when considering the size of the obtained photon energy, the difference between the wavelength and the bond energy of the organic matter, it is most preferred to use a xenon lamp that emits an excimer laser with a central wavelength of 172nm as the light source. The lower the wavelength and the stronger the energy of the first ionizing radiation, the more it can cut the molecular bonds of the organic matter and thus the easier it is to cause surface shrinkage, so it is preferred. On the other hand, when considering the cost involved in equipment maintenance, the acquisition of materials, etc., it is most preferred to use a xenon lamp as the light source.
[0060] Here, the light with a wavelength of less than 380nm is called ultraviolet light (UV), and the light with a wavelength of less than 200nm is called vacuum ultraviolet light (VUV), and the light is absorbed by the oxygen in the atmosphere and attenuated. Therefore, by removing the oxygen under the first ionizing radiation irradiation environment, the surface modification effect of the ionizing radiation curing resin can be further improved. In addition, it is preferred that the required reaction gas (for example, nitrogen) is introduced to control the reaction atmosphere, or a chamber system in which the oxygen concentration is suppressed to less than 2000ppm is used to irradiate the ionizing radiation curing resin with ultraviolet light (especially, light less than 250nm). Light can cut off the molecular bonds of the organic substances in the ionizing radiation curing resin, hydrogen atoms are taken away, and the composition of the molecules is easily changed, thereby easily causing the surface modification (contraction) of the ionizing radiation curing resin.
[0061] In order to prevent stains such as hand oil and fingerprints from adhering to the resin surface, it is necessary to have oleophobicity. Therefore, by irradiating the ionizing radiation with the oxygen concentration in the ionizing radiation irradiation atmosphere as low as possible (ideally under the condition of 400 ppm or less), the performance of the decorative sheet for the purpose of this application can be exhibited. By adjusting the oxygen concentration during light irradiation, the desired surface performance can be exhibited.
[0062] The photons excited by the irradiation of the excimer laser are strongly absorbed into the polymer chains of the ionizing radiation curing resin as the surface protective layer on the surface of the decorative sheet until they reach a depth of about tens to hundreds of nanometers of the ionizing radiation curing resin, thereby generating polymer free radicals. Through the polymer free radicals, the polymer chains of the ionizing radiation curing resin are cut, rebonded, and recrosslinked. As a result, on the surface of the ionizing radiation curing resin, the molecular weight increases, and the free volume (void ratio) in the polymer decreases, thereby generating fine concave and convex shapes connected in a wavy shape like folded folds.
[0063] The period (pitch of concavities and convexities) I of the contracted microstructure produced by irradiating the ionizing radiation-curing resin with an excimer laser can be obtained according to the Polanyi equation represented by the following equation (1) and the Polanyi equation represented by equation (2) focusing on the 0th-order diffracted light and the 1st-order diffracted light.
[0064]
[0065] l·sin[arctan(x / d)]=λ···(2)
[0066] Here, in formula (1), l is the period of the microstructure, is the angle of the diffracted light of the excimer laser, m is an integer greater than 0, and λ is the wavelength of the excimer laser. In addition, in formula (2), x is the distance between the 0th order diffracted light and the 1st order diffracted light on the screen, and d is the distance between the screen on which the diffracted light is projected and the ionizing radiation curing resin as a sample. In addition, in the formula.
[0067] By changing the incident angle θ of the laser irradiated to the ionizing radiation curing resin, the pattern of the contracted microstructure produced in the ionizing radiation curing resin can be controlled. When the incident angle θ of the excimer laser is close to 0 degrees, the pattern of the microstructure is isotropic relative to the laser irradiated part, and a random microstructure is produced. On the other hand, the larger the incident angle θ of the laser, the greater the anisotropy of the pattern of the microstructure relative to the laser irradiated part. The surface shape of the ionizing radiation curing resin contracted by the laser with an incident angle of 0 degrees is effective for improving (for example) fingerprint resistance, contamination resistance, and scratch resistance. This is because the adhesion, damage, gloss change, etc. of pollutants become less obvious through the random microstructure arranged in an isotropic manner. The interval (period) l of the microstructure formed by irradiating the laser at an incident angle of 0 degrees is approximately the same as the wavelength λ of the irradiated excimer laser. In addition, when the incident angle θ is changed, the shape of the microstructure changes while maintaining the vertical stripe pattern. The interval l is based on the incident angle θ of the laser and is obtained by the following formula (3).
[0068] l=λ / cosθ···(3)
[0069] As the ionizing radiation curing resin constituting the first surface protection layer 13, for example, an ultraviolet curing resin can be used. As the ultraviolet curing resin, for example, (meth) acrylic resin, silicone resin, polyester resin, urethane resin, amide resin, epoxy resin can be used. The ultraviolet curing resin can be any of a water-based resin or a non-aqueous (organic solvent-based) resin.
[0070] The first surface protection layer 13 may contain inorganic particles. As inorganic particles, for example, microparticles formed by inorganic materials such as silicon dioxide, glass, aluminum oxide, titanium dioxide, zirconium oxide, calcium carbonate, and barium sulfate can be listed. Preferably, the amount of inorganic particles added in the first surface protection layer 13 is more than 0 mass% and less than 5 mass%, preferably more than 0 mass% and less than 3 mass%, more preferably more than 0 mass% and less than 1 mass%, and further preferably in the range of more than 0.1 mass% and less than 0.5 mass%. The first surface protection layer 13 is preferably preferably in the range of more than 0.1 mass% and less than 0.5 mass% by containing the above-mentioned amount of inorganic particles. The wear resistance and scratch resistance of the first surface protection layer 13 are improved. In addition, when inorganic particles are contained in the first surface protection layer 13, the scratch resistance is improved compared with the case where no inorganic particles are contained, but when the content of inorganic particles is too much, the inorganic particles fall off from the surface of the first surface protection layer 13, or have an adverse effect on the fingerprint resistance of fingerprint attachment, etc. Therefore, the amount of inorganic particles added is preferably more than 0 mass% and less than 3 mass%.
[0071] As required, for example, one or more additives selected from colorants, matting agents, fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, antistatic agents, slip agents, flame retardants, antibacterial agents, mildewproof agents, friction reducers, and light scattering agents can be added to the first surface protection layer 13. However, the first surface protection layer 13 does not contain a gloss regulator that reduces oleophobicity and makes fingerprints easily attached.
[0072] The first surface protection layer 13 only needs to completely cover the colored pattern layer 12, and can function as a surface protection layer over the entire surface of the decorative sheet 1. In addition, the density of the first surface protection layer 13 can be adjusted according to the target gloss and performance.
[0073] The thickness of the first surface protective layer 13 is preferably in the range of 1.0 μm to 50 μm. By making the thickness of the first surface protective layer 13 within the above range, the design can be protected by protecting the raw material layer 11 and the colored pattern layer 12 to prevent damage. When the thickness of the first surface protective layer 13 is 1.0 μm or more, it can fully have the functions such as wear resistance required as a surface protective layer. In addition, when the thickness of the first surface protective layer 13 is 50 μm or less, the first surface protective layer 13 will not become unnecessarily thick, thereby having the effect of not excessively increasing the manufacturing cost.
[0074] Although such a decorative sheet 1 does not contain a gloss regulator (matting additive), the glossiness is less than 5.0, thus becoming a decorative sheet with extremely low glossiness. In conventional decorative sheets, when the glossiness of a decorative sheet having a surface protective layer is about 8 or less, the content of the gloss regulator in the surface protective layer is high, so that the surface protective layer becomes turbid. Therefore, the color and pattern of the colored pattern layer may not be clearly expressed, or the design of the decorative sheet may be reduced. In addition, in the case of obtaining a decorative sheet with a glossiness close to 0, the content of the gloss regulator in the surface protective layer is higher, so when forming the surface protective layer, it is difficult to form a surface protective layer with a smooth surface without generating streaks, spots, etc.
[0075] A decorative sheet with a low gloss of 5.0 or less, preferably 2.0 or less, can be obtained while maintaining the same performance of the decorative sheet 1 as a decorative sheet having a gloss of 20±3 or more. Here, "gloss" is a measured value when measured at an incident angle of 60 degrees using a gloss meter gloss measuring device. Therefore, a decorative sheet 1 with high oleophobicity and difficult fingerprint adhesion can be obtained while maintaining the performance required as a decorative sheet 1.
[0076] (1.2) Method for manufacturing decorative sheet
[0077] A resin film is used as the raw material layer 11, and a desired color ink is printed on the raw material layer 11 to form the coloring layer 12A. Next, a desired color ink is printed in a desired pattern on the coloring layer 12A to form the pattern layer 12B.
[0078] Subsequently, an ionizing radiation curing resin is applied to the colored layer 12A (colored pattern layer 12) formed with the pattern layer 12B. At this time, the amount of the ionizing radiation curing resin applied is at least enough to completely cover the colored pattern layer 12, and can be adjusted according to the target gloss and performance, for example, preferably 2.0 g / m 2 Above 20g / m 2 Below left and right.
[0079] Then, the surface coated with the ionizing radiation curing resin is irradiated with a first ionizing radiation having an energy that can cut at least one of a carbonyl bond and a carbon-carbon bond to shrink the surface of the ionizing radiation curing resin. The first ionizing radiation can be a single ionizing radiation having a predetermined wavelength, or a plurality of ionizing radiations having different wavelengths. As the first ionizing radiation, for example, an excimer laser having high energy can be cited. The medium of the excimer laser can be any medium (discharge gas) used in the past, as long as it has an energy that can cut at least one of a carbonyl bond and a carbon-carbon bond. As the discharge gas, a rare gas such as Xe, Ar, Kr, or a mixed gas of a rare gas such as ArBr, ArF, KrCl, XeI, XeCl, XeBr, KrBr, KrF and a halogen gas can be used. The wavelength (center wavelength) of excimer laser varies depending on the medium, for example, it has wavelengths of about 172nm (Xe), about 126nm (Ar), about 146nm (Kr), about 165nm (ArBr), about 193nm (ArF), about 222nm (KrCl), about 253nm (XeI), about 308nm (XeCl), about 283nm (XeBr), about 207nm (KrBr), and about 248nm (KrF).
[0080] By irradiating the ionizing radiation curing resin with high energy, a ridge-like concavo-convex shape is formed on the surface of the ionizing radiation curing resin. At this time, the shrinkage rate of the ionizing radiation curing resin is adjusted by adjusting the resin coating amount of the ionizing radiation curing resin and the ionizing radiation irradiation time, thereby adjusting the final gloss of the finished decorative sheet 1.
[0081] When forming a ridge-like concave-convex shape, by changing the type of the first ionizing radiation irradiated on the ionizing radiation curing resin, the tactile feel of the surface of the decorative sheet 1 and the visual effect obtained can be changed. For example, the ionizing radiation curing resin is irradiated with a first ionizing radiation with a wavelength of about 250nm, and then irradiated with a first ionizing radiation with a wavelength of about 172nm to form a ridge-like concave-convex shape, and then the ionizing radiation curing resin is cured. In this way, the tactile feel (hand feel) of the decorative sheet 1 can be adjusted. In addition, for example, the ionizing radiation curing resin can be irradiated with a first ionizing radiation with a wavelength of about 172nm to form a ridge-like concave-convex shape, and then the ionizing radiation curing resin is cured. In this way, a decorative sheet 1 with a smooth surface and low gloss or a decorative sheet 1 with a glossy matte effect (visual embossed feeling) on the surface can be obtained.
[0082] Subsequently, the shrunk ionizing radiation curing resin is irradiated with a second ionizing radiation that cures the ionizing radiation curing resin, so that the ionizing radiation curing resin having a concavo-convex shape on the surface is cured. As the second ionizing radiation, for example, ultraviolet rays with a wavelength of less than 400nm can be cited. The ionizing radiation that cures the ionizing radiation curing resin has a wide band (i.e., a broad spectrum) within a range of less than 400nm.
[0083] Thus, the first surface protection layer 13 is formed.
[0084] As described above, the decorative sheet 1 including the first surface protection layer 13 having the core portion 13A and the ridge portion 13B provided to protrude in a ridge shape from one surface (upper surface) of the core portion 13A is formed.
[0085] (1.3) Modification
[0086] (1.3.1) Modification 1
[0087] In the decorative sheet of the first embodiment, the first surface protection layer 13 is formed of one layer, that is, formed by irradiating the surface of one layer of ionizing radiation curing resin with ionizing radiation, but the present invention is not limited to such a configuration.
[0088] For example, the decorative sheet 1A may be a multi-layer first surface protection layer 13. That is, the first surface protection layer 13 may be a layer of the same ionizing radiation curing resin or a layer of different ionizing radiation curing resin, and a concavo-convex shape is formed on the surface. However, it is important that the outermost layer of the first surface protection layer 13 has a concavo-convex shape formed by shrinking the ionizing radiation of the specific wavelength.
[0089] (1.3.2) Modification 2
[0090] In the decorative sheet of the first embodiment, the structure in which the raw material layer 11 is formed of a single resin film has been described, but the present invention is not limited to this structure.
[0091] For example, Figure 6As shown, instead of a layer of raw material layer 11, a decorative sheet 1B having a first film layer 11A and a second film layer 11B may be provided. The first film layer 11A and the second film layer 11B may be resin films formed of the same resin material, or may be resin films formed of different resin materials. For example, the first film layer 11A may be a polyethylene film, and the second film layer 11B may be a polypropylene film. In this case, it is preferred that a colored pattern layer 12 is provided on the first film layer 11A, and an adhesive resin layer 14 and a second film layer 11B are stacked on the colored pattern layer 12. In addition, the first surface protection layer 13 is preferably provided on the second film layer 11B. By such a stacked structure, it is possible to prevent the colored pattern layer 12 from being exposed, thereby reducing the wear resistance, scratch resistance, stain resistance and weather resistance. When the colored pattern layer 12 is exposed, the weather resistance is particularly prone to reduction. Therefore, when the decorative sheet is required to have high weather resistance, a decorative sheet 1B using films (first film layer 11A and second film layer 11B) as raw material layers and sandwiching a colored pattern layer 12 between the films is preferred.
[0092] The first film layer 11A and the second film layer 11B have the function of two layers as raw material layers. The total thickness of the first film layer 11A and the second film layer 11B functioning as raw material layers is preferably in the range of 50 μm to 250 μm, and more preferably in the range of 70 μm to 200 μm. When the total thickness of the first film layer 11A and the second film layer 11B is within the above range, the lamination suitability can be improved and cracks generated in the bending portion of the sheet can be reduced.
[0093] It should be noted that the film layer that functions as the raw material layer may be three or more layers.
[0094] (1.3.3) Modification 3
[0095] In the decorative sheet of the first embodiment, the structure in which the raw material layer 11 is formed of one layer of paper material has been described, but the present invention is not limited to such a structure.
[0096] For example, Figure 7 As shown, instead of the single raw material layer 11, the decorative sheet 1C may be provided with a laminated raw material layer 11' in which a first paper material 11C, a moisture-proof resin layer 11D, and a second paper material 11E are laminated in this order.
[0097] The moisture-proof resin layer 11D is made of, for example, polyethylene resin, etc. In this case, the moisture permeability can be finely adjusted by the type of resin material constituting the moisture-proof resin layer 11D and the thickness of the moisture-proof resin layer 11D, and the effect of suppressing the warping of the moisture-proof resin layer 11D can be obtained.
[0098] The first paper material 11C, the moisture-proof resin layer 11D, and the second paper material 11E have the function of three layers as raw material layers. The total thickness of the first paper material 11C, the moisture-proof resin layer 11D, and the second paper material 11E functioning as raw material layers is preferably in the range of 50 μm to 250 μm, and more preferably in the range of 70 μm to 200 μm. When the total thickness of the first paper material 11C and the second paper material 11E is within the above range, the lamination suitability can be improved and cracks generated in the bent portion of the sheet can be reduced.
[0099] In addition, the paper material functioning as the raw material layer may be a layer of three or more layers laminated via a moisture-proof resin layer.
[0100] (1.3.4) Modification 4
[0101] In the decorative sheet of the first embodiment, the configuration in which the first surface protection layer 13 is formed on the colored pattern layer 12 has been described, but the present invention is not limited to this configuration.
[0102] For example, Figure 8 As shown, the decorative sheet 1D may be provided with a transparent layer 15 between the colored pattern layer 12 and the first surface protection layer 13. By providing the transparent layer 15, similarly to the decorative sheet 1B of the second modification, the colored pattern layer 12 can be prevented from being exposed, thereby reducing the wear resistance, scratch resistance, stain resistance and weather resistance.
[0103] The resin material constituting the transparent layer 15 may be, for example, a thermosetting resin, or may be an acrylic resin, a silicone resin, a polyester resin, a urethane resin, an amide resin, or an epoxy resin, etc. In addition, an adhesive resin layer may be provided under the transparent layer 15 .
[0104] Alternatively, the raw material layer 11 may be made of a polyolefin film such as a polyethylene film or a polypropylene film.
[0105] <Effects of the First Embodiment>
[0106] The decorative sheet 1 according to the present embodiment has the following effects.
[0107] (1) The decorative sheet 1 of the present embodiment includes the first surface protection layer 13 having a concavo-convex shape formed on the surface.
[0108] According to this configuration, even if the first surface protective layer 13 does not contain a gloss regulator (matting additive), the gloss (glossiness) of the first surface protective layer 13 can be adjusted. The gloss regulator reduces the oleophobicity of the layer formed by the resin material, so fingerprints are easily attached. The first surface protective layer 13 does not contain a gloss regulator, so it does not absorb oil, and the oleophobicity is relatively improved. Therefore, in various scenes during on-site construction, when assembling furniture, and in the daily life of residents, the decorative sheet 1 having the first surface protective layer 13 is difficult to be attached with fingerprints.
[0109] (2) The decorative sheet 1 of the present embodiment includes the first surface protection layer 13 having a concavo-convex shape formed on the surface.
[0110] According to this configuration, the oil repellency of the first surface protection layer 13 is improved, and adsorption of oil stains and contaminants on the surface of the decorative sheet 1 can be suppressed.
[0111] (3) The decorative sheet 1 of the present embodiment includes the first surface protection layer 13 that does not contain a gloss adjuster.
[0112] According to this configuration, when the surface of the decorative sheet 1 is scratched, the particles of the gloss adjuster do not fall off, and gloss changes and scratches are unlikely to occur on the surface of the decorative sheet 1 .
[0113] (4) The decorative sheet 1 of the present embodiment includes the first surface protection layer 13 that does not contain a gloss adjuster.
[0114] According to this configuration, the content of the additive in the first surface protective layer 13 can be reduced, so that the first surface protective layer 13 can be prevented from becoming cloudy, and the first surface protective layer 13 can be easily formed.
[0115] 2. Second Implementation
[0116] use Fig. 9 A decorative sheet according to a second embodiment of the present disclosure will be described.
[0117] Fig. 9 It is a cross-sectional view for explaining a configuration example of the decorative sheet 2 according to the second embodiment of the present disclosure.
[0118] The decorative sheet 2 includes: a raw material layer 11, a colored pattern layer 12, a first surface protection layer 13, and a second surface protection layer 26. The decorative sheet 2 is composed of the raw material layer 11, the colored pattern layer 12, the first surface protection layer 13, and the second surface protection layer 26 stacked in sequence. That is, the decorative sheet 2 is different from the decorative sheet 1 according to the first embodiment in that the second surface protection layer 26 is provided on the first surface protection layer 13.
[0119] The second surface protection layer 26 will be described below. It should be noted that the layers other than the second surface protection layer 26 (raw material layer 11, colored pattern layer 12, and first surface protection layer 13) have the same structure as the layers of the decorative sheet 1, and thus description thereof will be omitted.
[0120] (2.1) Basic composition of decorative sheets
[0121] <Second surface protection layer>
[0122] The second surface protection layer 26 is provided on a portion of the concavo-convex shape forming surface of the first surface protection layer 13. The second surface protection layer 26 is a layer that is partially formed on the first surface protection layer 13 to generate a gloss difference with the first surface protection layer 13, thereby visually expressing an embossed feeling through a gloss matte effect.
[0123] The second surface protection layer 26 is formed of a resin material such as an ionizing radiation curing resin or a thermosetting resin, and is preferably formed of an ionizing radiation curing resin.
[0124] As the ionizing radiation curing resin, the same material as that of the first surface protective layer 13 can be used.
[0125] As the thermosetting resin, from the viewpoint of the difference in gloss with the first surface protection layer 13 , for example, a thermosetting resin having a urethane bond such as a two-component curable urethane resin is preferably used.
[0126] As the two-component curable urethane resin, for example, a urethane resin containing polyol as a main component and isocyanate as a crosslinking agent (curing agent) can be used.
[0127] The polyol may be a polyol having two or more hydroxyl groups in the molecule, and for example, polyethylene glycol, polypropylene glycol, acrylic polyol, polyester polyol, polyether polyol, polycarbonate polyol, and polyurethane polyol can be used.
[0128] In addition, as isocyanate, a polyisocyanate having two or more isocyanate groups in the molecule can be used. As polyisocyanate, for example, aromatic isocyanates such as 2,4-toluene diisocyanate, xylene diisocyanate, and 4,4′-diphenylmethane diisocyanate, or aliphatic (or alicyclic) isocyanates such as 1,6-hexamethylene diisocyanate, isophorone diisocyanate, hydrogenated toluene diisocyanate, and hydrogenated diphenylmethane diisocyanate can be used. In addition, adducts or polymers of the above-mentioned various isocyanates can be used. For example, there are adducts of toluene diisocyanate, toluene diisocyanate trimers, etc. It should be noted that among the above-mentioned isocyanates, aliphatic (or alicyclic) isocyanates are preferred in terms of being able to make weather resistance and heat yellowing resistance good, for example, 1,6-hexamethylene diisocyanate can be used.
[0129] The second surface protection layer 26 is partially formed on the first surface protection layer 13, and the coating area can be adjusted according to the design and target performance. The second surface protection layer 26 is preferably arranged in a manner that covers more than 10% and less than 90% of the surface of the first surface protection layer 13. In the case of showing a glossy matte effect (visual embossing), it is preferably arranged in a manner that covers more than 10% and less than 80% of the surface of the first surface protection layer 13. In addition, in the case where the decorative sheet 2 is required to improve the scratch resistance, stain resistance, and oleophobicity, the second surface protection layer 26 is preferably arranged in a manner that covers more than 10% and less than 80% of the surface of the first surface protection layer 13, and more preferably arranged in a manner that covers more than 10% and less than 30%.
[0130] The raw material layer 11 , the colored pattern layer 12 , and the first surface protection layer 13 of the decorative sheet 2 are formed in the same manner as the decorative sheet 1 .
[0131] The second surface protection layer 26 is formed by, for example, applying a resin material on the first surface protection layer 13 by screen printing, offset printing, gravure printing, or the like, and curing the resin material.
[0132] Thus, the decorative sheet 2 is formed.
[0133] (2.2) Modification
[0134] In the decorative sheet 2, the pattern layer 12B of the colored pattern layer 12 can be synchronized with the gloss matte effect (visual embossed feeling) produced by the gloss difference between the first surface protection layer 13 and the second surface protection layer 26. Compared with the gloss matte effect only produced by the gloss difference between the first surface protection layer 13 and the second surface protection layer 26, the decorative sheet 1 in which the pattern layer 12B is synchronized with the visual embossed feeling can produce a more excellent visual embossed feeling.
[0135] <Effects of the Second Embodiment>
[0136] In addition to the effects described in the first embodiment, the decorative sheet 2 according to the present embodiment has the following effects.
[0137] (5) The decorative sheet 2 of the present embodiment has the second surface protection layer 26 having relatively high glossiness on a part of the concavo-convex shape forming surface of the low-gloss first surface protection layer 13 .
[0138] According to this configuration, it is possible to obtain a decorative sheet 2 in which the first surface protection layer 13 and the second surface protection layer 26 do not become cloudy and have a glossy matte effect (visual embossed feeling).
[0139] 3. Third Implementation
[0140] use Fig.10 A decorative board according to a third embodiment of the present disclosure will be described.
[0141] Fig.10 It is a cross-sectional view for explaining a configuration example of a decorative board 30 according to a third embodiment of the present disclosure.
[0142] The decorative board 30 includes a decorative sheet 1 and a base material 31. The decorative board 30 is formed by laminating the base material 31, the raw material layer 11, the colored pattern layer 12, and the first surface protection layer 13 in this order.
[0143] It should be noted that the decorative plate 30 may include the decorative sheet 2 instead of the decorative sheet 1. In addition, the decorative plate 30 may include decorative sheets 1A to 1D which are modified examples of the decorative sheet 1 instead of the decorative sheet 1.
[0144] The following describes the substrate 31. It should be noted that the layers other than the substrate 31 (including the raw material layer 11, the colored pattern layer 12, and the layers of the decorative sheet of the first surface protection layer 13) are the same as those described in the first embodiment and the second embodiment, and therefore the description thereof is omitted.
[0145] (3.1) Basic composition of decorative sheets
[0146] <Base material>
[0147] The substrate 31 is, for example, a wood substrate or medium density fiberboard (MDF). It may be a particle board, a metal substrate, a non-combustible substrate, a composite substrate composed of multiple materials, or a bright substrate. In addition, the substrate 31 may be a combination of plywood and MDF.
[0148] In addition, a primer layer, a concealing layer, or the like may be provided on the surface of the base material 31 facing the decorative sheet 1 .
[0149] Example
[0150] Hereinafter, the decorative sheet according to the present disclosure will be described with reference to examples.
[0151] In the examples, a decorative sheet having the configuration described in the first embodiment was produced and evaluated as described below.
[0152] <Example 1>
[0153] A 55 μm thick olefin film (manufactured by RIKEN TECHNOS CORP.) was used as a base material layer, and urethane ink (manufactured by Toyo Ink Co., Ltd.) was printed on the entire surface of one side of the base material layer to form a colored layer. Next, a pattern was printed on the colored layer using urethane ink to form a pattern layer.
[0154] Subsequently, a transparent olefin film different from the raw material layer was stacked as a transparent layer on the colored layer (colored pattern layer) formed with the pattern layer. Subsequently, an ionizing radiation curing resin was applied. As the ionizing radiation curing resin, a (meth) acrylic resin containing no gloss modifier was used. In addition, the coating amount of the ionizing radiation curing resin was set to 12 g / m 2 to completely cover the colored pattern layer.
[0155] After that, the surface of the ionizing radiation curing resin is irradiated with ionizing radiation (KrF excimer laser) with a wavelength of 250nm, and then irradiated with ionizing radiation (Xe excimer laser) with a wavelength of 172nm. As a result, the surface of the ionizing radiation curing resin is shrunk, thereby forming a concave-convex shape on the surface of the ionizing radiation curing resin. At this time, the ionizing radiation is irradiated at a linear speed of 10m / min. Subsequently, the ionizing radiation curing resin after the surface shrinkage is irradiated with ionizing radiation having a wide band (a band below 400nm). At this time, two UV lamps, gallium (Ga) lamp and mercury (Hg) lamp, are used. As described above, the ionizing radiation curing resin having a concave-convex shape on the surface is cured, thereby forming a decorative sheet provided with a first surface protective layer. The first surface protective layer formed is in such a shape that a ridge portion with a height of 7μm is formed on a core portion with a thickness of 20μm. Finally, a wooden substrate as a substrate is attached to the back of the raw material layer of the decorative sheet.
[0156] As described above, the decorative board of Example 1 was formed.
[0157] <Example 2>
[0158] As the raw material layer, the unit weight is 30g / m 2The decorative board of Example 2 was formed in the same manner as Example 1 except that the transparent layer was not provided on the patterned resin layer but the first surface protection layer was directly formed. It should be noted that in the decorative board of Example 2, as the first surface protection layer, the same amount of ionizing radiation curing resin as that of Example 1 was applied, but since the raw material layer was paper, part of the ionizing radiation curing resin penetrated into the raw material layer, and therefore the thickness of the first surface protection layer was slightly thinner than that of the decorative board of Example 1. In addition, the decorative board of Example 2 was formed by the raw material layer and the substrate being integrated and cured by the first surface protection layer penetrating into the raw material layer.
[0159] <Example 3>
[0160] As the raw material layer, the unit weight is 30g / m 2 The amount of ionizing radiation curing resin applied was set to 25 g / m 2 , except for this, the decorative plate of Example 3 was formed in the same manner as Example 2.
[0161] <Example 4>
[0162] A decorative board of Example 4 was formed in the same manner as in Example 1, except that a high chemical resistance / high scratch resistance ionizing radiation curing resin having better chemical resistance and scratch resistance than the material used in Example 1 was used as the ionizing radiation curing resin forming the first surface protection layer.
[0163] <Example 5>
[0164] The thickness of the raw material layer was set to 50 μm, and the first surface protection layer was directly formed on the patterned resin layer without providing a transparent layer, and the second surface protection layer was formed on a part of the concavo-convex shape forming surface of the first surface protection layer using the same material as the first surface protection layer. The decorative board of Example 5 was formed in the same manner as in Example 1. The decorative board of Example 5 was a decorative board in which a visual embossing sense due to a glossy matte effect was exhibited on the surface of the decorative sheet by the second surface protection layer.
[0165] <Comparative Example 1>
[0166] As an ionizing radiation curing resin, an acrylic resin (manufactured by DIC Graphics Corporation) containing 15% by mass of a gloss regulator is used. The ionizing radiation curing resin is applied to the colored pattern layer, and then the ionizing radiation curing resin is cured by irradiating it with ionizing radiation of a wide band (a band below 400 nm) without forming a concave-convex shape, thereby forming a first surface protective layer with a smooth surface, thereby forming a decorative sheet.
[0167] A decorative board of Comparative Example 1 was formed in the same manner as in Example 2 except for the above.
[0168] <Evaluation>
[0169] Each of the decorative boards of Examples and Comparative Example 1 was subjected to the following evaluations.
[0170] (A) Design: Evaluation of the clarity of the colored pattern layer
[0171] Whether the color / pattern of the colored pattern layer is clearly visible was visually confirmed from the surface side (decorative sheet side) of the decorative plate of Example 1 and Comparative Example 1. At this time, the case where the colored pattern layer is clearly visible was evaluated as "A", and the case where the colored pattern layer is not clearly visible was evaluated as "C".
[0172] (B) Design: Evaluation of white turbidity of first surface protective layer
[0173] Whether or not white turbidity was generated in the first surface protective layer was visually confirmed from the surface side (decorative sheet side) of the decorative board of Example 1 and Comparative Example 1. At this time, the case where white turbidity was not generated in the first surface protective layer was evaluated as "A", and the case where white turbidity was generated in the first surface protective layer was evaluated as "C".
[0174] (C) Fingerprint resistance: Wiping performance evaluation
[0175] The 60-degree specular gloss of the surface (surface protection layer) of the decorative plate of each embodiment and comparative example was measured using a gloss meter (GS-4K manufactured by Suga Test Instruments Co., Ltd.) as the initial gloss. Subsequently, the anti-fingerprint evaluation liquid was attached to the surface protection layer, and the specular gloss of the portion to which the anti-fingerprint evaluation liquid was attached was measured as the gloss before wiping. Then, the anti-fingerprint evaluation liquid attached to the surface of the decorative sheet was wiped, and the specular gloss of the portion after the anti-fingerprint evaluation liquid was wiped off was measured as the gloss after wiping. Here, a higher fatty acid was used as the anti-fingerprint evaluation liquid.
[0176] Then, based on the measured initial glossiness, glossiness before wiping, and glossiness after wiping, the post-wiping evaluation rate (%) was calculated according to the following formula (4).
[0177] Evaluation rate after wiping (%) = (gloss after wiping / initial gloss) × 100 (4)
[0178] At this time, the case where the evaluation rate after wiping (%) is greater than 70% and less than 250% is evaluated as "A", the case where the evaluation rate after wiping (%) is greater than 50% and less than 70%, or greater than 250% and less than 300% is evaluated as "B", and the case where the evaluation rate after wiping (%) is less than 50%, or greater than 300% is evaluated as "C".
[0179] (D) Fingerprint resistance: Evaluation of the slide angle
[0180] The decorative plates of the embodiments and comparative examples are arranged on a horizontal measuring table, and a certain amount of measuring liquid is placed on the surface of the decorative sheet of the decorative plate. Next, the measuring table is tilted at a certain speed, and the inclination of the measuring table when the droplet begins to slide is measured as the sliding angle. The measuring liquid uses n-hexadecane, and a droplet of 5 μl is dripped on the surface of the decorative sheet. At this time, the case where the sliding angle is less than 20 degrees is evaluated as "A", the case where the sliding angle is greater than 20 degrees and less than 30 degrees is evaluated as "B", and the case where the sliding angle is greater than 30 degrees is evaluated as "C". That is, it is evaluated as follows: the lower the sliding angle, the higher the liquid repellency, and the more difficult it is for fingerprints to remain.
[0181] (E) Anti-fouling property: Evaluation of oleophobicity
[0182] Hand oil was attached to the decorative sheet side surface of the decorative plate of each example and comparative example, and then the hand oil was wiped off with a cloth, and the state of the decorative sheet surface after wiping was visually confirmed. At this time, the case where the hand oil on the decorative sheet surface was easily wiped off was evaluated as "A", and the case where the hand oil on the decorative sheet surface could not be wiped off and oil stains remained was evaluated as "C".
[0183] (F) Anti-fouling property: Evaluation of ink anti-fouling property
[0184] The stain resistance of the ink was evaluated by using a stain A test specified in the Japanese Agricultural Standards (JAS) for plywood, using blue ink, black quick-drying ink and red crayon to draw lines with a width of 10 mm on the surface of the decorative sheet of each embodiment and comparative example, leaving them for 4 hours, and then rubbing the lines of the blue ink, black quick-drying ink and red crayon with ethanol contained in a cloth.
[0185] At this time, the case where the threads of each color can be easily wiped off is evaluated as "A", the case where part of the threads of each color can be wiped off but some stains remain is evaluated as "B", and the case where the threads of each color cannot be wiped off is evaluated as "C".
[0186] (G) Scratch resistance test: Hoffman scratch test (gloss change)
[0187] The decorative sheet surface of the decorative board of each embodiment and comparative example was subjected to a scratch test using a Hoffman scratch hardness tester (manufactured by GARDCO) to confirm the gloss change on the decorative sheet surface. In the scratch test, the heaviest load at which no gloss change occurred on the surface of the decorative sheet was measured. After the test, the portion of the surface where gloss change occurred was confirmed.
[0188] At this time, the case where no gloss change occurred on the surface under a load of 200g was evaluated as "A", the case where gloss change occurred between a load of 125g or more and less than 200g was evaluated as "B", and the case where gloss change occurred under a load less than 125g was evaluated as "C".
[0189] (H) Damage resistance / scratch resistance test: Hoffman scratch test (breakage)
[0190] The decorative sheet surface of the decorative board of each embodiment and comparative example was subjected to a scratch test using a Hoffman scratch hardness tester (manufactured by GARDCO) to confirm the damage on the decorative sheet surface. In the scratch test, the heaviest load at which the surface of the decorative sheet did not produce damage or the like was measured. After the test, the portion where the gloss change and damage or the like occurred on the surface was confirmed.
[0191] At this time, the case where no surface damage occurred under a load of 400g was evaluated as "A", the case where damage occurred between a load of 200g or more and less than 400g was evaluated as "B", and the case where damage occurred under a load of less than 200g was evaluated as "C".
[0192] (I) Scratch resistance test: pencil hardness test
[0193] The decorative sheet surface of the decorative board of each example and comparative example was measured by a pencil scratch test to determine the hardness of the hardest pencil that did not scratch the decorative sheet surface (pencil hardness). The scratch hardness test was performed in accordance with old JIS K5400.
[0194] At this time, the case where the pencil hardness was harder than H was evaluated as "A", and the case where the pencil hardness was softer than F was evaluated as "B".
[0195] (J) Damage resistance / scratch resistance test: coin scratch test
[0196] For the decorative sheet surface of the decorative plate of each embodiment and comparative example, a coin scratch test was performed, in which a 10-yen coin was placed against the surface of the decorative sheet and scratched at a certain speed to measure the maximum load at which no continuous scratches were produced on the surface. It should be noted that in the coin scratch test, the test was started from a load of 500g, and the load was gradually increased to 1Kg and 2Kg.
[0197] At this time, the maximum load at which no continuous scratches were generated on the surface was evaluated as "A" when it was 1 kg or more, "B" when it was 500 g or more and less than 1 kg, and "C" when it was less than 500 g.
[0198] (K) Scratch resistance test: Steel wool friction test
[0199] The decorative sheet surface of the decorative board of each example and comparative example was rubbed back and forth 20 times with steel wool under a load of 500 g, and scratches on the decorative sheet surface and changes in gloss were visually observed.
[0200] At this time, the case where the surface had no scratches or gloss changes was evaluated as "A", the case where the surface had slight scratches or gloss changes was evaluated as "B", and the case where the surface had significant scratches or gloss changes was evaluated as "C".
[0201] (L) Printability: Evaluation of printability of the first surface protective layer
[0202] The streaks and spots generated when the first surface protective layer of the decorative board of each example and comparative example was formed were visually confirmed.
[0203] At this time, the case where no streaks or spots were generated in the first surface protection layer was evaluated as “A”, and the case where streaks or spots were generated in the first surface protection layer was evaluated as “B”.
[0204] The following Table 1 shows the extracts of the configurations and evaluation results of each Example and Comparative Example. It should be noted that "A" is the most preferable evaluation in each evaluation.
[0205] [Table 1]
[0206]
[0207] As shown in Table 1, in the decorative sheet of Example 1 having projections and depressions formed thereon, all evaluations were the most preferred evaluation results, wherein the projections and depressions were formed by irradiating the surface of a first surface protective layer that does not contain a gloss regulator and is formed by an ionizing radiation-curing resin with ionizing radiation of a predetermined wavelength to shrink the ionizing radiation-curing resin.
[0208] On the other hand, in the decorative sheet of Comparative Example 1 in which the first surface protective layer formed of an ionizing radiation curing resin and containing a gloss regulator has no surface irregularities, the color / pattern of the colored pattern layer is not clearly visible on the surface of the decorative sheet, and white turbidity of the first surface protective layer is also observed.
[0209] In addition, the various colors of ink and crayon lines on the surface of the decorative sheet could not be easily wiped off in the decorative sheet of Comparative Example 1. In addition, the hardness of the first surface protective layer was relatively low, resulting in scratches or gloss changes, and streaks / spots were also generated in the first surface protective layer.
[0210] According to the above evaluation results, it was confirmed that in a decorative sheet formed with projections and depressions, the projections and depressions were formed by irradiating the surface of the first surface protective layer formed of an ionizing radiation curing resin without a gloss modifier with ionizing radiation of a predetermined wavelength to shrink the ionizing radiation curing resin, and the decorative sheet had high fingerprint resistance compared with a decorative sheet without such a first surface protective layer. In addition, it was confirmed that in addition to fingerprint resistance, the decorative sheet also had high performance in design, stain resistance, scratch resistance / abrasion resistance, and printability.
[0211] The scope of the present disclosure is not limited to the exemplary embodiments described in the drawings, but includes all embodiments having equivalent effects to the purpose of the present disclosure. In addition, the scope of the present disclosure is not limited to the combination of features of the invention defined by the claims, but can be defined by all desired combinations of specific features among all disclosed features.
[0212] Explanation of symbols
[0213] 1,1A,1B,1C,1D,2 Decorative sheet
[0214] 11 Raw material layer
[0215] 11' stacked raw material layer
[0216] 11A First film layer
[0217] 11B Second film layer
[0218] 11C First Paper Material
[0219] 11D moisture-proof resin layer
[0220] 11E Second paper material
[0221] 12 Coloring pattern layer
[0222] 12A Coloring layer
[0223] 12B pattern layer
[0224] 13. First surface protective layer
[0225] 13A Core
[0226] 13B Ridge
[0227] 14 Adhesive resin layer
[0228] 15 Transparent Layer
[0229] 26 Second surface protection layer
[0230] 30 Decorative panels
[0231] 31 Substrate
Claims
1. A method for manufacturing a decorative sheet, The first ionizing radiation having energy capable of cutting polymer chains of the ionizing radiation curing resin is irradiated onto the surface of the applied ionizing radiation curing resin to shrink the surface of the ionizing radiation curing resin, thereby forming a concavo-convex shape on the surface of the ionizing radiation curing resin, wherein the incident angle θ of the first ionizing radiation is 0 degrees. The ionizing radiation curing resin is cured by irradiating the shrunk ionizing radiation curing resin with a second ionizing radiation that cures the ionizing radiation curing resin, thereby forming a first surface protective layer having a core portion and a ridge portion protruding from one surface of the core portion in a ridge shape, As the first ionizing radiation, a first excimer laser and a second excimer laser are sequentially irradiated, The first excimer laser is a KrF excimer laser with a wavelength of 250 nm. The second excimer laser is a Xe excimer laser having a wavelength of 172 nm.
2. A decorative sheet manufactured by the method for manufacturing a decorative sheet according to claim 1, the decorative sheet comprising: Raw material layer, a colored pattern layer disposed on one surface of the raw material layer, and The first surface protection layer is provided on the surface of the colored pattern layer opposite to the raw material layer, has a core portion and a ridge portion provided to protrude from one surface of the core portion in a ridge shape, and has a concavo-convex shape formed on the surface. The height of the ridge portion is not less than 7 μm and not more than 15 μm, and the period between adjacent ridge portions is not more than 50 μm. The concavoconvex shape exhibits isotropy, The first surface protection layer is formed of an ionizing radiation curable resin.
3. The decorative sheet according to claim 2, in, The ridges have a different composition than the core.
4. The decorative sheet according to claim 2 or 3, in, The ridge portion and the core portion are integrally formed of a resin material, The ridge portion has a composition in which a ratio of a carbonyl bond to a carbon-carbon bond contained in the resin material is lower than that of the core portion.
5. The decorative sheet according to claim 4, in, The ridge portion has a composition in which a ratio of a carbonyl bond and a carbon-carbon bond contained in the resin material is reduced by 10% or more compared with the core portion.
6. The decorative sheet according to claim 2 or 3, in, The ridge portion has a higher cross-link density than the core portion.
7. The decorative sheet according to claim 2 or 3, in, The surface of the ridge portion has a curved shape in a cross-sectional view.
8. The decorative sheet according to claim 2 or 3, in, The coating amount of the ionizing radiation curing resin is 2.0 g / m 2 Above 20g / m 2 the following.
9. The decorative sheet according to claim 8, in, The ionizing radiation curable resin is a (meth)acrylic resin.
10. The decorative sheet according to claim 2 or 3, in, The first surface protection layer does not contain inorganic particles.
11. The decorative sheet according to claim 2 or 3, in, The first surface protection layer comprises inorganic particles, The amount of the inorganic particles added to the first surface protection layer is more than 0 mass % and less than 3 mass %.
12. The decorative sheet according to claim 2 or 3, in, A second surface protection layer is provided on a portion of the concavo-convex shape forming surface of the first surface protection layer.
13. The decorative sheet according to claim 12, in, The second surface protection layer is provided so as to cover 10% to 80% of the surface of the first surface protection layer.
14. The decorative sheet according to claim 2 or 3, in, The first surface protective layer does not contain a gloss regulator, The glossiness of the first surface protection layer is 5.0 or less.
15. A decorative panel comprising: The decorative sheet according to any one of claims 2 to 14; and A base material layer is provided on a surface of the raw material layer opposite to the colored pattern layer.
Citation Information
Patent Citations
Decorative plate
JP2001129959A
Process for scratch- and abrasion-resistant coating and physical matting of plastics substrates, more particularly polymethyl methacrylate, with nanocomposite coating material
CN102985469A
Article and active energy ray-curable resin composition
CN104364677A
Decorative sheet and decorative panel
CN107848253A
Periodical structure of crystal and method for forming the same
JP2004172424A