Catalyst composition and method for preparing isobutylene-isoprene copolymer using the same
The isobutene-isoprene copolymer is efficiently prepared in a wide temperature range by the composition of imidazolinium ionic catalyst and aluminum cocatalyst, which solves the defects of Lewis acid catalysts in the prior art and achieves environmentally friendly and efficient Butyl rubber preparation simplifies the process flow and improves product quality.
Patent Information
- Application Number
- CN202180009221.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-18
- Filing Date
- 2021-09-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-09-07
AI Technical Summary
The prior art uses Lewis acid catalysts when preparing butyl rubber, which has weak moisture resistance, strong corrosion, high investment equipment, difficulty in low temperature control, use of toxic solvents and production of highly toxic waste, resulting in unecotched preparation process and efficiency. Low.
The isobutylene-isoprene copolymer is efficiently prepared by cationic polymerization in a wide temperature range (-50°C to -10°C) using a composition of imidazolinium ionic catalyst and an aluminum cocatalyst. It uses halogen-free The solvent is then removed by physical filtration to simplify the process flow.
High polymerization conversion rate, economic feasibility and efficiency are improved, butyl rubber with high molecular weight and narrow molecular weight distribution is prepared, reducing environmental pollution, simplifying the process flow and reducing waste production.
Smart Images

Figure BDA0003746552010000021 
Figure BDA0003746552010000041 
Figure BDA0003746552010000051
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0120298 filed on September 18, 2020, the entire contents of which are incorporated into this specification by reference. Technical Field
[0004] The present invention relates to a catalyst composition comprising an imidazolinium ion catalyst and an aluminum co-catalyst, and a method for preparing an isobutylene-isoprene copolymer using the catalyst composition. Background Art
[0005] Butyl rubber (isobutylene-isoprene rubber, IIR) is an isobutylene-isoprene copolymer containing isobutylene and about 1% to 6% of isoprene, and has excellent chemical resistance, moisture resistance, electrical insulation, etc., and is therefore used as an adhesive composition, an adhesive sheet, etc. In addition, butyl rubber is used for crosslinking / compounding with other rubbers by undergoing an additional halogenation reaction on the double bond of isoprene and then used, and is characterized in that it does not show air permeability, and is therefore widely used in inner tubes and airtight layers of tires.
[0006] As a synthesis method used for polymerizing butyl rubber, cationic polymerization is generally used, and as a catalyst, a Lewis acid catalyst such as BF 3 and AlCl 3 Lewis acid catalysts are weak to moisture resistance, and if reacted with water, strong acids such as HCl and HF are generated, which are mixed into the product to cause defects that deteriorate the product quality. In addition, due to the strong corrosiveness of Lewis acid catalysts, high investment settings are required when designing the process in consideration of corrosion resistance.
[0007] Cationic polymerization is mostly carried out at low temperatures, and it is difficult to carefully control the polymerization temperature at around -100°C depending on the molecular weight of the butyl rubber to be prepared. Specifically, in order to increase the molecular weight of butyl rubber products having a medium molecular weight or above, polymerization is carried out after lowering the reaction temperature to an extremely low temperature of -100°C. In order to control the temperature, it is necessary to install and use an expensive ethylene refrigerator. In order to ensure safety, many refrigerators are designed as double-layer or triple-layer, which has the disadvantage of increasing investment costs.
[0008] In addition, in order to fully enhance the reactivity, toxic solvents such as methyl chloride (CH 3 Cl), dichloromethane (CH 2 Cl 2 ) and ethyl chloride (CH 3 CH 2Cl), they are halogen-containing solvents, which is considered a disadvantage.
[0009] In addition, in the quenching work after using Lewis acid catalysts, a large amount of organic bases such as NaOH, KOH, NaNH 4 and KNH 4 This organic base reacts with Lewis acids to form highly toxic wastes such as Na(BF 3 OH), Na(AlCl 3 OH), K(BF 3 OH) and K(AlCl 3 OH), and if the waste is washed, a large amount of waste water is generated.
[0010] The conventional method for preparing butyl rubber as described above has defects in many aspects, and there is still a need to develop a method for efficiently preparing butyl rubber using an environmentally friendly method.
[0011] [Prior art literature]
[0012] [Patent Document]
[0013] U.S. Patent Publication No. 2013-0178679 Summary of the invention
[0014] Technical issues
[0015] An object of the present invention is to provide a catalyst composition which can prepare an isobutylene-isoprene copolymer having a high polymerization conversion while controlling the number average molecular weight.
[0016] Another object of the present invention is to provide a method for preparing an isobutylene-isoprene copolymer using the catalyst composition.
[0017] Technical Solution
[0018] In order to solve the above-mentioned task, the present invention provides a catalyst composition comprising a catalyst represented by the following Formula 1 and a co-catalyst represented by the following Formula 2.
[0019] [Formula 1]
[0020]
[0021] In formula 1,
[0022] R is an alkyl group of 2 to 12 carbon atoms,
[0023] R 1 To R 6 are each independently a halogen group,
[0024] a to f are each independently an integer from 1 to 5,
[0025] [Formula 2]
[0026] (R a ) n Al(X) 3-n
[0027] In formula 2,
[0028] R a is a hydrocarbon group of 1 to 20 carbon atoms,
[0029] X is a halogen group,
[0030] n is an integer of 0-3.
[0031] In addition, the present invention provides a method for preparing an isobutylene-isoprene copolymer, comprising copolymerizing isobutylene and isoprene in the presence of the catalyst composition.
[0032] Beneficial Effects
[0033] The catalyst composition of the present invention is a combination of an imidazolinium ion catalyst and an aluminum co-catalyst having excellent catalyst activity. When the catalyst composition is used to prepare an isobutylene-isoprene copolymer, the isobutylene-isoprene copolymer can be prepared at a high polymerization conversion rate, the economic feasibility and efficiency of the preparation process can be improved, and a copolymer with a high molecular weight and a narrow molecular weight distribution can be prepared. DETAILED DESCRIPTION
[0034] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.
[0035] It should be understood that the words or terms used in the specification and claims of the present invention should not be understood as the meanings defined in commonly used dictionaries. It should also be understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best illustrate the invention, the words or terms should be understood to have meanings consistent with their meanings in the technical concept of the present invention.
[0036] <Catalyst composition>
[0037] The catalyst composition of the present invention is characterized by comprising a catalyst represented by the following Formula 1 and a co-catalyst represented by the following Formula 2.
[0038] [Formula 1]
[0039]
[0040] In formula 1,
[0041] R is an alkyl group of 2 to 12 carbon atoms,
[0042] R 1 To R 6 are each independently a halogen group,
[0043] a to f are each independently an integer from 1 to 5,
[0044] [Formula 2]
[0045] (R a ) n Al(X) 3-n
[0046] In formula 2,
[0047] R a is a hydrocarbon group of 1 to 20 carbon atoms,
[0048] X is a halogen group,
[0049] n is an integer of 0-3.
[0050] "Alkyl" may refer to a monovalent aliphatic saturated hydrocarbon and may include both: a straight chain alkyl group such as methyl, ethyl, propyl and butyl; and a branched chain alkyl group such as isopropyl, sec-butyl, tert-butyl and neopentyl. Specifically, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, sec-butyl, 1-methyl-butyl, 1-ethyl-butyl, pentyl, isopentyl, neopentyl, tert-pentyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, hexyl, isohexyl, 4-methylhexyl, 5-methylhexyl, heptyl, etc. may be used without limitation.
[0051] Specifically, R can be an alkyl group of 2 to 12 carbon atoms, an alkyl group of 2 to 8 carbon atoms, an alkyl group of 2 to 6 carbon atoms, an alkyl group of 2 to 4 carbon atoms, or an ethyl group. 1 To R 4 Each of R is independently a halogen group, specifically, F or Cl, for example, F, a to f are independently an integer of 1 to 5, an integer of 3 to 5, or an integer of 4 or 5. Most preferably, R 1 To R 4 A may be a fluorine group, and a to f may be 5.
[0052] More specifically, the catalyst represented by Formula 1 may be represented by the following Formula 1-1 or Formula 1-2 without limitation.
[0053] [Formula 1-1]
[0054]
[0055] [Formula 1-2]
[0056]
[0057] The catalyst of the present invention comprises an organic borate radical containing one or more halogen substituents with strong electron-withdrawing phenomenon in the phenyl group as an anion part, and the CB bond is strong. Therefore, although mixed with the aluminum-based cocatalyst of the present invention, the CB bond remains and the catalyst activity is not lost, so the catalyst is used for cationic polymerization to show excellent efficiency.
[0058] In addition, in the anionic part, two boron (B) groups bonded with three phenyls are included, and the feature of the structure is that imidazolinium is arranged on the bridge connecting two boron atoms. Due to comprising two B groups bonded with three phenyls, therefore, the structure is large in volume in space, and the imidazolinium bridge connecting two Bs has a bent structure and does not form a plane. Therefore, in three dimensions, even more parts can be occupied, and even larger volume structures can be obtained. Similarly, the bulky structure in the anionic part in the catalyst stabilizes the terminal cations of the chains polymerized in the cationic polymerization process of isobutylene and isoprene, to improve stability, and enables monomers to be continuously bonded to be polymerized, and does not end cationic polymerization. The isobutylene-isoprene copolymer prepared by this method can achieve high molecular weight.
[0059] On the contrary, in the case of including only one B group, the size of the anion part is relatively small, and if combined with the cation at the terminal of the polymer chain, a relatively unstable state is obtained compared with the case of using the catalyst represented by Formula 1. In this case, due to the instability of the terminal cation of the chain, the cationic polymerization is terminated prematurely, or chain transfer occurs, thereby causing a defect of preparing only a copolymer having a low molecular weight.
[0060] In addition, even if two B groups are contained, if imidazolinium is not set on the bridge connecting them, but a bridge with a linear and planar shape such as nitrile and azide is set, the anion part will become relatively small in space, the terminal cation of the chain will become unstable, and the reactivity will be significantly deteriorated.
[0061] The catalyst composition of the present invention includes a co-catalyst represented by Formula 2 together with a catalyst represented by Formula 1. Here, the co-catalyst represented by Formula 2 may refer to, for example, trialkylaluminum compounds, dialkylaluminum halide compounds, alkylaluminum dihalide compounds, aluminum trihalide compounds, and the like.
[0062] [Formula 2]
[0063] (R a ) n Al(X) 3-n
[0064] In formula 2,
[0065] R a is a hydrocarbon group of 1 to 20 carbon atoms,
[0066] X is a halogen group,
[0067] n is an integer of 0-3.
[0068] R a It may be an alkyl group of 1 to 12 carbon atoms, a cycloalkyl group of 3 to 12 carbon atoms, or an aryl group of 6 to 12 carbon atoms, preferably an alkyl group of 1 to 12 carbon atoms, an alkyl group of 1 to 6 carbon atoms, an alkyl group of 1 to 3 carbon atoms, or an ethyl group. X may preferably be Cl or Br, preferably Cl, and n may be an integer of 1 to 3 or an integer of 2 or 3.
[0069] The co-catalyst represented by Formula 2 can use: trialkylaluminum, such as trimethylaluminum, triethylaluminum, tri-n-propylaluminum, triisopropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-tert-butylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum and tri-2-ethylhexylaluminum; dialkylaluminum halide, such as dimethylaluminum chloride, diethylaluminum chloride, diisopropylaluminum chloride, diisobutylaluminum chloride and dimethylaluminum bromide; alkylaluminum dihalide, such as methylaluminum dichloride, ethylaluminum dichloride, isopropylaluminum dichloride and ethylaluminum dibromide; aluminum trihalide, such as aluminum trihalide; or a combination thereof without limitation.
[0070] The catalyst composition of the present invention is suitable for the cationic polymerization reaction of preparing isobutylene-isoprene copolymer. In the process of cationic polymerization, it is important to stabilize the cationic part formed in the polymerization process. The cocatalyst represented by Formula 2 is a strong Lewis acid and can form an ion pair with the borate-type bulky anion in the catalyst structure, thereby playing a role in effectively stabilizing the cationic part. Therefore, an isobutylene-isoprene copolymer with a high molecular weight can be prepared.
[0071] Specifically, in the process of copolymerizing isobutylene and isoprene, unlike homopolymerization of isobutylene, isoprene may be combined with a cationic chain undergoing polymerization to obtain a resonance structure, thereby deteriorating the additional reaction of the cation, and it is understood that the additional polymerization proceeds very slowly or causes a termination reaction. In view of these points, it is important to select and use a catalyst and a co-catalyst having high reactivity so as not to cause premature termination.
[0072] As in the present invention, if the catalyst represented by Formula 1 and the co-catalyst represented by Formula 2 are used in combination in a polymerization reaction, the alkyl group bonded to aluminum in the co-catalyst represented by Formula 2 reacts with the hydrogen of the catalyst represented by Formula 1 to dissociate into an alkane. Thereafter, the vacancy in the co-catalyst represented by Formula 2 enables the ether of the catalyst represented by Formula 1 and another molecule of the co-catalyst represented by Formula 2 to strongly combine to form an aluminum cation having a strong Lewis acid property, and this can efficiently act as a polymerization initiator for the copolymerization reaction of isobutylene and isoprene. For example, if Et is used, 2 AlCl is used as a co-catalyst represented by Formula 2 in the present invention to form aluminum cations such as [Al(Et)Cl] + and [AlCl] 2+ , and these can act as polymerization catalysts.
[0073] On the contrary, other types of cocatalysts not containing aluminum do not cause the above reaction, specifically, as metals other than aluminum, aluminum oxides such as aluminoxane, etc., metal compounds containing elements such as magnesium (Mg), zinc (Zn) and iron (Fe) have low reactivity, and it is difficult to form metal cations through reaction with the catalyst, and are not suitable for use as cocatalysts for cationic polymerization. In addition, although aluminum is contained, if the cocatalyst does not have a structure that easily induces cationic polymerization by a mechanism that dissociates part of the functional groups into alkanes, it is difficult to use the cocatalyst together with the catalyst represented by Formula 1.
[0074] As described above, the present invention is characterized in that an isobutylene-isoprene copolymer can be efficiently prepared by cationic polymerization at a high conversion rate using the catalyst represented by Formula 1 and the co-catalyst represented by Formula 2 as an appropriate combination.
[0075] The weight ratio of the catalyst represented by Formula 1 to the co-catalyst represented by Formula 2 may be 1:2 to 1:16, specifically, 1:4 to 1:12, or 1:8, to improve production yield while easily controlling the weight average molecular weight of the isobutylene-isoprene copolymer to a suitable value within a desired range.
[0076] If the weight of the co-catalyst represented by Formula 2 deviates from the above range and is too small, the catalyst activation by the co-catalyst will not be sufficiently caused, and the defect of inefficient cationic polymerization will be caused. If the weight of the catalyst represented by Formula 1 deviates from the above range and is too small, the polymerization reaction using the catalyst will not occur sufficiently, and there will be a defect of deteriorating the polymerization efficiency compared with the co-catalyst used.
[0077] <Method for preparing isobutylene-isoprene copolymer>
[0078] The method for preparing an isobutylene-isoprene copolymer of the present invention is characterized by comprising copolymerizing isobutylene and isoprene in the presence of the catalyst composition.
[0079] Considering the efficient preparation of the isobutylene-isoprene copolymer having a high molecular weight, which is the purpose of the present invention, the copolymerization of isobutylene and isoprene may be carried out at a temperature of -50° C. to -10° C., and may be specifically carried out at a temperature of -40° C. to -20° C. In addition, the polymerization reaction at this temperature may be carried out for 30 minutes to 5 hours, or 1 hour to 3 hours.
[0080] If the polymerization temperature is higher than -10°C, chain growth occurs rapidly at a relatively high temperature and the conversion rate is increased, but the molecular weight becomes low. Therefore, there is a defect that an isobutylene-isoprene copolymer having a high molecular weight as in the present invention is not formed. If the polymerization temperature is lower than -50°C, the catalyst activity is reduced due to the low temperature, a larger amount of catalyst is required for the same polymerization reaction, and there is a defect that the economic feasibility and efficiency of the polymerization are greatly reduced.
[0081] In the present invention, based on the total weight of isobutylene and isoprene, the amount of the catalyst represented by Formula 1 may be 0.002 wt % to 0.05 wt %, specifically, 0.002 wt % or more, 0.005 wt % or more, 0.010 wt % or more, and 0.050 wt % or less, 0.040 wt % or less, 0.030 wt % or less. If the above range is met, the polymerization reaction can be efficiently carried out. If the catalyst is used in an excess amount exceeding the above numerical range, the polymerization efficiency will not be significantly improved compared to the increase in raw material cost.
[0082] In addition, based on the total weight of isobutylene and isoprene, the amount of the co-catalyst can be 0.05 wt % to 0.4 wt %, specifically, 0.05 wt % or more, 0.10 wt % or more, 0.15 wt % or more, and 0.40 wt % or less, 0.30 wt % or less, 0.20 wt % or less. If the co-catalyst is used within the above range, the appropriate effect of using the co-catalyst can be obtained, and the isobutylene-isoprene copolymer can be prepared with excellent efficiency. If added in excess, the process cost will increase as the amount of residual by-products in the final copolymer increases, and it is preferred to control and use an appropriate amount of the co-catalyst within the above range.
[0083] The amount of isoprene may be appropriately selected within a range satisfying desired physical properties, and may specifically be 1 mol% or more, 1.5 mol% or more, and 10 mol% or less, 8 mol% or less, 5 mol% or less, 3 mol% or less, or 2.5 mol% or less based on isobutylene.
[0084] The molecular weight distribution of the isobutylene-isoprene copolymer prepared by the preparation method of the present invention may be 1.5 to 3.0, specifically, 2.9 or less, 2.8 or less, 2.5 or less, or 2.4 or less.
[0085] By the preparation method of the present invention, the physical properties of the copolymer can be variously controlled within the above ranges, and specifically, by controlling the type or amount of the co-catalyst, the molecular weight and molecular weight distribution can be easily controlled according to the desired purpose.
[0086] The weight average molecular weight and the number average molecular weight are polystyrene-equivalent molecular weights analyzed by gel permeation chromatography (GPC), and the molecular weight distribution is calculated from the ratio of (weight average molecular weight) / (number average molecular weight).
[0087] The catalyst composition of the present invention is suitable for preparing an isobutylene-isoprene copolymer having the molecular weight and molecular weight distribution values, and the initiation reaction and the chain growth reaction are easily controlled using the catalyst represented by Formula 1 and the co-catalyst represented by Formula 2, so as to prepare an isobutylene-isoprene copolymer having a high weight average molecular weight and a low molecular weight distribution within the above range.
[0088] Therefore, in order to prepare an isobutylene-isoprene copolymer having a desired high weight average molecular weight, the polymerization temperature may be set to -50°C to -10°C, but the polymerization temperature is not limited thereto. A person skilled in the art may appropriately control the reaction temperature in consideration of the molecular weight, molecular weight distribution, etc. of the prepared isobutylene-isoprene copolymer.
[0089] In addition, in the present invention, the catalyst composition may include a halogen-free solvent. That is, copolymerization may be carried out under a halogen-free solvent. Specifically, the catalyst composition of the present invention includes a hydrocarbon solvent together with the catalyst and the co-catalyst, and the hydrocarbon solvent may use a mixture of a halogenated hydrocarbon solvent and a halogen-free solvent, or a halogen-free solvent alone.
[0090] The halogen-free solvent may be an aliphatic hydrocarbon solvent or an aromatic hydrocarbon solvent. For example, the aliphatic hydrocarbon solvent may be one or more selected from butane, pentane, neopentane, hexane, cyclohexane, methylcyclohexane, heptane and octane, and the aromatic hydrocarbon solvent may be one or more selected from benzene, toluene, xylene and ethylbenzene, without limitation.
[0091] The halogenated hydrocarbon solvent may be one or more selected from methyl chloride, dichloromethane, chloroform, 1-chlorobutane and chlorobenzene without limitation.
[0092] In the present invention, if a halogen-free solvent and a halogenated hydrocarbon solvent are mixed and used as a solvent, the mixing ratio may be 100:1 to 1:2 by volume, specifically, 100:1 to 1:1 by volume without limitation.
[0093] The method for preparing isobutylene-isoprene copolymer of the present invention can also carry out the step of removing the catalyst after the step of carrying out the cationic polymerization of the monomer. Since the catalyst of the present invention can be efficiently removed by a simple physical filtration step, it is more advantageous to use and remove it when compared with the Lewis acid catalyst of the conventional technology.
[0094] Specifically, after polymerizing the isobutylene-isoprene copolymer, the organic solvent may be removed to control the organic solvent to be less than 40 wt %, less than 20 wt %, or less than 5 wt % of the oligomer or polymer. Then, in the case of a polymer having fluidity, a step of filtering the insoluble matter using a glass filter of 80 mesh or more, 100 mesh or more, or 200 mesh or more may be performed. Otherwise, the catalyst may be removed by passing the polymer having fluidity through a silica, diatomaceous earth, or zeolite filter.
[0095] Meanwhile, in the case of a polymer having little fluidity, one or more selected from a linear alkyl solvent such as pentane, cyclopentane, hexane, cyclohexane, heptane and octane, and an ether solvent such as diethyl ether and petroleum ether are used to provide fluidity, and then, a step of filtering through a glass filter, or a silica, diatomaceous earth or zeolite filter may be performed.
[0096] Typically, the isobutylene-isoprene copolymer thus prepared is dissolved in an organic solvent such as pentane, cyclopentane, hexane, cyclohexane, heptane, octane, diethyl ether and petroleum ether, and washed to remove the catalyst. However, in the present invention, the catalyst represented by Formula 1 can be efficiently removed by a simple filtering step as described above, and a separate washing step is not required.
[0097] In addition, the preparation method of the present invention may further include a step of drying the remaining solvent after the filtering step. For example, the drying temperature may be 30° C. to 200° C. or 40° C. to 150° C., and the vacuum degree may be 300 torr or less, 200 torr or less, or 100 torr or less. Thus, the desired isobutylene-isoprene copolymer may be obtained efficiently. In addition, the drying method is not specifically limited, and conventional methods may be applied.
[0098] In addition, in the method for preparing isobutylene-isoprene copolymer of the present invention, after the polymerization step and before filtering, a step of drying the halogenated hydrocarbon solvent may be performed separately, or may not be performed. If a drying step is performed, the drying conditions may be the same as described above without specific limitation.
[0099] In the case of performing the drying step of the halogenated hydrocarbon solvent separately, there is an advantage in that a higher purity isobutylene-isoprene copolymer can be obtained. However, according to the present invention, since the catalyst can be easily removed by simple filtration as described above, the drying step of the halogenated hydrocarbon solvent separately after the polymerization step and before filtration can be omitted, and there is an advantage in simplifying the process.
[0100] Example
[0101] Hereinafter, the present invention will be described in more detail by way of examples. However, the following examples are merely illustrative of the present invention, and the scope of the present invention is not limited thereto.
[0102] <Preparation of Catalyst>
[0103] Preparation Example 1
[0104]
[0105] In the presence of DCM, sodium imidazole and 2 equivalents of B(C) compared to sodium imidazole were reacted. 6 F 5 ) 3 Mix and stir at room temperature for 15 hours to prepare [Na] + [Imd(B(C 6 F 5 ) 3 ) 2 ] - A solution of HCl in diethyl ether was injected thereinto at low temperature, the temperature was raised to room temperature, and stirring was performed for 1 hour. The diethyl ether was removed in vacuo, and the NaCl salt by-product was removed by filtration.
[0106] To the thus obtained substance and DCM were added 3 equivalents of dibutyl ether and stirred at room temperature for 30 minutes, and the solvent and dibutyl ether were vacuum dried to obtain the catalyst of Preparation Example 1.
[0107] Preparation Example 2
[0108]
[0109] In the presence of DCM, sodium imidazole and 2 equivalents of B(C) compared to sodium imidazole were reacted. 6 F 5 ) 3 Mix and stir at room temperature for 15 hours to prepare [Na] + [Imd(B(C 6 F 5 ) 3 ) 2 ] -. A HCl solution in diethyl ether was injected thereinto at low temperature, the temperature was raised to room temperature, and stirring was performed for 1 hour. The diethyl ether was removed in vacuo, and the NaCl salt by-product was removed by filtration to obtain the catalyst of Preparation Example 2.
[0110] Comparative Preparation Example 1
[0111]
[0112] In the presence of DCM, a solution of HCl in diethyl ether was injected into the LiB(C) 6 F 5 ) 4 The temperature was raised to room temperature and stirring was performed for 1 hour. The diethyl ether was removed in vacuo and the NaCl salt by-product was removed by filtration.
[0113] To the thus obtained substance and DCM were added 3 equivalents of dibutyl ether and stirred at room temperature for 30 minutes, and the solvent and dibutyl ether were vacuum dried to obtain a catalyst of Comparative Preparation Example 1.
[0114] Comparative Preparation Example 2
[0115]
[0116] In the presence of DCM, a solution of HCl in diethyl ether was injected into the LiB(C) 6 F 5 ) 4 The temperature was raised to room temperature and stirring was performed for 1 hour. Diethyl ether was removed in vacuo and the NaCl salt by-product was removed by filtration to obtain the catalyst of Comparative Preparation Example 2.
[0117] Comparative Preparation Example 3
[0118]
[0119] In the presence of DCM, NaCN and 2 equivalents of B(C) compared to NaCN were reacted. 6 F 5 ) 3 Mix and stir at room temperature for 15 hours to prepare [Na] + CN(B(C 6 F 5 ) 3 ) 2 ] - . HCl solution in diethyl ether was injected at low temperature, the temperature was raised to room temperature, and stirring was performed for 1 hour. The diethyl ether was removed in vacuo, and the NaCl salt by-product was removed by filtration.
[0120] To the thus obtained substance and DCM were added 3 equivalents of dibutyl ether and stirred at room temperature for 30 minutes, and the solvent and dibutyl ether were vacuum dried to obtain a catalyst of Comparative Preparation Example 3.
[0121] Comparative Preparation Example 4
[0122]
[0123] In the presence of DCM, NaN 3 Sum and NaN 3 Compared with 2 equivalents of B(C 6 F 5 ) 3 Mix and stir at room temperature for 15 hours to prepare [Na] + N 3 (B(C 6 F 5 ) 3 ) 2 ] - . HCl solution in diethyl ether was injected at low temperature, the temperature was raised to room temperature, and stirring was performed for 1 hour. The diethyl ether was removed in vacuo, and the NaCl salt by-product was removed by filtration.
[0124] To the thus obtained substance and DCM were added 3 equivalents of dibutyl ether and stirred at room temperature for 30 minutes, and the solvent and dibutyl ether were vacuum dried to obtain a catalyst of Comparative Preparation Example 4.
[0125] Comparative Preparation Example 5
[0126]
[0127] In a glove box, 100 mg of LiAlH 4 Dissolve in 5 mL of THF, slowly inject 4 equivalents of pentafluorophenyl, and open the stopcock to fully generate H 2 . After stirring at room temperature for 1 hour, the stopcock was closed, the reaction system was taken out from the glove box, and 3 equivalents of HCl in diethyl ether were slowly injected therein. After stirring for 1 hour, the solvent was removed in vacuo, and the reaction system was placed in a glove box. After the product was dissolved in DCM, LiCl was removed using a syringe filter, the solvent was removed in vacuo, and the remaining product was washed with anhydrous hexane. Then, the product thus obtained was vacuum dried to obtain the catalyst of Comparative Preparation Example 5 in a white solid state.
[0128] <Preparation of isobutylene-isoprene copolymer>
[0129] Example 1
[0130] An Andreus glass pressure reactor from which moisture and oxygen were removed was prepared. 20 g of isobutylene was injected through a pipeline connecting an isobutylene tank and an Andreus glass cooled to -40°C. As a solvent, hexane that had passed through a moisture purification column was used, and after calculating the monomer concentration in the reactant (total solution of the compound, TSC), an amount suitable for the corresponding TSC was separately taken out using a syringe and injected through the top of the Andreus glass.
[0131] The isoprene comonomer was used after passing through an alumina column in a glove box. 1.65 mol% of isoprene was weighed using a syringe based on isobutylene and injected through the top of the Andre glass. As a catalyst, 0.025 wt% of the catalyst of Preparation Example 1 stored in a glove box at low temperature was weighed based on the total weight of isobutylene and isoprene, and dissolved in a dichloromethane (DCM) solvent. Co-catalyst (Et) 2 AlCl was also stored in the glove box, and the co-catalyst was diluted to 25 wt% in hexane, and 0.200 wt% based on the total weight of isobutylene and isoprene was weighed and mixed with the catalyst solution.
[0132] The mixed catalyst + co-catalyst solution was transferred to a syringe, transferred to the outside of the glove box, and then injected through the top of the Andreus glass. After the catalyst was injected, the reaction was carried out at -40°C for 60 minutes. After the reaction was completed, the valve on the top of the Andreus glass was opened to remove the remaining unreacted isobutylene, and then the Andreus glass was opened to recover the butyl rubber and solvent. The recovered butyl rubber was dried in an oven at 110°C for 2 hours to remove the remaining solvent and analyzed.
[0133] Examples 2 to 5 and Comparative Examples 1 to 12
[0134] An isobutylene-isoprene copolymer was prepared by the same method as in Example 1, except that the polymerization conditions were changed as shown in Table 1 below.
[0135] [Table 1]
[0136]
[0137] <Analysis of Physical Properties of Isobutylene-Isoprene Copolymer>
[0138] Experimental Example 1
[0139] For the isobutylene-isoprene copolymers prepared in Examples and Comparative Examples, physical properties were measured by the following methods, and the results are summarized in Table 2.
[0140] (1) Yield (%)
[0141] The calculation is performed by dividing the weight (g) of the obtained isobutylene-isoprene copolymer by the sum of the weight (g) of isobutylene and the weight (g) of isoprene.
[0142] (2) Isoprene content (mol %)
[0143] A 500 MHz NMR (Agilent Co.) (sample concentration: 0.5 wt %, solvent: CDCl 3 )Measurement 1 H NMR. 1 The presence of isoprene in the copolymer was confirmed in the H NMR spectrum, and the isoprene content was calculated by the following equation.
[0144] - Isoprene content (mol %) = (number of moles of isoprene in the copolymer) / (number of moles of isobutylene in the copolymer) + (number of moles of isoprene in the copolymer)
[0145] (3) Weight average molecular weight and molecular weight distribution
[0146] The measurement of the isobutylene-isoprene copolymer was performed under the following gel permeation chromatography (GPC) analysis conditions, and the weight average molecular weight (Mw) and the number average molecular weight (Mn) were measured, and then the molecular weight distribution was calculated from the value of (weight average molecular weight) / (number average molecular weight).
[0147] -Chromatographic column: PL MiniMixed B×2
[0148] -Solvent: THF
[0149] -Flow rate: 0.3ml / min
[0150] - Sample concentration: 2.0mg / ml
[0151] -Injection volume: 10μl
[0152] - Column temperature: 40℃
[0153] -Detector: Agilent RI detector
[0154] -Standard: Polystyrene (calibrated by cubic function)
[0155] -Data processing: ChemStation
[0156] [Table 2]
[0157]
[0158] In the case of Comparative Examples 1 and 2 using the catalyst of the Comparative Preparation Example not conforming to Formula 1, a copolymer having a significantly low weight average molecular weight was prepared when compared with Example 1 using the catalyst of Preparation Example 1 under the same conditions.
[0159] In addition, Comparative Examples 3 to 5 using the catalyst of the comparative preparation example, and Comparative Examples 6 and 7 using the catalyst of the present invention but without using a co-catalyst, copolymerization of isobutylene and isoprene could not be performed, and an isobutylene-isoprene copolymer could not be obtained.
[0160] In Comparative Examples 8 to 12 using the catalyst of the present invention and a co-catalyst not conforming to Formula 2, it can be confirmed that isobutylene-isoprene copolymers can be obtained only in Comparative Examples 9 and 12, and copolymers having a low weight average molecular weight and a wide molecular weight distribution compared to the examples are prepared in both Comparative Examples 9 and 12.
[0161] As shown in the above results, it can be found that when the catalyst represented by Formula 1 according to the present invention and the co-catalyst represented by Formula 2 are used together, an isobutylene-isoprene copolymer having a high weight average molecular weight and a narrow molecular weight distribution can be prepared with excellent yield.
Claims
1. A method for preparing an isobutylene-isoprene copolymer, the method comprising copolymerizing isobutylene and isoprene in the presence of a catalyst composition comprising a catalyst represented by the following formula 1 and a co-catalyst represented by the following formula 2: [Formula 1] In formula 1, R is an alkyl group of 2 to 12 carbon atoms, R1 to R6 are each independently a halogen group, a to f are each independently an integer from 1 to 5, [Formula 2] (Ra)nAl(X)3-n In formula 2, R a is an alkyl group of 1 to 12 carbon atoms, X is a halogen group, n is an integer from 0 to 3, in, A weight ratio of the catalyst represented by Formula 1 to the co-catalyst represented by Formula 2 is 1:2 to 1:
16.
2. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: The copolymerization is carried out at a temperature of -50°C to -10°C.
3. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: The amount of the catalyst represented by Formula 1 is 0.002 wt% to 0.05 wt% based on the total weight of isobutylene and isoprene.
4. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: The amount of the co-catalyst represented by Formula 2 is 0.05 wt % to 0.4 wt % based on the total weight of isobutylene and isoprene.
5. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: In formula 1, R is an alkyl group of 2 to 8 carbon atoms, R1 to R6 are each independently F or Cl, a to f are each independently an integer of 3 to 5.
6. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: In formula 1, R is an alkyl group of 2 to 6 carbon atoms, R1 to R6 are F, a to f are each independently an integer of 4 or 5.
7. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: The catalyst represented by Formula 1 is a compound represented by the following Formula 1-1 or Formula 1-2: [Formula 1-1] [Formula 1-2] 8. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: In formula 2, R a is an alkyl group of 1 to 12 carbon atoms, X is Cl or Br, n is an integer of 1 to 3.
9. The method for preparing an isobutylene-isoprene copolymer according to claim 1, wherein: In formula 2, R a is an alkyl group of 1 to 12 carbon atoms, X is Cl, n is an integer of 2 or 3.
Citation Information
Patent Citations
Gel polymer electrolyte for electrochemical gas sensor comprising polysaccharide polymer and method of fabricating of the same
KR1020200120298A
Solvent-stable metal complexes having slightly co-ordinating counter anions as polymerisation catalysts
CN101282785A
Method for producing highly reactive isobutylene homo- or copolymers using metal-containing catalyst complexes
CN101331159A
Highly reactive polyisobutylene having a high percentage of vinylidene double bonds in the side chains
CN105377910A
Method for preparing polybutene oligomer
CN111587258A