A welding method for header and pipe seat

During the welding process of the collector and pipe seat of the power station boiler, the transition tube seat surfacing and non-destructive flaw detection methods are used to solve the problem of cracks caused by heat treatment after welding, and the restraint and internal stress are reduced, ensuring the welding quality And reduce production costs.

CN114952053BActive Publication Date: 2024-11-08DONGFANG BOILER GROUP OF DONGFANG ELECTRIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110188349.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-11-08
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

During the welding process of the collector and pipe seat of power station boilers, cracks are easily generated after heat treatment after welding, especially in alloy steel or heat-resistant steel materials. Traditional processes are difficult to prevent and solve the problems of reheat cracks or aging cracks, which limits the Materials applications and development of high-parameter power plant boilers.

Method used

The center line of the pipe seat pipe hole is cut on the cylinder and the bottom hole is processed to perform the transition pipe seat surfacing to ensure that the height of the transition pipe seat is not less than 2.5mm, and a 100% non-destructive flaw detection is performed. The intermediate heat treatment is performed first, and the transition is then carried out. The pipe seat is welded to the pipe seat, and finally undergoes a comprehensive post-weld heat treatment to ensure the quality of the weld through non-destructive flaw detection.

Benefits of technology

It reduces the constraints and internal stress of welding, avoids cracks caused by heat treatment of pipe seat fillet welds after welding, ensures welding quality and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114952053B_ABST
    Figure CN114952053B_ABST
Patent Text Reader

Abstract

The invention discloses a method for welding a header and a pipe seat, comprising the following steps: A) marking the center line of the pipe hole of the pipe seat on the cylinder, and processing the bottom hole; B) marking the position line of the transition pipe seat welding area, performing surfacing welding on the transition pipe seat, ensuring that the height of the transition pipe seat is not less than h, processing the transition pipe seat to the height h and the top plane, and then processing the pipe hole; C) performing 100% non-destructive flaw detection inspection on the transition pipe seat, and performing post-weld heat treatment on the cylinder and the transition pipe seat; D) assembling the transition pipe seat and the pipe seat and welding the butt welds of the two; E) performing 100% non-destructive flaw detection inspection on the butt welds, and performing post-weld heat treatment on the cylinder, the transition pipe seat, the pipe seat and the butt welds; the invention can reduce the constraint degree and eliminate the internal stress after welding, avoid cracks caused by the post-weld heat treatment of the pipe seat fillet weld, ensure the welding quality, and reduce the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a welding method for a header and a pipe seat, in particular to a welding method for a header and a pipe seat used for a power station boiler. Background Art

[0002] The header is an important pressure-bearing component of the power station boiler. A large number of pipe seats are arranged axially and circumferentially on the cylinder, which are usually connected to the header cylinder by welding. Due to the large number of pipe seats on the header, the large welding volume, and the large specifications of the header cylinder, the large thermal expansion and contraction during welding, resulting in a large degree of restraint and a large internal stress after welding. Post-weld heat treatment is usually required to eliminate welding residual stress and improve the mechanical properties of the joint. However, for some alloy steel or heat-resistant steel (such as T / P23, etc.) headers, cracks usually occur at the toe of the pipe seat fillet weld after post-weld heat treatment, which is usually called reheat cracks or stress relief cracks. In addition, in order to develop higher parameter and more efficient power station boilers, it is necessary to use age-hardened alloy materials to make header products. Their service state is the aged state, but in order to ensure that they have good weldability, they usually need to be welded in the solid solution state with a large degree of restraint. After welding, they are subjected to heat treatment to restore their mechanical properties (such as aging heat treatment). However, for some header products made of special age-hardened alloy materials, cracks are easily generated at the toe of the pipe seat corner weld after aging heat treatment after welding, which is called age-effect strain cracking.

[0003] For the above-mentioned products such as headers made of materials with reheat crack sensitivity and aging strain cracking characteristics, the corner welds of the tube sockets are prone to cracking after post-weld heat treatment. Under the condition that the material and product structure remain unchanged, the traditional process cannot prevent and solve the problem of reheat cracks or aging cracks in the corner welds of the header tube sockets, which seriously restricts the application of such materials and the development of products such as power station boilers with higher parameters. Summary of the invention

[0004] The purpose of the present invention is to provide a welding method for a header and a tube seat in view of the above-mentioned deficiencies in the prior art, which can reduce the degree of constraint and eliminate the internal stress after welding, avoid cracks caused by heat treatment of the tube seat corner weld after welding, ensure welding quality, and reduce production costs.

[0005] In order to achieve the above-mentioned purpose, a method for welding a header and a pipe seat of the present invention comprises the following steps: A) marking the center line of the pipe hole of the pipe seat on the cylinder and processing the bottom hole; characterized in that: B) marking the position line of the transition pipe seat welding area, performing surfacing welding of the transition pipe seat, ensuring that the height of the transition pipe seat is not less than h, processing the transition pipe seat to the height h and the top plane, the height h is not less than 2.5mm, and then processing the pipe hole; C) performing 100% non-destructive flaw detection inspection on the transition pipe seat, and performing post-weld heat treatment on the cylinder and the transition pipe seat; D) assembling the transition pipe seat and the pipe seat and welding the butt welds of the two; E) performing 100% non-destructive flaw detection inspection on the butt welds, and performing post-weld heat treatment on the cylinder, the transition pipe seat, the pipe seat and the butt welds;

[0006] The present invention first welds the transition pipe seat, one side of which is in a free state with a small degree of restraint. Through intermediate heat treatment, the internal stress of the connection between the cylinder and the transition pipe seat is eliminated and redistributed, thereby avoiding the accumulation of stress after subsequent pipe seat welding. The top plane of the transition pipe seat is butted and welded with the pipe seat, and the welding stress is small, which is also convenient for processing. Finally, through the final heat treatment, the welding residual stress is completely eliminated, and cracks are avoided in the heat treatment of the pipe seat corner weld after welding, thereby ensuring the welding quality and reducing the production cost. The height h is not less than 2.5 mm, which can ensure a sufficient transition pipe seat height.

[0007] As a further improvement of the present invention, the non-destructive testing method is one or a combination of more than one of RT, UT, MT, PT, phased array and TOFD testing; all of which can detect cracks;

[0008] As a further improvement of the present invention, in step B), a groove is pre-processed on the cylinder; in step D), a groove is pre-processed on the pipe seat; the weld penetration can be ensured;

[0009] As a further improvement of the present invention, after step E), the butt weld between the transition pipe seat and the pipe seat is subjected to 100% X-ray + 100% magnetic powder nondestructive testing to ensure that there are no post-weld cracks;

[0010] In summary, the present invention can reduce the degree of restraint and eliminate the internal stress after welding, avoid cracks caused by heat treatment of the pipe seat corner weld after welding, ensure welding quality, and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a front view of a process in an embodiment of the present invention.

[0012] Figure 2 for Figure 1 Left view of .

[0013] Figure 3It is a front view of another process in an embodiment of the present invention.

[0014] Figure 4 for Figure 3 Left view of .

[0015] Figure 5 It is a front view of another process in an embodiment of the present invention.

[0016] Figure 6 for Figure 5 Left view of . DETAILED DESCRIPTION

[0017] In conjunction with the accompanying drawings, the present invention will be further described in detail below, taking a boiler header cylinder of a certain project as being made of 12Cr1MoVG with a specification of φ584×100, and a pipe seat made of 12Cr1MoVG with a specification of φ57×15 being arranged on the cylinder.

[0018] A method for welding a header and a pipe socket in this embodiment includes the following steps: A) Figure 1 , Figure 2 As shown in the figure, the center line of the tube hole of the tube seat is marked on the cylinder 1, and the bottom hole 2 with a diameter of 27mm is processed; B) Figure 3 , Figure 4 As shown, the transition pipe seat welding area position line is marked on the cylinder 1 and the groove is pre-processed. The transition pipe seat 3 is surfacing welded by arc welding. The welding material is 12Cr1MoVG steel matching welding material. The height of the transition pipe seat 3 is guaranteed to be not less than 15mm. The transition pipe seat 3 is processed to a height of 15mm and a top plane, and then the pipe hole 4 with a diameter of 27mm is processed; C) The transition pipe seat is 100% non-destructive inspection, and the cylinder and the transition pipe seat are subjected to post-weld heat treatment; D) As shown in FIG. Figure 5 , Figure 6 As shown, a groove is pre-processed on the tube seat 5, and the transition tube seat 3 and the tube seat 5 are assembled and welded to the butt weld 6 between the two; E) 100% non-destructive flaw detection is performed on the butt weld, and post-weld heat treatment is performed on the cylinder, transition tube seat, tube seat and butt weld; F) 100% X-ray + 100% magnetic particle non-destructive flaw detection is performed on the butt weld between the transition tube seat and the tube seat;

[0019] The above nondestructive flaw detection method is a combination of one or more flaw detection methods selected from RT, UT, MT, PT, phased array and TOFD. The post-weld heat treatment process is determined according to the material and size of the cylinder and the tube seat. The present invention first welds the transition tube seat, with only one side restricted by the cylinder and the other side in a free state, with small constraint and welding stress. The internal stress of the connection between the cylinder and the transition tube seat is eliminated and redistributed through intermediate heat treatment, and the accumulation of stress after subsequent tube seat welding is avoided. The top plane of the transition tube seat is butt-jointed and welded with the tube seat, and the welding stress is small, which is also convenient for processing. The final heat treatment is then performed to completely eliminate the welding residual stress, avoid cracks caused by the post-weld heat treatment of the tube seat fillet weld, ensure welding quality, and reduce manufacturing costs. The butt weld between the transition tube seat and the tube seat is subjected to 100% RT+100% MT nondestructive flaw detection inspection to ensure that there are no post-weld cracks.

Claims

1. A method for welding a header and a pipe socket, comprising the following steps: A) Draw the center line of the tube hole of the tube seat on the cylinder and process the bottom hole; the characteristics are: B) Draw the position line of the transition tube seat welding area, perform cladding welding on the transition tube seat, ensure that the height of the transition tube seat is not less than h, process the transition tube seat to the height h and the top plane, the height h is not less than 2.5mm, and then process the tube hole; C) Perform 100% non-destructive flaw detection on the transition tube seat, and perform post-weld heat treatment on the cylinder and the transition tube seat; D) Assemble the transition tube seat and the tube seat and weld the butt weld between the two; E) Perform 100% non-destructive flaw detection on the butt weld, and perform post-weld heat treatment on the cylinder, transition tube seat, tube seat and butt weld.

2. A method for welding a header and a pipe socket according to claim 1, characterized in that: The non-destructive flaw detection method is one or a combination of more than one of the following flaw detection methods: X-ray, ultrasound, magnetic powder, penetration, phased array and ultrasonic diffraction time-of-flight flaw detection.

3. A method for welding a header and a pipe socket according to claim 1 or 2, characterized in that: In the step B), a groove is pre-processed on the cylinder; in the step D), a groove is pre-processed on the pipe seat.

4. A method for welding a header and a pipe socket according to claim 3, characterized in that: After the step E), the butt weld between the transition pipe seat and the pipe seat is subjected to 100% X-ray + 100% magnetic powder nondestructive testing.