A composite material porous joint forming mold and preparation method
By designing composite porous joint molding molds and prepreg winding and laying processes, the problems of surface roughness and inaccurate dimensions in the prior art are solved, and high strength and low cost production of composite porous joints are achieved.
Patent Information
- Application Number
- CN202210165821.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-02-23
AI Technical Summary
The existing methods of porous joint molding of carbon fiber composite materials are difficult to achieve surface smoothness and precise dimensional control, and later surface processing will damage the fibers and reduce product strength.
A composite porous joint mold was designed. Through the combination of multiple outer molds and core molds, combined with the prepreg winding and laying process, multi-layer fiber and resin composite materials are used to form them in one piece to ensure smooth surface and high dimensional accuracy. .
The surface smooth surface and precise control of the cavity dimensions of the composite porous joints are achieved, which avoids damage to fibers during later surface processing, improves product strength, and simplifies mold design and reduces costs.
Smart Images

Figure CN114953500B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite material application, and more specifically, to a composite material porous joint forming die and a preparation method thereof. Background Art
[0002] Carbon fiber composite pipe fittings have important application value in aerospace structures and are widely used in the internal skeleton of spacecraft and aircraft, fixing brackets of engine and other parts, etc.
[0003] The main forming methods of carbon fiber composite pipe fittings include pultrusion, compression molding, vacuum bag-autoclave molding, thermal expansion molding, etc., but they all have their own shortcomings. Pultrusion has high production efficiency and is suitable for mass production, but requires special equipment and molds; vacuum bag-autoclave molding has a rough surface, and later surface processing will damage the fiber and reduce the strength of the rod. In addition, the above methods are mostly used to prepare straight tube rod parts, and are rarely used to prepare special-shaped rods such as porous joints. In addition, special-shaped rods such as porous joints often use rubber bags or water-soluble sand core molds as core molds, resulting in a rough surface state of the inner cavity after the product is formed, and the inner cavity size cannot be accurately controlled. Summary of the invention
[0004] The purpose of the present invention is to design and develop a composite material porous joint forming mold and a preparation method, through the cooperation of multiple outer molds and core molds, combined with the prepreg winding and laying process to form an integrated mold, so that the obtained composite material porous joint has a smooth surface and high dimensional accuracy.
[0005] The technical solution provided by the present invention is:
[0006] A composite material porous joint forming die, comprising:
[0007] an upper template, one side of which is provided with a groove; and
[0008] A lower template, one side of which is provided with a protrusion that engages with the groove, and a plurality of first accommodating cavities are formed between the lower template and the upper template;
[0009] A plurality of wedge-shaped blocks, which are arranged in pairs in the plurality of first accommodating cavities opposite to each other, and a plurality of second accommodating cavities are formed between the plurality of wedge-shaped blocks and the upper template;
[0010] A left side template is engaged between the other side of the upper template and the other side of the lower template, and a mold cavity is formed between the left side template, the upper template and the lower template;
[0011] A right side template, which is arranged on one side of the upper template and the lower template;
[0012] A front baffle plate is arranged on one end of the upper template, the lower template, the left template and the right template, and a first through hole is arranged on the front baffle plate;
[0013] A rear baffle plate is arranged on the other end of the upper template, the lower template, the left template and the right template, and a second through hole is arranged on the rear baffle plate;
[0014] A core mold, a gap of which is arranged in the mold cavity, and two ends of the core mold respectively pass through the first through hole and the second through hole without a gap;
[0015] A plurality of protruding blocks, which are respectively arranged in the second accommodating cavity in a one-to-one correspondence, and the plurality of protruding blocks are selectively connected to the core mold;
[0016] Wherein, multiple layers of fiber and resin composite material are wound and laid on the assembly of the core mold and the plurality of protruding blocks, and the volume content of the fiber in the fiber and resin composite material is 57±3%;
[0017] The plying sequence of the multi-layer fiber and resin composite material is:
[0018] The axial direction of the core mold is 0° and the laying angle is quasi-isotropic laying. The single layer thickness of the fiber and resin prepreg is 0.1mm-0.2mm, and the number of laying layers is determined according to the wall thickness of the porous joint of the composite material.
[0019] Preferably, the material of the multiple wedge blocks is aluminum alloy, and the material of the upper template, lower template, left template, right template, front baffle, rear baffle, core mold and multiple raised blocks are all carbon steel.
[0020] Preferably, it also includes:
[0021] Two threaded holes are provided at both ends of the core mold for selective connection and demoulding with a winding machine.
[0022] Preferably, there are straight limiters between the left side template and the upper template and the lower template.
[0023] Preferably, the upper template, the lower template and the left template are all processed with rounded corners.
[0024] A method for preparing a composite porous joint, using the composite porous joint forming mold, comprises the following steps:
[0025] Step 1: After wrapping the tetrafluoroethylene film around the core mold, fix the two ends with high-temperature tape;
[0026] Step 2: Winding and laying the fiber and resin composite material on the core mold:
[0027] The axial direction of the core mold is 0°, and the laying angle is quasi-isotropic laying, and vacuum compaction is performed after laying 3 to 4 layers of fiber and resin prepreg;
[0028] When the laying angle is 45°, use D-width prepreg cut at 45 degrees for winding, and when the laying angle is 90°, use 10mm-20mm width prepreg for winding;
[0029] D = S × sin45°;
[0030] Where D is the width of the long strip prepreg, S is the circumference of the main square tube section of the composite porous joint;
[0031] The vacuuming pressure is 0.05MPa-0.1MPa, and the time is 10-15min / time;
[0032] The single layer thickness of the fiber and resin prepreg is 0.1 mm to 0.2 mm, and the number of layers laid is determined according to the wall thickness of the porous joint of the composite material;
[0033] Step 3: laying a layer of prepreg on the outermost layer of the fiber and resin composite material, and simultaneously laying the prepreg at the midline of the tenon plane of the porous joint of the composite material;
[0034] The width of the prepreg is the circumference of the main square tube section of the composite porous joint;
[0035] Step 4: Place the core mold and multiple wedge blocks on the lower mold, install the left mold, the upper mold and the right mold on the lower mold in sequence, install the front baffle and the rear baffle at both ends of the core mold, and pre-compact the prepreg until the mold clearance is less than or equal to 0.2 mm after cyclic pressurization;
[0036] Step 5: Place the mold in a curing furnace and heat it according to the heat sealing system, then take it out and pressurize the mold until the mold clearance is less than or equal to 0.1 mm;
[0037] Step 6: Place the mold in a curing furnace and complete curing according to the curing system, then cool the mold naturally until the temperature is below 40° C., remove the mold, and obtain a composite porous joint.
[0038] Preferably, the fiber is carbon fiber, glass fiber, quartz fiber or high silica fiber, and the resin is cyanate resin, epoxy resin, bismaleimide resin, polyimide resin or o-phthalonitrile resin.
[0039] Preferably, the thermal expansion coefficient of the fiber and resin prepreg in the single layer 0° direction is α1, -1×10 -6 / K<α1<1×10 -6 / K; the thermal expansion coefficient in the 90° direction of a single layer is α2, 15×10 -6 / K<α2<35×10 -6 / K.
[0040] Preferably, when the prepreg is butt-laid at the midline of the tenon plane of the composite porous joint in the step three, the tenon area of the prepreg is allowed to overlap, the overlap size is greater than or equal to 10 mm, and the overlap seams of each layer do not overlap.
[0041] Preferably, the cyclic pressurization in step 4 includes the following process:
[0042] The pressure bolts are used to uniformly apply pressure to the upper template, lower template, left template and right template in sequence. After multiple cycles of pressurization, the prepreg is pre-compacted to a mold clearance of 0.25mm to 0.3mm. The upper template and the lower template are closed first by the force rod, and then the left template and the right template are closed to make the mold clearance less than or equal to 0.2mm.
[0043] The beneficial effects of the present invention are:
[0044] The present invention designs and develops a composite material porous joint forming mold and a preparation method thereof. The forming mold for making the composite material porous joint is made of metal material, has a smooth surface, and has high dimensional accuracy. After the product is formed, the surface of the inner cavity is smooth, and the size of the inner cavity can be accurately controlled. Later surface processing will not damage the fiber, thereby avoiding reducing the strength of the composite material porous joint. At the same time, the forming mold is simple and inexpensive, and irregular pipe fittings such as porous joints can be made. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a schematic structural diagram of the composite material porous joint forming mold of the present invention.
[0046] Figure 2 It is a schematic diagram of the partial assembly structure of the composite material porous joint forming mold of the present invention.
[0047] Figure 3 It is a schematic diagram of the main structure of the upper template described in the present invention.
[0048] Figure 4 This is a schematic diagram of the axonometric structure of the upper template described in the present invention.
[0049] Figure 5 This is a schematic diagram of the main structure of the lower template described in the present invention.
[0050] Figure 6 This is a schematic diagram of the axonometric structure of the upper template described in the present invention.
[0051] Figure 7It is a schematic diagram of the assembly front view of the upper template and the lower template of the present invention.
[0052] Figure 8 It is a schematic diagram of the assembly axonometric structure of the upper template and the lower template of the present invention.
[0053] Fig. 9 It is a schematic diagram of the assembly structure of the upper template, the lower template and the wedge block of the present invention.
[0054] Fig.10 It is a side structural schematic diagram of the left side template described in the present invention.
[0055] Fig.11 This is a schematic diagram of the axonometric structure of the left side template described in the present invention.
[0056] Fig.12 The figure is a schematic diagram of the assembly structure of the upper template, the lower template, the left template and the wedge block according to the present invention.
[0057] Fig.13 It is a structural schematic diagram of the core mold described in the present invention.
[0058] Fig.14 It is a schematic diagram of the assembly structure of the core mold and multiple raised blocks described in the present invention.
[0059] Fig.15 The present invention is a flow chart of the method for preparing the composite porous joint. DETAILED DESCRIPTION
[0060] The present invention is further described in detail below so that those skilled in the art can implement it according to the description.
[0061] like Figure 1 , Figure 2 As shown, a composite material porous joint forming mold provided by the present invention includes: an upper template 110, a lower template 120, 6 wedge blocks 130, a left template 140, a core mold 150, 3 protruding blocks 160, a right template 170, a front baffle 180 and a rear baffle 190, wherein the upper template 110, the lower template 120, the 6 wedge blocks 130, the left template 140, the 3 protruding blocks 160, the right template 170, the front baffle 180 and the rear baffle 190 are outer molds, and the composite material porous joint forming mold is obtained by assembling the outer mold and the core mold 150.
[0062] Among them, Figure 3 , Figure 4 As shown, the upper template 110 is an L-shaped structure, and one side is provided with two grooves of different structures; Figure 5 , Figure 6As shown, the lower template 120 is an L-shaped structure, and one side is provided with two protrusions that engage with the two grooves, and the two protrusions and the two grooves form a wedge-shaped structure that limits each other; Figure 7 , Figure 8 As shown, the lower template 120 and the upper template 110 are mutually engaged and form three first accommodating cavities, and the first accommodating cavities are wedge-shaped groove structures; Fig. 9 As shown, the six wedge blocks 130 are arranged in pairs opposite to each other and can be movably arranged in the three first accommodating chambers, and three second accommodating chambers are formed between the six wedge blocks 130 and the upper template 110, and the second accommodating chambers are rectangular parallelepiped structures; Fig.10 , Fig.11 As shown, the left template 140 is a convex structure; Fig.12 As shown, the left side template 140 is clamped between the other side of the upper template 110 and the other side of the lower template 120 through a straight mouth limiter, and a mold cavity is formed between the left side template 140, the upper template 110 and the lower template 120; Fig.13 As shown, the core mold 150 is a rectangular parallelepiped structure and a gap is set in the mold cavity, and threaded holes are set at both ends of the core mold 150. The core mold 150 is fixed to the winding machine through the threaded holes, and the prepreg is wound and laid as the winding machine rotates. At the same time, the threaded holes are used to apply tension to pull out the core mold 150 during demoulding; Fig.14 As shown, the three protruding blocks 160 are selectively connected to the core mold 150 via bolts, and are respectively arranged in the second accommodating cavity in a one-to-one correspondence.
[0063] Among them, Figure 2 As shown, after the core mold 150 and the three raised blocks 160 are assembled, multiple layers of fiber and resin composite materials are laid on the mold. After the laying is completed, an external template is used to pressurize and cure to obtain a composite porous joint (composite product) 200. The composite porous joint 200 consists of a main square tube and a plurality of tenons on the main body. It is made by one-piece molding through a prepreg winding and laying process. The fibers must be continuous, and ply overlap is allowed in the tenon area. The overlap size is not less than 10 mm, and overlap is not allowed between the lap seams of each layer.
[0064] like Figure 1As shown, the right side template 170 is detachably arranged on one side of the upper template 110 and the lower template 120 by bolts to prevent overflow at the tenon; the front baffle 180 is detachably arranged on one end of the upper template 110, the lower template 120, the left side template 140 and the right side template 170 by bolts, and the front baffle 180 is provided with a first through hole; the rear baffle 190 is detachably arranged on the other end of the upper template 110, the lower template 120, the left side template 140 and the right side template 170 by bolts, and the rear baffle 190 is provided with a second through hole, the first through hole and the second through hole are both square openings and have the same size as the core mold 150, and the two ends of the core mold 150 pass through the first through hole and the second through hole without gap, respectively, to ensure that the mold cavity is uniformly the wall thickness of the composite porous joint 200, and to prevent the prepreg from overflowing during the pressurized curing process, and the front baffle 180 and the rear baffle 190 are provided with observation holes to monitor the mold closing state.
[0065] Among them, the left template 140 is processed with a groove with a fillet radius and two fillets corresponding to the product, the corners of the lower template 120 and the upper template 110 are processed with fillets corresponding to the product, the radius of the fillet is equal to the outer fillet radius of the composite porous joint 200, the fillet on the core mold 150 is the same as the inner fillet of the composite porous joint 200, the outer contour size of the core mold 150 is equal to the inner contour size of the composite porous joint 200, and the main body straightness of the core mold 150 is better than 0.1mm.
[0066] The upper template 110, the left template 140, the right template 170, the front baffle 180, the core mold 150, the three raised blocks 160, the rear baffle 190, the wedge block 130 and the lower template 120 are all made of metal materials, among which the wedge block 130 is made of aluminum alloy, and the rest are carbon steel. It is difficult to pressurize the tenon of the porous joint, and the aluminum alloy wedge block is convenient for mold closing. At the same time, the expansion coefficient of aluminum alloy is larger than that of carbon steel, and it is convenient to pressurize the tenon due to thermal expansion, and the product is denser.
[0067] The present invention designs and develops a composite material porous joint forming mold and a preparation method. The forming mold for making the composite material porous joint is made of metal material, has a smooth surface, and has high dimensional accuracy. After the product is formed, the surface of the inner cavity is smooth, and the size of the inner cavity can be accurately controlled. Later surface processing will not damage the fiber, thereby avoiding reducing the strength of the composite material porous joint. At the same time, the forming mold is simple and inexpensive, and irregular pipe fittings such as porous joints can be made.
[0068] like Fig.15 As shown, the present invention also provides a method for preparing a composite porous joint, using the composite porous joint forming mold, specifically comprising the following steps:
[0069] Step 1: Wrap a layer of tetrafluoroethylene film at 45° on the core mold and fix the two ends with high-temperature tape;
[0070] The longitudinal direction of the core mold is 0 degrees, the circumferential direction is 90 degrees, and the starting point of the tetrafluoroethylene film winding is the direction in which the core mold is pulled out during demoulding, so as to facilitate the removal of the core mold during demoulding;
[0071] Step 2: Winding and laying the fiber and resin composite material on the core mold:
[0072] The axial direction of the core mold is 0°, the laying angle is quasi-isotropic laying, and after laying 3 to 4 layers of fiber and resin prepreg, a vacuum bag is made for vacuum compaction to shape the product. The vacuum pressure should reach 0.05MPa to 0.1MPa, and the time is 10 to 15min / time;
[0073] When the laying angle is 45°, use D-width prepreg to cut a 45-degree bevel before winding. When the laying angle is 90°, use 10mm-20mm width prepreg for winding, and try to ensure fiber continuity at the corners.
[0074] D = S × sin45°;
[0075] Where D is the width of the long strip prepreg, S is the circumference of the main square tube section of the composite porous joint;
[0076] The single layer thickness of the fiber and resin prepreg is 0.1 mm to 0.2 mm, and the number of layers laid is determined according to the wall thickness of the porous joint of the composite material;
[0077] Step 3: Lay a layer of prepreg on the outermost layer of the fiber and resin composite material, and lay the prepreg at the midline of the tenon plane of the porous joint of the composite material. When laying the prepreg in the tenon area, overlap is allowed, and the overlap size is not less than 10 mm. The overlap seams of each layer are not allowed to overlap;
[0078] The width of the prepreg is the circumference of the main square tube section of the composite porous joint, and the thickness of a single layer of the prepreg is 0.1 mm-0.2 mm;
[0079] Step 4: Place the core mold and 6 wedge blocks on the lower mold, install the left mold, upper mold and right mold on the lower mold in sequence, and require that the fillets on all molds correspond to the fillets of the prepreg on the core mold. Install the front baffle and the rear baffle on both ends of the core mold, and then apply pressure to the upper and lower molds, the left and right molds through the pressure bolts. After all the bolts are tightened by hand, first apply pressure evenly to the upper and lower molds, and then to the left and right molds in sequence. After multiple cycles, pre-compact the prepreg, use a feeler gauge to detect through the observation hole, and adjust the mold clearance to be uniform at 0.25-0.3mm after multiple cycles of pressurization. Use the force rod to close the upper and lower molds first, and then close the left and right molds to ensure that the mold clearance is less than or equal to 0.2mm.
[0080] Step 5: After the mold prepreg is pre-compacted, it is put into the furnace as a whole and heated according to the heat sealing system. After the heating is completed according to the heat sealing system, it is taken out of the curing furnace, and the force is applied to the upper and lower templates, and then the left and right templates in sequence to evenly apply pressure to ensure that the mold clearance is less than or equal to 0.1mm;
[0081] Step six, placing the mold in a curing furnace for heating and curing according to the curing system. After the product curing process is completed, the mold temperature naturally drops to below 40°C, and then it is taken out of the curing furnace. When demolding, the front baffle, rear baffle, right template, upper template and left template are disassembled in sequence, and the core mold is taken out from the lower template. After removing the raised blocks at the tenons on the core mold, the core mold is pulled out from the demolding end, the product is trimmed to clean up the flash and burrs, and finally a composite porous joint structure is obtained.
[0082] Wherein, in the step 2, if necessary, it is allowed to use plain carbon cloth to replace the inner and outer surface fibers, and the plain carbon cloth can not only meet the performance requirements but also make the product more beautiful;
[0083] The volume content of the fiber in the prepreg is 57±3%, and the thermal expansion coefficient of the prepreg in the single layer 0° direction is α1, -1×10 -6 / K<α1<1×10 -6 / K; the thermal expansion coefficient in the 90° direction of a single layer is α2, 15×10 -6 / K<α2<35×10 -6 / K, K is the temperature constant, such as at a temperature of 120K, K is 120, at a temperature of 100K, K is 100.
[0084] The fibers of the prepreg are carbon fibers, glass fibers, quartz fibers or high-silica fibers, and the resin of the prepreg is cyanate resin, epoxy resin, bismaleimide resin, polyimide resin or o-phthalonitrile resin.
[0085] Example 1
[0086] Step 1: The wall thickness of the product is 1.8mm. After machining the outer mold and core mold required for product molding, fix the core mold on the winding machine and wrap the tetrafluoroethylene film, and then fix the two ends with high-temperature tape;
[0087] Step 2: With the first layer laid at an angle of 0° as the first layer, wind and lay the carbon fiber / cyanate resin prepreg on the core mold connected to the raised block in the laying order of [0 / +45 / 90 / -45]4+[prepreg], with a single layer thickness of 0.1mm, and lay 16 layers in total. After laying 4 layers of prepreg, make a vacuum bag for vacuum compaction to shape the product;
[0088] The axial direction of the core mold is 0°, the circumferential direction is 90°, and it is stipulated that when laying at 45°, long strips of prepreg are cut at 45° angles for winding, and 90° thin strips of prepreg with a width of 10mm to 20mm are used for winding, and the fiber continuity is ensured as much as possible at the corners;
[0089] During the laying process, the vacuum pressure should reach 0.05MPa~0.1MPa, and the time is 10~15min / time;
[0090] The width of the long strip prepreg satisfies:
[0091] D = S × sin45°;
[0092] Where D is the width of the long strip prepreg, S is the circumference of the main square tube section of the composite porous joint;
[0093] Step 3: After the prepreg is laid, a layer of prepreg cloth is laid on the outermost layer, and the thickness of the single layer of prepreg cloth is 0.2mm;
[0094] The prepreg is cut into a long strip with a width equal to the circumference of the main cross section of the square tube and laid at the midline of the tenon plane. The tenon area allows for overlapping of the plies, with an overlap size of no less than 10mm, and overlap between the lap seams of each layer is not allowed;
[0095] Step 4: Cold mold closing:
[0096] Place the connecting raised block core mold and wedge block with the prepreg laid on the lower mold; install the left mold, upper mold, and right mold on the lower mold in sequence, and require that the fillets on all molds correspond to the fillets on the prepreg on the core mold. Install the front baffle and the rear baffle at both ends, and then apply pressure to the upper and lower molds, the left and right molds through the pressure bolts. After all the bolts are tightened by hand, first apply pressure evenly to the upper and lower molds, and then the left and right molds in sequence. After multiple cycles, pre-compact the prepreg, use a feeler gauge to detect through the observation hole, and adjust the mold clearance evenly to 0.25-0.3mm after multiple cycles of pressure. Use the force rod to close the upper and lower molds first, and then close the left and right molds to ensure that the mold clearance is less than or equal to 0.2mm;
[0097] Step 5: After the prepreg is pre-compacted, it is put into the furnace as a whole and heated according to the heat sealing system at 70±5℃ / 1h. After the heating is completed according to the heat sealing system, it is taken out of the curing furnace, and the force is applied by the upper and lower templates first, and then the left and right templates in sequence to evenly apply pressure to ensure that the mold clearance is less than or equal to 0.1mm;
[0098] Step six, place the product in a curing furnace and heat it according to the curing system of 110±5℃ / 2h~150±5℃ / 6h to cure it. After the curing process of the product is completed, it is naturally cooled to a mold temperature below 40℃, and then taken out of the curing furnace. When demolding, remove the front baffle and rear baffle, right template, upper template, and left template in turn, take the core mold out from the bottom plate, remove the multiple raised blocks on the core mold, pull the core mold out from one end, trim and clean the burrs on the product, and finally obtain a composite porous joint structure.
[0099] Example 2
[0100] Step 1: The wall thickness of the product is 3.4mm. After machining the outer mold and core mold required for product molding, fix the core mold on the winding machine and wrap the tetrafluoroethylene film, and then fix the two ends with high-temperature tape;
[0101] Step 2: With the first layer laid at an angle of 0° as the first layer, in the laying order of [0 / +45 / 90 / -45]4+[prepreg], lay the carbon fiber / epoxy resin prepreg on the core mold connected to the raised block. The thickness of the single prepreg layer is 0.2mm. A total of 16 layers are laid. After laying 4 layers of prepreg, a vacuum bag is made for vacuum compaction to shape the product.
[0102] The fiber and resin composite material is oriented along the axial direction of the core mold as 0° and the circumferential direction as 90°. When laying at 45°, long strips of prepreg are cut at 45° and wound. When laying at 90°, thin strips of prepreg with a width of 10 mm to 20 mm are wound. The fiber continuity is ensured as much as possible at the corners.
[0103] During the laying process, the vacuum pressure should reach 0.05MPa~0.1MPa, and the time is 10~15min / time;
[0104] The width of the long strip prepreg satisfies:
[0105] D = S × sin45°;
[0106] Where D is the width of the long strip prepreg, S is the circumference of the main square tube section of the composite porous joint;
[0107] Step 3: After the prepreg is laid, a layer of prepreg cloth is laid on the outermost layer, and the thickness of the single layer of prepreg cloth is 0.2mm;
[0108] The prepreg is cut into a long strip with a width equal to the circumference of the main cross section of the square tube and laid at the midline of the tenon plane; when laying the prepreg in the tenon area, overlap is allowed, and the overlap size is not less than 10mm, and overlap between the overlap seams of each layer is not allowed;
[0109] Step 4: Cold mold closing:
[0110] Place the core mold and wedge-shaped block of the connection protrusion block with the prepreg laid on the lower mold; install the left mold, upper mold, and right mold on the lower mold in sequence, and require that the fillets on all molds correspond to the fillets of the prepreg on the core mold. Install the front baffle and the rear baffle at both ends, and then apply pressure to the upper and lower molds, the left and right molds through the pressure bolts. After all the bolts are tightened by hand, first apply pressure evenly to the upper and lower molds, and then the left and right molds in sequence. After multiple cycles, pre-compact the prepreg, use a feeler gauge to detect through the observation hole, and adjust the mold clearance evenly to 0.25-0.3mm after multiple cycles of pressure. Use the force rod to close the upper and lower molds first, and then close the left and right molds to ensure that the mold clearance is less than or equal to 0.2mm;
[0111] Step 5: After the prepreg is pre-compacted, it is put into the furnace as a whole and heated according to the heat sealing system of 100±5℃ / 2h±5min. After the heating is completed according to the heat sealing system, it is taken out of the curing furnace, and the pressure is evenly applied by the upper and lower templates first, and then the left and right templates in sequence to ensure that the mold clearance is ≤0.1mm;
[0112] Step six, place the product in a curing furnace and heat it according to the curing system (135±5)℃ / 2h±5min~(150±5)℃ / 6h±5min. After the product curing process is completed, cool down naturally to the mold temperature below 40℃, take it out of the curing furnace, remove the front baffle, rear baffle, right template, upper template and left template in turn during demolding, take the core mold out from the bottom plate, remove the multiple raised blocks on the core mold, pull the core mold out from one end, trim and clean the burrs on the product, and finally obtain a composite porous joint structure.
[0113] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown and described herein.
Claims
1. A composite porous joint forming die, characterized in that: include: An upper template, one side of which is provided with a groove; as well as A lower template, one side of which is provided with a protrusion that engages with the groove, and a plurality of first accommodating cavities are formed between the lower template and the upper template; A plurality of wedge-shaped blocks, which are arranged in pairs in the plurality of first accommodating cavities opposite to each other, and a plurality of second accommodating cavities are formed between the plurality of wedge-shaped blocks and the upper template; A left side template is engaged between the other side of the upper template and the other side of the lower template, and a mold cavity is formed between the left side template, the upper template and the lower template; A right side template, which is arranged on one side of the upper template and the lower template; A front baffle plate is arranged on one end of the upper template, the lower template, the left template and the right template, and a first through hole is arranged on the front baffle plate; A rear baffle plate is arranged on the other end of the upper template, the lower template, the left template and the right template, and a second through hole is arranged on the rear baffle plate; A core mold, a gap of which is arranged in the mold cavity, and two ends of the core mold respectively pass through the first through hole and the second through hole without a gap; A plurality of protruding blocks, which are respectively arranged in the second accommodating cavity in a one-to-one correspondence, and the plurality of protruding blocks are selectively connected to the core mold; Wherein, multiple layers of fiber and resin composite material are wound and laid on the assembly of the core mold and the plurality of protruding blocks, and the volume content of the fiber in the fiber and resin composite material is 57±3%; The plying sequence of the multi-layer fiber and resin composite material is: The axial direction of the core mold is 0° and the laying angle is quasi-isotropic laying. The single layer thickness of the fiber and resin prepreg is 0.1mm-0.2mm, and the number of laying layers is determined according to the wall thickness of the porous joint of the composite material.
2. The composite porous joint forming mold according to claim 1, characterized in that: The material of the multiple wedge blocks is aluminum alloy, and the material of the upper template, the lower template, the left template, the right template, the front baffle, the rear baffle, the core mold and the multiple raised blocks are all carbon steel.
3. The composite porous joint forming mold according to claim 2, characterized in that: Also includes: Two threaded holes are provided at both ends of the core mold for selective connection and demoulding with a winding machine.
4. The composite porous joint forming mold according to claim 3, characterized in that: There are straight limiters between the left side template and the upper template and the lower template.
5. The composite porous joint forming mold according to claim 4, characterized in that: The upper template, the lower template and the left template are all processed with rounded corners.
6. A method for preparing a composite porous joint, using the composite porous joint forming mold according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: After wrapping the tetrafluoroethylene film around the core mold, fix the two ends with high-temperature tape; Step 2: Winding and laying the fiber and resin composite material on the core mold: The axial direction of the core mold is 0°, and the laying angle is quasi-isotropic laying, and vacuum compaction is performed after laying 3 to 4 layers of fiber and resin prepreg; When the laying angle is 45°, the prepreg with a width of D is cut at a 45-degree angle for winding, and when the laying angle is 90°, the prepreg with a width of 10mm to 20mm is used for winding; D = S × sin45°; Where D is the width of the long prepreg strip, S is the circumference of the main square tube section of the composite porous joint; The vacuuming pressure is 0.05MPa-0.1MPa, and the time is 10-15min / time; The single layer thickness of the fiber and resin prepreg is 0.1 mm to 0.2 mm, and the number of layers laid is determined according to the wall thickness of the porous joint of the composite material; Step 3: laying a layer of prepreg on the outermost layer of the fiber and resin composite material, and simultaneously laying the prepreg at the midline of the tenon plane of the porous joint of the composite material; The width of the prepreg is the circumference of the main square tube section of the composite porous joint; Step 4: Place the core mold and multiple wedge blocks on the lower mold, install the left mold, the upper mold and the right mold on the lower mold in sequence, install the front baffle and the rear baffle at both ends of the core mold, and pre-compact the prepreg until the mold clearance is less than or equal to 0.2 mm after cyclic pressurization; Step 5: Place the mold in a curing furnace and heat it according to the heat sealing system, then take it out and pressurize the mold until the mold clearance is less than or equal to 0.1 mm; Step 6: Place the mold in a curing furnace and complete curing according to the curing system, then cool the mold naturally until the temperature is below 40° C., remove the mold, and obtain a composite porous joint.
7. The method for preparing a composite porous joint according to claim 6, characterized in that: The fiber is carbon fiber, glass fiber, quartz fiber or high silica fiber, and the resin is cyanate resin, epoxy resin, bismaleimide resin, polyimide resin or o-phthalonitrile resin.
8. The method for preparing a composite porous joint according to claim 7, characterized in that: The thermal expansion coefficient of the fiber and resin prepreg in the single layer 0° direction is α1, -1×10 -6 / K<α1<1×10 -6 / K; the thermal expansion coefficient in the 90° direction of a single layer is α2, 15×10 -6 / K<α2<35×10 -6 / K.
9. The method for preparing a composite porous joint according to claim 8, characterized in that: The prepreg laying tenon area allows ply overlap, the overlap size is greater than or equal to 10 mm, and the overlap seams of each layer do not overlap.
10. The method for preparing a composite porous joint according to claim 9, characterized in that: The cyclic pressurization in step 4 includes the following process: The pressure bolts are used to uniformly apply pressure to the upper template, lower template, left template and right template in sequence. After multiple cycles of pressurization, the prepreg is pre-compacted to a mold clearance of 0.25mm to 0.3mm. The upper template and the lower template are closed first by the force rod, and then the left template and the right template are closed to make the mold clearance less than or equal to 0.2mm.
Citation Information
Patent Citations
Manufacturing die and forming method of large-length-diameter-ratio carbon fiber composite pipe
CN109318507A
Compression molding method of carbon fiber composite material mechanical arm
CN111196044A
Composite material space truss structure and preparation method based on curing forming mold
CN111976228A
Magnetic levitation vehicle cross beam outer frame preparation mold
CN214872824U