A method for preparing two-dimensional diamond nanosheet material
Through graphite template limited-domain growth and chemical etching technology, two-dimensional diamond nanosheets were successfully prepared under high temperature and high methane conditions, solving the problem of preparation of non-layered diamond materials and achieving high efficiency and low efficiency on non-ferrous-based substrates Cost nanosheet preparation, suitable for a variety of applications.
Patent Information
- Application Number
- CN202210523167.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-05-13
AI Technical Summary
The prior art is difficult to effectively prepare two-dimensional nanosheets of non-layered diamond materials, especially when the growth conditions are harsh and the defects are uncontrollable, and a single- or polycrystalline diamond substrate is required, which limits its universality and preparation. Difficulty.
Using graphite as a template, diamond/graphite composite films are grown under high temperature and high methane conditions through chemical vapor deposition of microwave plasma. The vertical growth of diamond is restricted by the co-uniform relationship between graphite (0002) and diamond (111) planes, and chemical wet The graphite phase and amorphous carbon phase were selectively etched by etching and thermal oxidation to obtain two-dimensional diamond nanosheets.
It realizes the preparation of two-dimensional diamond nanosheets on any non-ferrous-based substrate that can withstand high temperatures, simplifies the process, reduces costs, avoids the use of additional template materials, and provides high-quality nanosheets suitable for optoelectronics. In the fields of devices and electrochemical sensing.
Smart Images

Figure HDA0003642788070000011 
Figure HDA0003642788070000012 
Figure HDA0003642788070000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of diamond processing and preparation, and in particular to a method for preparing a two-dimensional diamond nanosheet material. Background Art
[0002] As we all know, two-dimensional diamond materials not only have the excellent mechanical, optical, electrical and chemical stability inherent in diamond, but also have a large specific surface area and can be used in the fields of electrochemistry and biosensors. At the same time, due to the high-density edge structure and the negative electron affinity of diamond, it has a high field enhancement factor in the field of electron emission or display imaging. In addition, the combination of two-dimensional diamond and other materials can construct heterogeneous optoelectronic devices, which will produce novel optoelectronic properties. Therefore, two-dimensional diamond is a nanomaterial with important research value.
[0003] At present, the preparation method of two-dimensional materials is mainly carried out for layered materials bonded by van der Waals forces, including mechanical exfoliation, chemical intercalation, and chemical vapor deposition methods. However, for non-layered materials, the above methods often fail, so the preparation of two-dimensional materials is very difficult. For diamond in the present invention, it usually forms a cubic close-packed structure under conventional high temperature and high pressure and chemical vapor deposition growth conditions, and forms equiaxed nanoparticles at the submicron scale, and the carbon-carbon bonds in diamond have the characteristics of short length and high bond strength, and the preparation of two-dimensional materials is more difficult. A small number of studies have reported that two-dimensional diamond nanosheets are obtained by chemical vapor deposition, but this method is mainly achieved by using diamond mid-face defects such as stacking faults or twin boundaries. Since the growth control of such defects is very difficult, the growth conditions of diamond nanosheets will be very harsh, and single crystal or polycrystalline diamond substrates are required to prepare two-dimensional diamonds. Therefore, in theory and in the actual preparation process, the method of preparing two-dimensional materials by regulating the crystal defects of diamond is not universal. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to provide a method for preparing a two-dimensional diamond nanosheet material, using graphite that is an allotrope with diamond as a diamond confined growth template to prepare diamond / graphite composite nanosheets, and etching the graphite phase and amorphous carbon phase therein by a post-treatment method, so that diamond nanosheets can be prepared on a large area.
[0005] The technical solution of the present invention is:
[0006] A method for preparing a two-dimensional diamond nanosheet material, based on the graphite template confined growth mechanism in the chemical vapor deposition process, using microwave plasma chemical vapor deposition method under high methane concentration and high temperature conditions, in-situ growth of diamond / graphite composite film structure, graphite (0002) plane and diamond (111) plane form a coherent relationship, graphite as a template to limit the diamond growth perpendicular to the (111) plane, parallel to the (111) plane growth is not hindered, thereby forming a diamond / composite nanosheet; further using chemical wet etching and thermal oxidation methods to selectively etch the graphite phase and amorphous sp 2 Carbon, and finally obtain two-dimensional diamond nanosheets.
[0007] The method for preparing the two-dimensional diamond nanosheet material specifically comprises the following steps:
[0008] a. Select non-ferrous materials that can withstand high temperatures as substrates, and use acetone, ultrapure water, and anhydrous alcohol to ultrasonically clean their surfaces for 5 to 15 minutes respectively to remove surface contaminants;
[0009] b. Place the cleaned substrate in a diamond seed solution and ultrasonicate for 30 to 60 minutes to form a substrate with uniform distribution of diamond seeds;
[0010] c. placing the substrate obtained in step b in a microwave plasma chemical vapor deposition apparatus, using methane and hydrogen as reaction gases, the flow ratio of methane to hydrogen is 12% to 15%, the microwave power and the working pressure are set to 8 to 10 kW and 80 to 100 mbar, the deposition temperature is 975 to 1025 ° C, and the growth is 2 to 5 hours to obtain a diamond / graphite composite film;
[0011] d. Place the diamond / graphite composite film in step c in a mixed solution of sulfuric acid and nitric acid at 100 to 200 ° C and heat for 1 to 3 hours to selectively etch the graphite phase to obtain amorphous sp 2 Diamond nanosheets of carbon;
[0012] e. The amorphous sp 2 The carbon diamond nanosheets are placed in an atmosphere of oxygen, air or Ar / O2 mixed gas and heated to 500-550°C to etch the amorphous sp 2 Carbon phase, obtaining two-dimensional diamond nanosheets.
[0013] In the method for preparing the two-dimensional diamond nanosheet material, in step a, the non-ferrous-based material is single crystal silicon, silicon carbide, metallic molybdenum or graphite.
[0014] In the method for preparing the two-dimensional diamond nanosheet material, in step b, the composition of the diamond seed solution is an aqueous solution containing 3-5wt% diamond nanocrystals, and the average grain size of the diamond nanocrystals is 4-6nm.
[0015] In the method for preparing the two-dimensional diamond nanosheet material, in step b, the substrate with uniformly distributed diamond seeds is ultrasonically cleaned with alcohol and deionized water for 3 to 6 minutes respectively, and dried to obtain a pretreated substrate.
[0016] In the method for preparing the two-dimensional diamond nanosheet material, in step c, the flow ratio of methane to hydrogen is 12% to 15%, the flow rate of methane is 48 to 60 sccm, and the grown graphite and diamond form a localized epitaxial core-shell structure.
[0017] In the preparation method of the two-dimensional diamond nanosheet material, the diameter of the diamond / graphite nanosheet is 0.1-2 μm, the thickness of the diamond sheet is less than 10 nm, and the thickness of the graphite sheet is greater than 5 nm.
[0018] The method for preparing the two-dimensional diamond nanosheet material comprises the following steps: in step d, selecting a mixed solution of sulfuric acid and nitric acid with a volume ratio of 3:1, a concentration of sulfuric acid of 98wt%, and a concentration of nitric acid of 96wt%, and selectively etching the graphite phase under stirring conditions at 150°C.
[0019] The method for preparing the two-dimensional diamond nanosheet material comprises: in step e, etching the graphite phase and containing amorphous sp 2 The carbon diamond nanosheets are treated for 5 to 10 minutes to etch the spherical diamond particles and retain the diamond nanosheets.
[0020] The design concept of the present invention is:
[0021] The present invention mainly focuses on the preparation method of two-dimensional diamond nanosheet materials, and the following description is a method for preparing diamond nanosheets. For layered materials bonded by van der Waals forces, two-dimensional materials can be prepared by mechanical exfoliation, chemical intercalation, and chemical vapor deposition. However, for non-layered materials, the above methods often fail; under this condition, finding a suitable method based on the physical and chemical properties of the material itself is the key to the preparation of two-dimensional materials. A small number of studies have reported that diamond nanosheets can be prepared based on internal defects of the diamond phase by chemical vapor deposition. Since the defect growth is uncontrollable, the growth and shape size of the nanosheet cannot be controlled. In addition, this growth method requires diamond as a substrate.
[0022] The preparation method of the present invention is based on the template confined growth mechanism of chemical vapor deposition and graphite phase. Under high-temperature growth conditions, a graphite sheet structure can be formed by high-concentration methane gas, and the graphite (0002) plane and the diamond (111) plane have a coherent relationship, that is, the (0002) plane of graphite usually grows along the diamond (111) plane, so the graphite template will limit the vertical growth of the diamond (111), while the (111) plane growth is not hindered, so that diamond / graphite composite nanosheets can be prepared, and the graphite phase and amorphous sp are selectively etched based on chemical wet etching and thermal oxidation methods. 2 The carbon phase retains the diamond nanosheets, thereby allowing the large-scale preparation of two-dimensional diamond nanosheet materials.
[0023] Compared with the existing two-dimensional material preparation technology of layered materials, the advantages and beneficial effects of the present invention are mainly reflected in:
[0024] (1) The present invention mainly targets non-layered materials and proposes a method for preparing two-dimensional diamond materials by using an in-situ template confined growth method. Since graphite is used as a template, graphite can be grown in-situ during the process of growing diamond. This method does not require the provision of additional template materials, thereby reducing the preparation steps of the two-dimensional material. At the same time, since there is no chemical contamination caused by other materials, high-quality diamond nanosheets can be provided.
[0025] (2) The method of the present invention can be grown on any non-ferrous substrate that can withstand high temperatures, without the need for single crystal or polycrystalline diamond as a substrate. This method has strong universality.
[0026] (3) The present invention adopts microwave plasma chemical vapor deposition to prepare diamond / graphite composite nanosheets, and combines chemical wet etching and thermal oxidation methods to etch the graphite phase and amorphous sp 2 Carbon phase, so the preparation method does not require high-precision preparation equipment and technology, and has the characteristics of simple process and low cost.
[0027] In summary, the method for preparing two-dimensional diamond nanosheets of the present invention is a specific template-confined growth method, which has the characteristics of simple process and strong universality, and can provide a reference method for the growth methods of other non-layered materials. At the same time, the prepared diamond nanosheets have very important scientific value and engineering significance in the fields of optoelectronic devices, electrochemical sensors, biomedicine, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Growth flow chart of two-dimensional diamond nanosheets.
[0029] Figure 2This is a scanning electron microscope image of a two-dimensional diamond / graphite composite nanosheet prepared on a silicon substrate using a microwave plasma chemical vapor deposition method. In the figure, Dia / graphite nanosheet represents a two-dimensional diamond / graphite composite nanosheet.
[0030] Figure 3 This is the Raman curve of two-dimensional diamond / graphite composite nanosheets prepared on a silicon substrate using microwave plasma chemical vapor deposition. In the figure, the horizontal axis Raman shift represents the Raman shift (cm -1 ), the ordinate Intensity represents the relative intensity (au), and Dia / graphite nanosheet represents the two-dimensional diamond / graphite composite nanosheet.
[0031] Figure 4 High-resolution transmission electron microscopy image of two-dimensional diamond / graphite composite nanosheets prepared on a silicon substrate using microwave plasma chemical vapor deposition. In the image, Dia represents two-dimensional diamond and graphite represents graphite.
[0032] Figure 5 This is a scanning electron microscope image of a two-dimensional diamond nanosheet on a silicon substrate after chemical wet etching and thermal oxidation. In the figure, Dia nanosheet stands for two-dimensional diamond nanosheet.
[0033] Figure 6 This is the Raman curve of the two-dimensional diamond nanosheet on the silicon substrate after chemical wet etching and thermal oxidation. In the figure, the horizontal axis Wavenumber represents the wave number (cm -1 ), the ordinate Intensity represents the relative intensity (au), and Diananosheet represents the two-dimensional diamond nanosheet.
[0034] Figure 7 This is a high-resolution transmission electron micrograph of a cross section of a two-dimensional diamond nanosheet on a silicon substrate after chemical wet etching and thermal oxidation. In the figure, Dia nanosheet stands for two-dimensional diamond nanosheet.
[0035] Figure 8 This is a scanning electron microscope image of a two-dimensional diamond / graphite composite nanosheet prepared on a silicon carbide substrate using a microwave plasma chemical vapor deposition method. In the figure, Dia / graphite nanosheet represents a two-dimensional diamond / graphite composite nanosheet.
[0036] Fig. 9 This is a scanning electron microscope image of a two-dimensional diamond nanosheet on a silicon carbide substrate after chemical wet etching and thermal oxidation. In the figure, Dia nanosheet stands for two-dimensional diamond nanosheet.
[0037] Fig.10 The following are transmission electron micrographs of two-dimensional diamond nanosheets on a silicon carbide substrate after chemical wet etching (a) and thermal oxidation (b). In the figure, Dia nanosheet stands for two-dimensional diamond nanosheets, and the inset in (b) is a selected area electron diffraction photograph, which confirms that it is a two-dimensional diamond nanosheet. DETAILED DESCRIPTION
[0038] In a specific implementation process, the present invention provides a method for preparing a two-dimensional diamond nanosheet material. Figure 1 As shown, the present invention is based on the confined growth mechanism of graphite templates, and uses microwave plasma chemical vapor deposition equipment to in-situ grow diamond and graphite phases on a substrate at high temperature and high methane concentration to form a diamond / graphite composite film. The prepared graphite (0002) plane and the diamond (111) plane have a coherent relationship, thereby limiting the growth of diamond perpendicular to the (111) plane, while the growth parallel to the (111) plane is unrestricted, forming a diamond / graphite composite structure nanosheet with a coherent relationship; then, the graphite phase is etched by a chemical wet etching method to form amorphous sp 2 Carbon diamond nanosheets; the amorphous sp 2 Carbon, thereby obtaining high-quality two-dimensional diamond nanosheets.
[0039] Among them, a mixed acid solution is used to selectively etch the graphite phase, and amorphous or nanocrystalline etching is performed by thermal oxidation method in an oxygen-containing atmosphere (such as air, oxygen or Ar / O2 mixed gas) at 500-550°C for 5-10 minutes. The processing time is very critical. If the time is too short, the amorphous sp 2 Carbon or spherical diamond particles cannot be etched; if the time is too long, the diamond nanosheets will be etched. The diamond nanosheets are retained to obtain large-area two-dimensional diamond nanosheets with a thickness of less than 10nm and a sheet diameter of 0.1 to 2μm. The preparation area can reach 20cm each time. 2 .
[0040] The present invention is further described below in conjunction with specific implementations, but the protection scope of the present invention is not limited thereto:
[0041] Embodiment 1:
[0042] In this embodiment, the preparation method of the one-dimensional diamond nanocone material is as follows:
[0043] (1) A single crystal silicon substrate with a length of 10 mm, a width of 10 mm, and a thickness of 0.5 mm was cleaned by ultrasonic treatment with acetone, ultrapure water, and anhydrous alcohol for 10 min each to remove surface contaminants.
[0044] (2) The cleaned single crystal silicon substrate is placed in a commercially available diamond seed solution with an average grain size of 4 to 6 nm (which is composed of an aqueous solution containing 3 to 5 wt% diamond nanocrystals) and ultrasonically treated for 30 minutes for seeding pretreatment, followed by ultrasonication in anhydrous ethanol for 3 minutes and drying to obtain a pretreated substrate. The seeds that are aggregated and loosely combined on the surface of the substrate are removed, and the diamond seeds are evenly distributed on the surface of the substrate and form a tight bond, thereby achieving the purpose of pre-nucleation.
[0045] (3) The inoculated single crystal substrate is placed at the center of the sample stage of a microwave plasma chemical vapor deposition device, and hydrogen and methane are introduced. The methane / hydrogen gas flow ratio is set to 12% to 15%, the methane flow concentration is 48 to 60 sccm, the microwave power and the working gas pressure are set to 8 kW and 80 to 100 mbar, and the substrate is grown at 975 to 1025° C. for 2 h to obtain a diamond / graphite composite nanosheet layer, such as Figure 2 As shown in Figure 2, the diameter of the nanosheet is about 1.1 μm and the thickness of the graphene sheet is greater than 9.5 nm. Figure 3 As shown in the figure, the Raman curve shows that the nanosheets are composed of diamond (Dia), graphite (located at 1590cm -1 G peak) and amorphous carbon (D). Figure 4 As shown in the figure, the high-resolution transmission electron micrograph shows that each nanosheet is composed of diamond and graphite, the (0002) plane of graphite is parallel to the (111) plane of diamond and has a coherent relationship, and the diamond and graphite are in the inner and outer layers respectively. The (0002) oriented graphite restricts the vertical growth of the diamond (111) plane, while the growth of the diamond (111) plane is unimpeded, thus forming a diamond / graphite composite nanosheet.
[0046] (4) The prepared diamond / graphite composite nanosheet sample was placed in a mixed solution of sulfuric acid and nitric acid in a volume ratio of 3:1 (the concentration of sulfuric acid was 98wt% and the concentration of nitric acid was 96wt%), and placed on a magnetic stirrer. The solution temperature was set to 150°C and stirred with a stirring bar. The treatment time was 2h to completely etch the graphite phase.
[0047] (5) The diamond nanosheet sample after etching graphite is placed in a tube furnace without any gas introduction, i.e., air atmosphere, and the annealing temperature is set to 500-550°C, and the treatment time is 5-10 min. The amorphous carbon on the diamond is etched to obtain a two-dimensional diamond nanosheet, such as Figure 5 As shown. Figure 6 As shown in Figure 2, the Raman curve shows that the crystal quality of diamond nanosheets has been greatly improved, and the corresponding high-resolution transmission electron microscopy cross-sectional photos show that the thickness of the diamond sheet is about 5nm, as shown in Figure 2. Figure 7 shown.
[0048] Embodiment 2:
[0049] In this embodiment, the preparation method of the two-dimensional diamond nanosheet material is as follows:
[0050] (1) A (001) oriented single crystal silicon carbide substrate with a length of 10 mm, a width of 10 mm, and a thickness of 0.5 mm was cleaned by ultrasonic treatment with acetone, ultrapure water, and anhydrous alcohol for 10 min each to remove surface contaminants.
[0051] (2) The cleaned silicon carbide substrate is placed in a commercially available diamond seed solution with an average grain size of 4 to 6 nm (the composition of which is an aqueous solution containing 3 to 5 wt% diamond nanocrystals) and ultrasonically treated for 60 minutes for seeding pretreatment, followed by ultrasonication in anhydrous ethanol for 3 minutes and drying to obtain a pretreated substrate. The seeds that are aggregated and loosely bonded on the surface of the substrate are removed, and the diamond seeds are evenly distributed on the surface of the substrate and form a tight bond, thereby achieving the purpose of pre-nucleation.
[0052] (3) The inoculated silicon carbide substrate is placed at the center of the sample stage of a microwave plasma chemical vapor deposition device, and hydrogen and methane are introduced. The methane / hydrogen gas flow ratio is set to 12% to 15%, the methane flow concentration is 48 to 60 sccm, the microwave power and the working gas pressure are set to 8 kW and 80 to 100 mbar, and the substrate is grown at 975 to 1025° C. for 2 h to obtain a diamond / graphite composite nanosheet layer, such as Figure 8 As shown, the diameter of the nanosheet is about 1.3 μm and the thickness of the graphene sheet is greater than 8 nm.
[0053] (4) The prepared diamond / graphite composite nanosheet sample was placed in a mixed solution of sulfuric acid and nitric acid in a volume ratio of 3:1 (the concentration of sulfuric acid was 98wt% and the concentration of nitric acid was 96wt%), and placed on a magnetic stirrer. The solution temperature was set to 150°C and stirred with a stirring bar. The treatment time was 2h to completely etch the graphite phase.
[0054] (5) The diamond nanosheet sample after etching graphite is placed in a tube furnace without any gas introduction, i.e., air atmosphere, and the annealing temperature is set to 500-550°C, and the treatment time is 5-10 min. The amorphous carbon on the diamond is etched to obtain a two-dimensional diamond nanosheet, such as Fig. 9 and 10 As shown, the thickness of the diamond layer is about 7 nm.
[0055] The results of the examples show that the method for preparing two-dimensional materials of non-layered materials provided by the method of the present invention has the characteristics of simple preparation process, strong universality and high efficiency. The prepared two-dimensional diamond nanosheets have a diameter of about 0.1 to 2 μm and a thickness of <10 nm, which can be used in important applications such as nano-photoelectric devices, electrochemical sensors and biomedicine. The research method provided by the present invention can provide reference significance for the preparation of other two-dimensional materials of non-layered materials.
Claims
1. A method for preparing a two-dimensional diamond nanosheet material, characterized in that: Based on the confined growth mechanism of graphite template in chemical vapor deposition process, the diamond / graphite composite film structure is in situ grown by microwave plasma chemical vapor deposition under high methane concentration and high temperature conditions. The graphite (002) plane and the diamond (111) plane form a coherent relationship. Graphite acts as a template to restrict the growth of diamond perpendicular to the (111) plane, while the growth parallel to the (111) plane is unhindered, thus forming diamond / composite nanosheets. The graphite phase and amorphous sp 2 Carbon, ultimately obtaining two-dimensional diamond nanosheets; The method for preparing the two-dimensional diamond nanosheet material specifically comprises the following steps: a. Select non-ferrous materials that can withstand high temperatures as substrates, and use acetone, ultrapure water, and anhydrous alcohol to ultrasonically clean their surfaces for 5 to 15 minutes in sequence to remove surface contaminants; b. Place the cleaned substrate in a diamond seed solution and ultrasonicate for 30 to 60 minutes to form a substrate with uniform distribution of diamond seeds; c. placing the substrate obtained in step b in a microwave plasma chemical vapor deposition device, using methane and hydrogen as reaction gases, the flow ratio of methane to hydrogen is 12% to 15%, the microwave power and the working pressure are set to 8 to 10 kW and 80 to 100 mbar, the deposition temperature is 975 to 1025 ° C, and the growth is 2 to 5 hours to obtain a diamond / graphite composite film, the flow rate of methane is 48 to 60 sccm, and the grown graphite and diamond form a localized epitaxial core-shell structure; d. Place the diamond / graphite composite film in step c in a mixed solution of sulfuric acid and nitric acid at 100 to 200 ° C and heat for 1 to 3 h to selectively etch the graphite phase to obtain amorphous sp 2 Diamond nanosheets of carbon; e. The amorphous sp 2 The carbon diamond nanosheets are placed in an atmosphere of oxygen, air or Ar / O2 mixed gas and heated to 500-550°C to etch the amorphous sp 2 The carbon diamond nanosheets were treated for 5 to 10 minutes to etch the spherical diamond particles and the amorphous sp 2 Carbon phase, retaining diamond nanosheets, to obtain two-dimensional diamond nanosheets with a thickness of less than 10 nm and a sheet diameter of 0.1 to 2 μm. Each preparation area reaches 20 cm 2 .
2. The method for preparing the two-dimensional diamond nanosheet material according to claim 1, characterized in that: In step a, the non-ferrous material is single crystal silicon, silicon carbide, metallic molybdenum or graphite.
3. The method for preparing the two-dimensional diamond nanosheet material according to claim 1, characterized in that: In step b, the composition of the diamond seed solution is an aqueous solution containing 3 to 5 wt% diamond nanocrystals, and the average grain size of the diamond nanocrystals is 4 to 6 nm.
4. The method for preparing the two-dimensional diamond nanosheet material according to claim 3, characterized in that: In step b, the substrate with uniformly distributed diamond seeds is ultrasonically cleaned with alcohol and deionized water for 3 to 6 minutes respectively, and dried to obtain a pretreated substrate.
5. The method for preparing the two-dimensional diamond nanosheet material according to claim 1, characterized in that: The diameter of the diamond / graphite nanosheets is 0.1 to 2 μm, the thickness of the diamond sheet is less than 10 nm, and the thickness of the graphite sheet is greater than 5 nm.
6. The method for preparing the two-dimensional diamond nanosheet material according to claim 1, characterized in that: In step d, a mixed solution of sulfuric acid and nitric acid is selected with a volume ratio of 3:1, a concentration of sulfuric acid of 98 wt %, and a concentration of nitric acid of 96 wt %, and the graphite phase is selectively etched under stirring conditions at 150° C.