A method for preparing a 100-micron transmission electron microscope sample

By using focused ion beam method and platinum carbide bonding technology in the preparation of transmission electron microscopy samples, the problem of bending and curling of hundreds of micron-level samples has been solved, the preparation of hundred-micron level transmission electron microscopy samples has been achieved, and the material microstructure has been significantly improved. Statistical analysis capabilities of structures.

CN114964969BActive Publication Date: 2024-10-08INSTITUTE OF NUCLEAR PHYSICS AND CHEMISTRY CHINA ACADEMY OF ENGINEERING PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210595584.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-26
Publication Date
2024-10-08
Estimated Expiration
2042-05-26

Smart Images

  • Figure CN114964969B_ABST
    Figure CN114964969B_ABST
Patent Text Reader

Abstract

The present invention proposes a method for preparing a 100-micron transmission electron microscope sample. The method is specifically as follows: (1) depositing a carbide protective layer and cutting a 100-micron thin-section sample; (2) depositing platinum carbide in the gap between the sample transfer needle and the top of the thin-section sample to complete the bonding of the thin-section sample; (3) moving the thin-section sample to the top of the micro-column, and depositing platinum carbide between the thin-section sample and the micro-column to complete the fixation of the thin-section sample; (4) thinning the front and rear areas of the thin-section sample, leaving a certain width range on the left, right and bottom of the thin-section sample as an unthinned area, and obtaining a 100-micron transmission electron microscope sample. This method not only overcomes the disadvantages of large-size transmission electron microscope samples being easy to bend, curl or break, but also realizes the preparation of 100-micron transmission electron microscope samples, and has a wide observation range, which meets the statistical understanding of the microstructure of the material and improves the reliability of the analysis results. It has important application prospects in the field of transmission electron microscopic analysis of materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of transmission electron microscope sample preparation, and in particular relates to a method for preparing a hundred-micron-level transmission electron microscope sample. Background Art

[0002] Transmission electron microscopy is one of the important technologies for understanding the microstructure of materials from the atomic scale. The basic requirement for analyzing samples is that the thickness of the thin area of ​​the sample is less than 100nm. According to the characteristics of materials in different forms (blocks, powders, etc.) and different systems (metals, non-metals, etc.), a variety of transmission electron microscope sample preparation technologies such as ion thinning, electrolytic polishing, ultrathin sectioning, focused ion beam, extraction, etc. have been developed and established, which have realized the understanding of the microstructure of materials and played an important role in promoting the research progress of materials.

[0003] The thin area size of the transmission electron microscope sample is usually on the order of a few microns. The analysis area and analysis results may not be representative, resulting in non-statistical or even inaccurate scientific understanding. Especially for materials with grains of several microns or materials with uneven grain size distribution, the transmission electron microscope sample with only a few microns thin area cannot obtain an accurate understanding of the material structure, which ultimately affects the research and development of the material. When the thickness of the thin area of ​​the sample is less than 100nm, the sample will usually bend or curl due to the release of residual stress. When the thin area is only on the order of a few microns, the thin area is supported by the surrounding thicker area, and the bending or curling phenomenon is not obvious. The electron microscope sample meets the basic analysis of the transmission electron microscope; but when the thin area size reaches tens of microns, hundreds of microns, or even larger, the thin area is supported by the surrounding area. The support is reduced, which eventually leads to the curling and damage of the thin area, or bending and cannot be analyzed. Therefore, the bending or curling of the thin area of ​​the sample is a bottleneck problem faced in the preparation of large-scale transmission electron microscope samples. The latest authorized patent [CN105842045B] shows that the focused ion beam method can be used to prepare transmission electron microscope samples with a length of more than ten microns. This method uses the two-end fixing method to alleviate the bending phenomenon of the sample to a certain extent. Compared with the transmission electron microscope samples of several microns prepared by the traditional method, it has made certain progress, but the transmission electron microscope samples of more than ten microns still cannot provide statistical structural information. The transmission electron microscope samples prepared by this method are only fixed at both ends and the bottom of the sample is suspended in the air. It is difficult to avoid the problem of bending when preparing transmission electron microscope samples of tens of microns. In view of this, there is an urgent need to develop a method for preparing transmission electron microscope samples of the order of hundreds of microns.

[0004] In summary, the existing electron microscope sample preparation technology still has difficulty in overcoming the bending or curling phenomenon of thin-section samples, which makes it impossible to prepare transmission electron microscope samples at the scale of 100 microns, and limits the statistical understanding of the microstructure of the material to a certain extent. It is necessary to propose an innovative preparation method for transmission electron microscope samples with a length of 100 microns to overcome the problems of sample bending, curling, and breakage. Summary of the invention

[0005] In view of this, the present invention proposes a method for preparing TEM samples at the 100-micron level, aiming to overcome the shortcomings of TEM samples at the 100-micron level that are easy to bend or curl, to achieve the preparation of TEM samples with a length of 100 microns, and ultimately to achieve the purpose of obtaining statistical scientific understanding of the microstructure of the material.

[0006] A method for preparing a 100-micron-level transmission electron microscope sample comprises the following steps:

[0007] S10 cutting 100-micron thin slice samples: deposit a carbide protective layer on the area to be sampled, and use the focused ion beam method to cut the front, back, right, bottom and left part of the thin slice sample to prepare a 100-micron thin slice sample, where a certain width of connection area is reserved on the left side of the thin slice sample to ensure that the thin slice sample does not fall into the pit formed during the cutting process of the thin slice sample, where the width is the distance between the left and right sides of the thin slice sample;

[0008] S20 bonding and extracting thin slice samples: Move the sample transfer needle with a tip less than 20μm to the top of the thin slice sample and keep a certain gap with the top of the sample. After depositing platinum carbide in the entire gap to bond the thin slice sample to the sample transfer needle, cut off the remaining connection area on the left side of the thin slice sample.

[0009] S30: Transfer and fix the thin slice sample: Use the sample transfer needle to move the thin slice sample to the top of the micro-column of the micro-grid for transmission electron microscopy, and keep a certain gap with the top of the micro-column, deposit platinum carbide in the gap to bond the thin slice sample to the micro-column, and cut off the connection area between the thin slice sample and the sample transfer needle;

[0010] S40 thin slice sample thinning: The front and back sides of the 100-micron thin slice sample were cut by the focused ion beam method. To avoid bending or curling of the sample, a certain width of unthinned area was retained on the left, right and bottom of the thin slice sample to obtain a 100-micron transmission electron microscope sample.

[0011] Optionally, in step S10, the thickness of the thin slice sample ranges from 1 μm to 3 μm, and the height of the thin slice sample ranges from 5 μm to 20 μm.

[0012] Optionally, in the step S10, the width of the left connecting area of ​​the thin slice sample is no more than 2 μm, and the carbide is platinum carbide or inorganic carbide.

[0013] Optionally, in step S20, the bonding area between the sample transfer needle and the thin slice sample is the middle area on the top of the thin slice sample, to ensure that the thin slice does not fall off during the transfer process due to its own weight.

[0014] Optionally, the micro-grid micro-columns for transmission electron microscopy described in step S30 have a width range of 120 μm to 200 μm and a thickness range of 20 μm to 50 μm, and the thin slice sample is aligned in the middle area of ​​the micro-column width direction and the thickness direction to ensure that the sample is not blocked by the micro-columns during analysis.

[0015] Optionally, the width of the unthinned areas retained on the left and right sides in step S40 ranges from 2 μm to 5 μm, the width of the unthinned area retained on the bottom ranges from 1 μm to 3 μm, and the thickness of the prepared transmission electron microscope sample is less than 100 nm.

[0016] Optionally, when the sample transfer needle is bonded to the thin slice sample in step 20, and when the thin slice sample is fixed to the top of the microcolumn in step 30, the gap between the sample transfer needle and the thin slice sample ranges from 1 μm to 3 μm, ensuring that the thin slice sample is firmly bonded and avoiding bonding failure caused by sample drift for too long.

[0017] The beneficial effects of the present invention are:

[0018] Based on the existing focused ion beam method for preparing electron microscope samples of about ten microns, the present invention attempts for the first time to deposit platinum carbide in the entire gap between the thin slice sample and the top of the micro-column of the micro-grid dedicated to the transmission electron microscope, thereby enhancing the fixation of the entire sample bottom and the top of the micro-column, and by controlling the focused ion beam cutting mode during thinning, the unthinned area is retained at both ends and the bottom of the thin slice sample, thereby achieving the function of supporting the thin slice sample at the left and right ends and the bottom, and at the same time, the unthinned area at the bottom can also further enhance the fixation with the top of the micro-column, solving the problem of bending or curling of electron microscope samples with a length of hundreds of micrometers. The preparation method of the present invention can alleviate the bending, curling, and breakage of the sample to a large extent, and the maximum length of the prepared transmission electron microscope sample can reach the order of hundreds of micrometers, which can significantly improve the statistical understanding of the microstructure of the material, and has important application prospects in the field of transmission electron microscopic analysis and research of materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is an electron microscope image of a thin slice sample with a length of 100 microns that has been cut;

[0020] Figure 2 This is an electron microscope image of a sample transfer needle bonding and extracting a thin slice sample of 100 microns in length;

[0021] Figure 3 This is an electron microscope image of a 100-micron-long thin-section sample bonded to a microgrid microcolumn dedicated to a transmission electron microscope;

[0022] Figure 4 This is a positive magnified view of the thin slice sample after it is bonded to the micro-grid micro-column dedicated to the transmission electron microscope and thinned;

[0023] Figure 5 This is the axial side view of the TEM sample of a 1 / 2 thin slice;

[0024] Figure 6 is a top view electron microscope image of the titanium hydride transmission electron microscope sample after thinning in Example 1;

[0025] Figure 7 is a forward electron microscope image of the titanium hydride transmission electron microscope sample after thinning in Example 1;

[0026] Figure 8 is a top view TEM image of the polycrystalline aluminum sample after thinning in Example 2;

[0027] Fig. 9 is a forward electron microscope image of the thinned polycrystalline aluminum TEM sample in Example 2;

[0028] Fig.10 is a transmission electron microscopic image of the polycrystalline aluminum transmission electron microscopic sample in Example 2;

[0029] In the figure: 1. Thin slice sample, 2. Sample transfer needle, 3. Micro-pillar, 4. Carbide; 11. Connection area, 12. Unthinned area, 13. Thinned area, 14. Nano-precipitates, 15. Grain boundary. DETAILED DESCRIPTION

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without any creative labor.

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods and drawings.

[0032] The method for preparing a 100-micron-level transmission electron microscope sample provided by the present invention comprises the following steps:

[0033] a. Cutting 100-micron thin slice samples

[0034] A carbide protective layer is deposited on the area to be sampled, and the carbide can be platinum carbide or inorganic carbide. The front, back, right, bottom and part of the left area of ​​the sample preparation area are cut by the focused ion beam method, and only the connection area with a width of no more than 2μm is retained on the left to ensure that the prepared 100-micron-level thin slice sample does not fall into the pit left after cutting the 100-micron-length thin slice sample. The thickness range and height range of the thin slice sample are 1μm to 3μm and 5μm to 20μm respectively. The distance between the front and back of the thin slice sample is the thickness, and the distance between the top and bottom of the thin slice sample is the height.

[0035] b. Bonding and extracting thin slice samples

[0036] Move the sample transfer needle with a tip less than 20μm to the top of the 100-micron thin sample and keep a certain gap with the top of the sample. To prevent the thin sample from falling off due to its own weight during the transfer process, the connection area between the sample transfer needle and the thin sample is the middle area at the top of the thin sample. The gap between the sample transfer needle and the thin sample ranges from 1μm to 3μm. Platinum carbide is deposited in the gap to bond the thin sample to the sample transfer needle. The purpose of controlling the gap range is to ensure that the sample is firmly bonded and to avoid long-term sample drift that may lead to bonding failure. Finally, cut off the remaining connection area on the left side of the thin sample, as shown in the schematic diagram. Figure 2 shown.

[0037] c. Transfer and fix thin slice samples

[0038] The thin slice sample is moved to the top of the microcolumn of the microgrid dedicated to the transmission electron microscope by using a sample transfer needle, and a certain gap is maintained with the top of the microcolumn. The width and thickness of the microcolumn range from 120μm to 200μm and 20μm to 50μm, respectively. To ensure that the sample is not blocked by the microcolumn during analysis, the thin slice sample is aligned in the middle area of ​​the width and thickness directions of the microcolumn. The gap between the thin slice sample and the top of the microcolumn ranges from 1μm to 3μm. Platinum carbide is deposited in the gap to bond the thin slice sample to the microcolumn. The purpose of controlling the gap range is to ensure that the sample is firmly bonded and to avoid sample drift for too long leading to bonding failure. Finally, the connection area between the thin slice sample and the sample transfer needle is cut off.

[0039] d. Thinning of thin slice samples

[0040] The front and back sides of the thin slice sample were cut by the focused ion beam method. To avoid bending or curling of the sample, unthinned areas of a certain width were retained on the left, right and bottom of the thin slice sample. The width of the unthinned areas retained on the left and right sides ranged from 2μm to 5μm, and the width of the unthinned areas retained on the bottom ranged from 1μm to 3μm. Finally, a hundred-micron-level transmission electron microscope sample was prepared, and the thickness of the transmission electron microscope sample was less than 100nm.

[0041] The focused ion beam microscope equipment used in the present invention is as follows:

[0042] Focused ion beam microscopy: A Scios 2 HiVac focused ion beam microscope from Thermofisher Scientific, USA, was used to thin the micronized particles and to perform microstructural analysis on the prepared micronized particle electron microscopy samples, with an acceleration voltage of 2 kV to 30 kV.

[0043] The experimental results show that the method for preparing 100-micron-scale transmission electron microscope samples of the present invention is a method for preparing ultra-large-scale transmission electron microscope samples with a length of 100 microns. This method overcomes the technical difficulties of bending, curling or damage of electron microscope samples in existing methods. The thickness of the transmission electron microscope samples prepared by this method is less than 100nm, which meets the requirements of transmission electron microscopy analysis. The analysis of large-scale 100-micron-scale electron microscope samples can increase the statistical understanding of the microstructure of the material, which is conducive to obtaining a more reliable understanding of the scientific mechanism.

[0044] Example 1

[0045] In this embodiment, a transmission electron microscope sample of titanium hydride with a length of 100 microns is prepared, and the specific steps are as follows:

[0046] Step 10: Cutting a 100-micron-long titanium hydride thin film sample

[0047] A platinum carbide protective layer was deposited on the sample preparation area, and the front, back, right and bottom areas of the sample preparation area, as well as part of the left area, were removed by using a Scios 2 HiVac focused ion beam microscope using a focused ion beam method. Only a connection area 11 with a width of no more than 2 μm was retained on the left side to prepare a titanium hydride thin sheet sample with a length of 100 microns. The thickness of the front and back sides and the top and bottom surface heights of the thin sheet sample 1 were 1.5 μm and 12 μm respectively. For specific results, see Figure 1 , Figure 1 The front, back, right and bottom of the medium-hundred-micron thin film sample 1 were cut off, and most of the left area was also cleared. Only a connecting area 11 with a width of no more than 2 μm was retained at the top left position to ensure that the thin film sample would not fall into the groove formed by the cutting.

[0048] Step 20: Bonding and extracting titanium hydride thin film samples

[0049] The sample transfer needle 2 with a tip less than 20 μm is moved to the top of the titanium hydride thin slice sample 1, and a 1 μm gap is maintained with the sample top 1. To prevent the thin slice sample 1 from falling off due to its own weight during the transfer process, the connection area 11 between the sample transfer needle 2 and the thin slice sample 1 is the middle area at the top of the thin slice sample 1. Platinum carbide is deposited in the gap to bond the titanium hydride thin slice sample 1 to the sample transfer needle 2, and finally the connection area 11 retained on the left side of the thin slice sample is cut off. Figure 2 The sample transfer needle 2 is shown moving to the top of the titanium hydride thin sheet sample 1 in preparation for bonding with the thin sheet sample 1 for extraction.

[0050] Step 30: Transfer and bonding of titanium hydride sheet samples

[0051] The sample transfer needle 2 is used to move the 100-micron titanium hydride thin slice sample 1 to the top of the micro-pillar 3 of the microgrid for transmission electron microscopy, and a gap of 1.5 μm is maintained with the top of the micro-pillar 3. The width and thickness of the micro-pillar 3 are 130 μm and 25 μm respectively. To ensure that the sample is not blocked by the micro-pillar during analysis, the thin slice sample is aligned to the middle area in the width and thickness directions of the micro-pillar 3. Carbide 4, such as platinum carbide, is deposited in the gap to bond the titanium hydride thin slice sample 1 to the micro-pillar 3, and finally the connection area between the thin slice sample 1 and the sample transfer needle 2 is cut off. Figure 3 The figure shows the process of the sample transfer needle 2 transferring the thin sheet sample 1 to the micro-pillar 3 and then separating from the thin sheet after the bonding is completed. The bottom of the thin sheet sample 1 is bonded to the micro-pillar 3, and the entire sample is relatively flat in shape.

[0052] Step 40: Thinning of titanium hydride sheet sample

[0053] The front and back sides of the 100-micron titanium hydride thin slice sample 1 were cut and thinned by the focused ion beam method. In order to avoid bending or curling of the sample, in addition to fixing the bottom of the thin slice sample 1 and the top of the microcolumn 3 in the previous step, it is necessary to retain a certain width of unthinned area 12 on the left, right and bottom of the thin slice sample 1 during thinning to enhance the overall rigidity of the thinned sample 1 to resist the bending and curling effects caused by the stress generated during the thinning process. Among them, the width of the unthinned area 12 retained on the left and right sides is 3μm, and the width of the unthinned area 12 retained on the bottom is 1μm, and finally a 100-micron titanium hydride transmission electron microscope sample is prepared. Figure 4 This is a positive magnified view of the thin slice sample 1 after being bonded to the microgrid microcolumn 3 for transmission electron microscopy and thinned. It can be seen from the figure that the bottom surface of the thin slice sample 1 and the top surface of the microcolumn 3 are bonded and fixed by the sediment, and a certain width of unthinned area is left on the left and right sides of the thin slice sample 1 and near the bottom of the microcolumn. Figure 5 This is an axial view of the 1 / 2 thin slice sample transmission electron microscope sample 1. The view more clearly shows the relationship between the thinned area and the non-thinned area, where the thinned area 13 needs to be thinned on both the front and rear sides. The thinning process is best to alternately thin the front and rear sides gradually to the required thickness.

[0054] The test results are as follows:

[0055] Figure 6 This is a top-down electron microscope image of a thinned titanium hydride transmission electron microscope sample. The total length of the electron microscope sample is 100 μm. The entire electron microscope sample is very straight, with no visible bending or curling. Figure 7This is the forward electron microscope image of the titanium hydride transmission electron microscope sample after thinning. The entire view shows that there is no damage in the thinned area and it is transparent under 30kV electron beam irradiation, indicating that the thickness of the electron microscope sample meets the requirement of less than 100nm. The width of the entire thinned area can reach more than 100 microns in width and 11μm in height. With such a large observation area, statistical analysis of the microstructure of titanium hydride can be fully realized.

[0056] Example 2

[0057] In this embodiment, a transmission electron microscope sample of polycrystalline aluminum with a length of 100 microns is prepared. The specific implementation method is basically the same as that of Example 1, with the main differences being that the carbide 4 is an inorganic carbide, the thickness and height of the thin slice sample 1 are 2 μm and 16 μm respectively, the gap between the sample transfer needle 2 and the thin slice sample 1 is 2 μm, the gap between the thin slice sample 1 and the top of the microcolumn 3 is 2 μm, the unthinned area 12 retained on the left and right sides of the thin slice sample 1 is 2 μm in width, and the unthinned area 12 retained at the bottom is 2 μm in width.

[0058] The test results are as follows:

[0059] Figure 8 This is a top-down electron microscope image of a thinned polycrystalline aluminum transmission electron microscope sample. The total length of the electron microscope sample is 100μm, and the entire sample is very straight in shape without obvious bending or curling. Fig. 9 This is the forward electron microscope image of the polycrystalline aluminum transmission electron microscope sample after thinning. From the image, it can be seen that there is no damage in the entire thinned area, and the entire thinned area appears transparent under 30kV electron beam irradiation, indicating that the thickness of the electron microscope sample meets the requirement of less than 100nm. The width of the entire thinned area can reach more than 100 microns in width and 14μm in height. Such a large observation area can realize statistical analysis of the microstructure of titanium hydride. Fig.10 This is a transmission electron microscopic image of the polycrystalline aluminum transmission electron microscope sample in Example 2. In the image, a nano-precipitated phase 14 with a scale of about 20 nm can be clearly observed, and a grain boundary 15 in the sample can also be observed in the entire thinning area, further confirming that the sample thickness prepared by the 100-micron transmission electron microscope sample preparation method of the present invention meets the basic requirement of 100 nm. It can be seen that the 100-micron thinning area not only shows rich and real structural information of the material, but also fully meets the statistical characteristics of material analysis.

Claims

1. A method for preparing a 100-micron-level transmission electron microscope sample, characterized in that: The following steps are involved: S10 cutting of 100-micron thin slice samples: depositing a carbide protective layer on the area to be prepared, using a focused ion beam method to cut the front, back, right, bottom and left part of the thin slice sample to prepare a 100-micron wide thin slice sample, wherein a connection area of ​​a certain width is reserved on the left side of the thin slice sample to ensure that the thin slice sample does not fall into the pit formed during the cutting of the thin slice sample, wherein the width is the distance between the left and right sides of the thin slice sample; S20 bonding and extracting the thin slice sample: moving a sample transfer needle with a tip less than 20 μm to the top of the thin slice sample, and keeping a certain gap with the top of the sample, depositing platinum carbide in the gap to bond the thin slice sample to the sample transfer needle, and then cutting off the reserved connection area on the left side of the thin slice sample; S30: Transfer and fix the thin slice sample: Use the sample transfer needle to move the thin slice sample to the top of the micro-column of the micro-grid for transmission electron microscopy, and keep a certain gap with the top of the micro-column, deposit platinum carbide in the entire gap to bond the thin slice sample to the micro-column, and cut off the connection area between the thin slice sample and the sample transfer needle; S40 thin slice sample thinning: the front and back sides of the 100-micron thin slice sample are cut by the focused ion beam method. To avoid bending or curling of the sample, unthinned areas of a certain width are retained on the left, right and bottom of the thin slice sample. The width of the unthinned areas retained on the left and right sides ranges from 2μm to 5μm, and the width of the unthinned areas retained on the bottom ranges from 1μm to 3μm. The thickness of the prepared transmission electron microscope sample is less than 100nm, i.e., a 100-micron transmission electron microscope sample is obtained.

2. The method for preparing a 100-micron-level transmission electron microscope sample according to claim 1, characterized in that: In the step S10, the thickness of the thin slice sample ranges from 1 μm to 3 μm, and the height of the thin slice sample ranges from 5 μm to 20 μm.

3. The method for preparing a 100-micron-level transmission electron microscope sample according to claim 1, characterized in that: In the step S10, the width of the left connecting area of ​​the thin slice sample is no more than 2 μm, and the carbide is platinum carbide or inorganic carbide.

4. The method for preparing a 100-micron-level transmission electron microscope sample according to claim 1, characterized in that: In step S20, the bonding area between the sample transfer needle and the thin slice sample is the middle area on the top of the thin slice sample, so as to ensure that the thin slice does not fall off during the transfer process due to its own weight.

5. The method for preparing a 100-micron-level transmission electron microscope sample according to claim 1, characterized in that: The micro-grid micro-columns for transmission electron microscopy described in step S30 have a width range of 120 μm to 200 μm and a thickness range of 20 μm to 50 μm. The thin slice sample is aligned in the middle area of ​​the micro-column width direction and the thickness direction to ensure that the sample is not blocked by the micro-column during analysis.

6. The method for preparing a 100-micron-level transmission electron microscope sample according to claim 1, characterized in that: The width of the unthinned areas retained on the left and right sides in step S40 ranges from 2 μm to 5 μm, the width of the unthinned area retained at the bottom ranges from 1 μm to 3 μm, and the thickness of the prepared transmission electron microscope sample is less than 100 nm.

7. The method for preparing a 100-micron-level transmission electron microscope sample according to claim 1, characterized in that: When the sample transfer needle is bonded to the thin slice sample in step S20, and when the thin slice sample is fixed to the top of the microcolumn in step S30, the gap between the sample transfer needle and the thin slice sample ranges from 1 μm to 3 μm, ensuring that the thin slice sample is firmly bonded and avoiding bonding failure caused by sample drift for too long.