A rubber magnetic material and its preparation method and application
By using composite adhesives of nitrile rubber and acrylate rubber in high-speed micro motors for high-temperature stacking vulcanization, the problem of damage to ordinary rubber magnetic strips at high speed is solved, and the high tensile strength of the material is achieved Temperature resistance, meets the requirements of high-speed motors.
Patent Information
- Application Number
- CN202210492858.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-05-07
AI Technical Summary
In high-speed micro motors, ordinary unvulcanized rubber magnetic strips are prone to breakage when rotating at high speed, and their tensile strength and temperature resistance are insufficient, which limits the high-speed and high-power development of permanent magnet motors.
Using a rubber magnetic material preparation method, by mixing nitrile rubber and acrylate rubber into a composite adhesive in a specific proportion, high-temperature stacking and vulcanization are carried out to ensure uniform dispersion and high filling degree of magnetic powder in the composite adhesive. Improve the tensile strength and winding properties of the material.
The prepared rubber magnetic material does not crack under long-term high temperature and high speed rotation, meets the requirements of high-speed motors, has significantly improved tensile strength and temperature resistance, and is suitable for high-speed micro motors.
Smart Images

Figure GDA0005049193070000121 
Figure GDA0005049193070000131 
Figure GDA0005049193070000132
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of permanent magnets, and in particular to a rubber magnetic material and a preparation method and application thereof. Background Art
[0002] High-speed micro motors usually refer to motors with rotor speeds higher than 10,000 r / min. High-speed micro motors are widely used in household air conditioners, refrigerators, communication base stations, automobiles and ships, and small electronic products such as electric toothbrushes, facial cleansers, beauty devices, electric toys, massagers, etc. also use high-speed micro motors.
[0003] The housing of the high-speed micro motor is provided with a ring-shaped rotor that can be magnetized, and a magnetic strip is provided on the ring-shaped rotor. The magnetic strip is fixed inside the housing, and after power is turned on, it will rotate at high speed with the motor housing. Under high-speed rotation, ordinary unvulcanized rubber magnetic strips cannot withstand the centrifugal force generated by the high-speed rotation of the motor, and will be damaged or broken. The physical properties of the rubber magnetic strips vulcanized by the vulcanization process will have a significant improvement in tensile strength, but because the rubber magnetic strips used in the motor need to be bent into a ring for use, it must be ensured that they have appropriate bending properties (indicates the degree of bending into a minimum diameter ring under the premise that the rubber magnetic strips have no cracks). Increasing the degree of vulcanization cross-linking can make the rubber magnetic strips have stronger tensile strength, but they are prone to cracking when bent. The tensile strength and anti-deformation ability of the rubber magnetic strips increased by the vulcanization cross-linking process alone cannot be adapted to the use of motors. Ordinary unvulcanized rubber magnetic strips have good bending properties and can be installed in motors for use, but their low tensile strength, large dimensional changes, and poor temperature resistance restrict the development of permanent magnet motors in the direction of high speed and high power. The research and development of rubber magnetic strips that can be applied to micro motors, have higher tensile strength, smaller high-temperature deformation, and good bending properties are of great significance to the development of high-speed motors. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing a rubber magnetic material. The obtained rubber magnetic material has significantly better tensile strength and temperature resistance than traditional rubber permanent magnet materials, and has good bending properties. It can withstand long-term high temperature and high-speed rotation without cracking, and can meet the requirements of high-speed motors.
[0005] At the same time, the invention also provides the rubber magnetic material obtained by the preparation method and the application thereof.
[0006] Specifically, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention is to provide a method for preparing a rubber magnetic material, comprising the following steps:
[0008] The magnetic powder and the composite binder are mixed once to obtain a primary mixed material; the composite binder comprises, by mass percentage, 75% to 90% of nitrile rubber (NBR) and 10% to 25% of acrylic rubber (ACM);
[0009] The primary mixed material is mixed with a coupling agent and then subjected to secondary mixing to obtain a secondary mixed material;
[0010] Calendering the secondary mixed material;
[0011] The formed product is laminated, and the temperature of the lamination process is increased from 50 to 60° C. to 100 to 105° C.;
[0012] The laminated product is vulcanized to obtain the rubber magnetic material.
[0013] The preparation method according to the first aspect of the present invention has at least the following beneficial effects:
[0014] The present invention utilizes the characteristics of ACM and NBR having similar solubility parameters and good thermodynamic compatibility, and uses NBR and a small amount of ACM to prepare a composite binder, thereby ensuring that magnetic powder can be evenly dispersed in the composite binder during mixing, and also avoiding the distribution of a vulcanizing agent and an accelerator in two phases during subsequent vulcanization, and the difference in vulcanization speeds in the two phases leading to asynchronous vulcanization speeds of the two phases, and a large difference in the vulcanization degree of the two phases, resulting in low mechanical properties of the product.
[0015] Adding coupling agent after mixing can solve the problem of uneven dispersion and agglomeration of magnetic powder and binder in a single mixing, and prevent installation cracks caused by surface expansion bubbles and deterioration of winding during subsequent vulcanization treatment after molding.
[0016] When laminating under continuous high temperature, the viscosity of the composite binder decreases and becomes a flowing state. At this time, the composite binder spreads and flows in the magnetic powder. The internal friction of the composite binder when flowing is relatively small, and the friction between the magnetic powder particles and between the binder and the magnetic powder particles is not very large. At the same time, under multiple double-roller mechanical orientation stresses, the magnetic powder particles are easier to rotate and slide, and are easy to orient along the calendering direction. The porosity between the magnetic powder particles is effectively reduced, the filling degree is improved, and the material has higher magnetic properties. Under high temperature and high mechanical pressure, the binder and the magnetic powder are more densely combined, and high-temperature vulcanization is immediately carried out after continuous high-roller temperature lamination. The temperature inside and outside the magnetic film is stable and consistent. During vulcanization, the rubber magnet is evenly cross-linked inside and outside, and can be made into a rubber magnetic material for high-speed motors that is compatible with tensile strength and winding properties.
[0017] In some examples of the present invention, the composite adhesive comprises, by mass percentage, 80% to 90% of nitrile rubber (NBR) and 10% to 20% of acrylic rubber (ACM); preferably 82% to 88% of nitrile rubber (NBR) and 12% to 18% of acrylic rubber (ACM); more preferably about 85% of nitrile rubber (NBR). About 15% of acrylic rubber (ACM). The "about" mentioned here means that there may be a certain error, and the error is acceptable within ±0.5%. For example, "about 85%" means a value of (85±0.5)%.
[0018] In some examples of the present invention, the acrylonitrile content in the nitrile rubber is 30% to 40%, for example, NBR3606 with an acrylonitrile content of 36% can be used; the acrylate rubber includes epoxy-type acrylate rubber, for example, ACM-62 can be used.
[0019] In some embodiments of the present invention, the preparation of the composite adhesive comprises the following steps: kneading nitrile rubber and acrylate rubber to obtain the composite adhesive. The kneading temperature of the nitrile rubber and acrylate rubber is 110-140° C., preferably 120-130° C., and the time is 18-20 minutes.
[0020] In some embodiments of the present invention, the primary mixing material includes the following components in percentage by weight:
[0021] Magnetic powder 80%~95%
[0022] Composite binder 4%~20%
[0023] Additives 0.5%~3%.
[0024] In some embodiments of the present invention, the primary mixing material includes the following components in percentage by weight:
[0025] Magnetic powder 80%~90%
[0026] Composite binder 9%~17%
[0027] Additives 1%~3%.
[0028] In some examples of the present invention, the magnetic powder includes at least one of anisotropic strontium ferrite magnetic powder, isotropic strontium ferrite magnetic powder, anisotropic barium ferrite magnetic powder, and isotropic barium ferrite magnetic powder.
[0029] In some examples of the present invention, the auxiliary agent includes at least one of a lubricant, an antioxidant, a plasticizer, a vulcanizing agent, and an accelerator. The lubricant includes stearic acid, paraffin, zinc stearate, vegetable oil, etc. The antioxidant includes antioxidant RD (2,2,4-trimethyl-1,2-dihydroquinoline polymer), antioxidant D (N-phenyl-2-naphthylamine), antioxidant MB (2-mercaptobenzimidazole), microcrystalline wax, etc. The plasticizer includes trioctyl trimellitate, dibutyl phthalate, dioctyl phthalate, etc. The vulcanizing agent includes sulfur, metal oxides (such as magnesium oxide), peroxides (such as diisopropyl peroxide, i.e., vulcanizing agent DCP), etc. The accelerator includes tetramethylthiuram disulfide TMTD, etc.
[0030] In some embodiments of the present invention, the primary mixing material includes the following components in percentage by weight:
[0031] Magnetic powder 80%~95%
[0032] Composite binder 4%~20%
[0033] Lubricant 0.05%~0.5%
[0034] Anti-aging agent 0.05%~0.1%
[0035] Vulcanizing agent 0.05%~0.5%
[0036] Accelerator 0.05%~0.1%.
[0037] In some examples of the present invention, the mass of the coupling agent is 0.5% to 1% of the primary mixed material.
[0038] In some examples of the present invention, considering the control of silicon elements in the motor, the coupling agent is a non-silane coupling agent, including at least one of a titanate coupling agent and an aluminate compound.
[0039] In some examples of the present invention, the method for preparing the rubber magnetic material specifically comprises the following steps:
[0040] The magnetic powder, the composite binder and the additive are mixed once to obtain a primary mixed material;
[0041] The primary mixed material is crushed into primary mixed granules, a coupling agent is sprayed into the primary mixed granules, and then secondary mixed is performed to obtain a secondary mixed material;
[0042] crushing the secondary mixed material and rolling it into thin sheets;
[0043] Laminating a plurality of the thin sheets;
[0044] The laminated product is vulcanized to obtain the rubber magnetic material.
[0045] In some embodiments of the present invention, the temperature of the first mixing is 120-150° C., preferably 120-140° C.; the time is 10-20 min, preferably 15-18 min.
[0046] In some embodiments of the present invention, the primary mixed material is crushed after being cooled to 100-110° C. The pellets after crushing the primary mixed material have a particle size of 0.3-2 mm, preferably 0.5-1.0 mm.
[0047] In some examples of the present invention, the coupling agent is added to the primary mixed granules by spraying, and the spraying process is accompanied by stirring, and the stirring time is 10 to 30 minutes.
[0048] In some embodiments of the present invention, the secondary mixing is performed at a temperature of 100 to 120° C. for 10 to 20 minutes, preferably 10 to 12 minutes.
[0049] In some examples of the present invention, the secondary mixed material has a particle size of 1 to 5 mm, preferably 2 to 4 mm after crushing.
[0050] In some embodiments of the present invention, the temperature of the calendering process is 60-80° C., preferably 65-75° C. This step is performed using a double-roll calender. The mechanical stress orientation is performed by calendering to improve the magnetic properties.
[0051] In some examples of the present invention, the thickness of the sheet is 0.5-2 mm, preferably 1.0-1.4 mm.
[0052] In some examples of the present invention, the lamination process is specifically: the formed product (several sheets) is laminated through at least five double-roll calenders in sequence, and the roller temperature of the first calender gradually increases to the roller temperature of the last calender, the roller temperature of the first calender is 50-60°C, and the roller temperature of the last calender is 100-105°C. Preferably, the formed product (several sheets) is laminated through five double-roll calenders in sequence, the roller temperature of the first calender is 50-60°C, the roller temperature of the second calender is 70-80°C, the roller temperature of the third calender is 80-90°C, the roller temperature of the fourth calender is 100-105°C, and the roller temperature of the fifth calender is 100-105°C.
[0053] In some embodiments of the present invention, during the lamination process, the lamination is performed at a thickness reduction of 1.5 to 2 times. The thickness reduction during the lamination process is 1.5 to 2 times. That is, the thickness reduction is 1.5 to 2 times the thickness after lamination. For example, after a 6.0 mm thick sheet is calendered by 5 calenders, the final thickness is 2.0 mm (the thickness reduction in this process is 4 mm, which is twice the final thickness of 2 mm).
[0054] In some embodiments of the present invention, the number of sheets used for lamination is 3 to 10 sheets, preferably 5 to 9 sheets, and more preferably 6 to 8 sheets.
[0055] In some embodiments of the present invention, the vulcanization temperature is 150-180° C., preferably 155-170° C., and the vulcanization time is 10-30 min, preferably 10-20 min. The vulcanization method can be a hot air continuous vulcanization method.
[0056] The second aspect of the present invention is to provide the rubber magnetic material obtained by the above preparation method.
[0057] The third aspect of the present invention is to provide the use of the rubber magnetic material in manufacturing a motor.
[0058] In some examples of the present invention, the motor is a high-speed micro motor, and its rotor speed is higher than 10000r / min.
[0059] More specifically, the rubber magnetic material is used to make magnetic strips on the rotor in the motor. The magnetic strips made of the rubber magnetic material rotate with the rotor at high speed and do not crack under high-speed rotation, which can meet the requirements of high-speed motors.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] The present invention utilizes the characteristics of ACM and NBR having similar solubility parameters and good thermodynamic compatibility, and uses NBR and a small amount of ACM together. First, ACM and NBR are blended at high temperature to form a polymer blend, so that the two phases are fully diffused and fused into a composite binder, ensuring that the magnetic powder and additives added during mixing can be evenly distributed in the composite binder. It can also avoid the distribution of the vulcanizer and the accelerator in the two phases during subsequent vulcanization, the difference in the vulcanization speed in the two phases leading to the asynchronous vulcanization speed of the two phases, and the large difference in the vulcanization degree of the two phases, resulting in low mechanical properties of the product.
[0062] After the first mixing, the powder is crushed into fine particles, and the coupling agent is added while stirring, in order to solve the problem of uneven dispersion and agglomeration of magnetic powder and binder in a single mixing, and to prevent the occurrence of surface expansion bubbles and installation cracks caused by deterioration of winding during the subsequent cross-linking treatment after molding.
[0063] A composite binder composed of ACM with good high temperature resistance and NBR rubber with good processing performance is used, and the magnetic powder and additives are mixed and calendered into thin sheets. When multiple sheets of magnetic rubber sheets are stacked, the viscosity of the magnetic film binder decreases under the heat conduction of the high roller temperature double rollers, and it becomes a flowing state. At this time, the binder spreads and flows in the magnetic powder, and the internal friction of the binder when flowing will be relatively small. The friction between the magnetic powder particles and between the binder is not very large. At the same time, under multiple double roller mechanical orientation stresses, the magnetic powder particles are easier to rotate and slide, and are easy to be oriented and arranged along the calendering direction, and the porosity between the magnetic powder particles is effectively reduced, the filling degree is improved, and the magnetic strip has higher magnetic properties. Under high temperature and high mechanical pressure, the binder and the magnetic powder are more densely combined, and high temperature vulcanization is immediately carried out after continuous high roller temperature lamination. The temperature inside and outside the magnetic film is stable and consistent. During vulcanization, the rubber magnet is evenly cross-linked inside and outside, and can be made into a rubber magnetic strip for high-speed motors with comprehensive compatibility of tensile strength and winding properties. DETAILED DESCRIPTION
[0064] The technical scheme of the present invention is further described below in conjunction with specific examples. The raw materials used in the following examples, unless otherwise specified, can all be obtained from conventional commercial sources; the processes used, unless otherwise specified, all adopt conventional processes in the art.
[0065] Embodiment 1
[0066] A magnetic strip for a high-speed micro motor, the raw material formula of which is:
[0067] NBR3606: 850g;
[0068] ACM-62: 150g;
[0069] Strontium ferrite magnetic powder: 10kg;
[0070] Titanate (coupling agent): 20g;
[0071] Zinc stearate (auxiliary agent): 10g;
[0072] Anti-aging agent MB (auxiliary agent): 10g;
[0073] Magnesium oxide (auxiliary agent): 20g;
[0074] DCP (auxiliary agent): 10g;
[0075] TMTD (auxiliary agent): 10g.
[0076] After weighing the weight of each material according to the above formula, first put ACM and NBR into the open mill and mix them evenly to 120℃, then cool them to make a composite binder. Add magnetic powder, additives, and composite binder to the internal mixer and mix them evenly to 135℃, then stir and cool them to 110℃, then pour them into the crusher and crush them into granules, add 0.5% mass ratio of coupling agent to the granules in the stirring tank by spraying, mix the granules with the internal mixer to 110℃ again, pour them into the crusher and crush them into granules, and produce 1.2mm thin sheets on the double-roll calender, and the calender roller temperature is 70℃. The 7 thin sheets are continuously stacked through 5 calenders, and the roller temperatures of the 5 calenders are: 50℃, 70℃, 80℃, 100℃, and 105℃ respectively. Finally, they are pressed into a thickness of 2.0mm. Then immediately put them into a 160℃ vulcanization furnace for vulcanization for 15 minutes, then take them out and cool them. Cut into appropriate sizes for magnetic properties, physical properties, flexibility, and high-speed installation tests.
[0077] Comparative Example 1
[0078] A magnetic strip for a high-speed micro motor, whose raw material formula is the same as that in Example 1, and whose preparation method is different from that in Example 1 in that: in the calendering step, the roller temperatures of 5 calenders are: 30°C, 30°C, 30°C, 30°C, 30°C, respectively.
[0079] Raw material formula:
[0080] NBR3606: 850g;
[0081] ACM-62: 150g;
[0082] Strontium ferrite magnetic powder: 10kg;
[0083] Titanate: 20g;
[0084] Zinc stearate: 10g;
[0085] Anti-aging agent MB: 10g;
[0086] Magnesium oxide: 20g;
[0087] DCP: 10g;
[0088] TMTD:10g.
[0089] After weighing the weight of each material according to the above formula, first put ACM and NBR into the open mill and mix them evenly to 120℃, then cool them to make a composite binder. Add magnetic powder, additives, and composite binder to the internal mixer and mix them evenly to 135℃, then stir and cool them to 110℃, then pour them into the crusher and crush them into granules. Add 0.5% mass ratio of coupling agent to the granules in the stirring tank by spraying, mix the granules with the internal mixer to 110℃ again, pour them into the crusher and crush them into granules, and produce 1.2mm thin sheets on the double-roll calender, and the calender roller temperature is 70℃. The 7 thin sheets are continuously stacked through 5 calenders, and the roller temperatures of the 5 calenders are: 30℃, 30℃, 30℃, 30℃, 30℃, and 30℃. Finally, they are pressed into a thickness of 2.0mm. Then immediately put them into a 160℃ vulcanization furnace for vulcanization for 15 minutes, then take them out and cool them. Cut into appropriate sizes for magnetic properties, physical properties, flexibility, and high-speed installation tests.
[0090] Comparative Example 2
[0091] A magnetic strip for a high-speed micro motor, the raw material formula of which is the same as that of the first embodiment, and the preparation method thereof is different from that of the first embodiment in that no vulcanization step is performed after calendering.
[0092] Raw material formula:
[0093] NBR3606: 850g;
[0094] ACM-62: 150g;
[0095] Strontium ferrite magnetic powder: 10kg;
[0096] Titanate: 20g;
[0097] Zinc stearate: 10g;
[0098] Anti-aging agent MB: 10g;
[0099] Magnesium oxide: 20g;
[0100] DCP: 10g;
[0101] TMTD:10g.
[0102] After weighing the weight of each material according to the above formula, first put ACM and NBR into the open mill and mix them evenly to 120℃, then cool them to make a composite binder. Add magnetic powder, additives, and composite binder to the internal mixer and mix them evenly to 135℃, then stir and cool them to 110℃, then pour them into the crusher and crush them into granules. Add 0.5% mass ratio of coupling agent to the granules in the stirring tank by spraying, mix the granules with the internal mixer to 110℃ again, pour them into the crusher and crush them into granules, and produce 1.2mm thin sheets on the double-roll calender, and the calender roller temperature is 70℃. The 7 thin sheets are continuously stacked through 5 calenders, and the roller temperatures of the 5 calenders are: 50℃, 70℃, 80℃, 100℃, and 105℃ respectively. Finally, they are pressed into a thickness of 2.0mm. After cooling, cut them into suitable sizes for magnetic properties, physical properties, winding properties, and high-speed installation tests.
[0103] Comparative Example 3
[0104] A magnetic strip for a high-speed micro motor, the preparation method of which is the same as that of the first embodiment, and the difference between the raw material formula and the first embodiment is that the amount of NBR is reduced and the amount of ACM is increased.
[0105] Raw material formula:
[0106] NBR3606: 700g;
[0107] ACM-62: 300g;
[0108] Strontium ferrite magnetic powder: 10kg;
[0109] Titanate: 20g;
[0110] Zinc stearate: 10g;
[0111] Anti-aging agent MB: 10g;
[0112] Magnesium oxide: 20g;
[0113] DCP: 10g;
[0114] TMTD:10g.
[0115] After weighing the weight of each material according to the above formula, first put ACM and NBR into the open mill and mix them evenly to 120℃, then cool them to make a composite binder. Add magnetic powder, additives, and composite binder to the internal mixer and mix them evenly to 135℃, then stir and cool them to 110℃, then pour them into the crusher and crush them into granules, add 0.5% mass ratio of coupling agent to the granules in the stirring tank by spraying, mix the granules with the internal mixer to 110℃ again, pour them into the crusher and crush them into granules, and produce 1.2mm thin sheets on the double-roll calender, and the calender roller temperature is 70℃. The 7 thin sheets are continuously stacked through 5 calenders, and the roller temperatures of the 5 calenders are: 50℃, 70℃, 80℃, 100℃, and 105℃ respectively. Finally, they are pressed into a thickness of 2.0mm. Then immediately put them into a 160℃ vulcanization furnace for vulcanization for 15 minutes, then take them out and cool them. Cut into appropriate sizes for magnetic properties, physical properties, flexibility, and high-speed installation tests.
[0116] Comparative Example 4
[0117] A magnetic strip for a high-speed micro motor, the preparation method of which is the same as that of the first embodiment, and the raw material formula thereof is different from that of the first embodiment in that it does not contain ACM.
[0118] Raw material formula:
[0119] NBR3606: 1000g;
[0120] ACM-62: 0g;
[0121] Strontium ferrite magnetic powder: 10kg;
[0122] Titanate: 20g;
[0123] Zinc stearate: 10g;
[0124] Anti-aging agent MB: 10g;
[0125] Magnesium oxide: 20g;
[0126] DCP: 10g;
[0127] TMTD:10g.
[0128] After weighing the weight of each material according to the above formula, add it to the internal mixer and mix it evenly to 135℃, then stir and cool it to 110℃, then pour it into the crusher to crush it into granules, add 0.5% mass ratio of coupling agent to the granules in the stirring tank by spraying, mix the granules with the internal mixer to 110℃ again, pour it into the crusher to crush it into granules, and produce 1.2mm thin sheets on the double-roll calender, and the roller temperature of the calender is 70℃. The 7 thin sheets are continuously stacked through 5 calenders, and the roller temperatures of the 5 calenders are: 50℃, 70℃, 80℃, 100℃, and 105℃ respectively. Finally, it is pressed into a thickness of 2.0mm. Then immediately put it into a 160℃ vulcanization furnace for vulcanization for 15 minutes, take it out, and cool it. Cut it into suitable sizes for magnetic properties, physical properties, winding, and high-speed installation tests.
[0129] Comparative Example 5
[0130] A magnetic strip for a high-speed micro motor, the raw material formula of which is the same as that of the first embodiment, and the preparation method thereof is different from that of the first embodiment in that no coupling agent is added before calendering.
[0131] Raw material formula:
[0132] NBR3606: 850g;
[0133] ACM-62: 150g;
[0134] Strontium ferrite magnetic powder: 10kg;
[0135] Titanate: 20g;
[0136] Zinc stearate: 10g;
[0137] Anti-aging agent MB: 10g;
[0138] Magnesium oxide: 20g;
[0139] DCP: 10g;
[0140] TMTD:10g.
[0141] After weighing the weight of each material according to the above formula, first put ACM and NBR into the open mill and mix them evenly to 120℃, then cool them to make a composite binder. Add magnetic powder, additives, and composite binder to the internal mixer and mix them evenly to 135℃, then stir and cool them to 110℃, then pour them into the crusher and crush them into granules, and then produce 1.2mm thin sheets on the double-roll calender, and the roller temperature of the calender is 70℃. The 7 thin sheets are continuously stacked through 5 calenders, and the roller temperatures of the 5 calenders are: 50℃, 70℃, 80℃, 100℃, and 105℃ respectively. Finally, they are pressed into a thickness of 2.0mm. Then immediately put them into a 160℃ vulcanization furnace for vulcanization for 15 minutes, take them out, and cool them. Cut them into suitable sizes for magnetic properties, physical properties, winding properties, and high-speed installation tests.
[0142] Comparative Example 6
[0143] Take the conventional vulcanized motor rubber magnetic strips on the market.
[0144] The performance of the magnetic strips in the various embodiments was tested, and the test results are shown in Tables 1 to 3 below.
[0145] Table 1: Magnetic properties and bending test results of magnetic strips
[0146]
[0147]
[0148] The bendability test method is: bend the magnetic strip on different specifications of shafts with a diameter of 2mm, bend it into a circle and observe its surface condition, and record the maximum diameter of the magnetic strip without cracks on the surface. For example, bending Φ14 means that the magnetic strip has no cracks on the surface when bent on a shaft with a diameter of Φ14, but cracks will appear on a shaft with a diameter of Φ12. Because the magnetic strip in the micro motor needs to be bent into a ring, the magnetic strip must have a certain degree of bendability.
[0149] Table 2: Physical properties and density test results of magnetic stripe
[0150]
[0151] Table 3: Magnetic stripe high speed test results
[0152]
[0153] The components of the finished micro motor are assembled very compactly. To ensure that the motor runs at high speed for a long time without any faults, the magnetic strip used in the actual high-speed motor must meet the requirement that the height change of the magnetic strip after it is installed in the casing is △h≤0.120mm, so that it will not touch other motor parts and cause parts damage, cracking, jamming and other faults. When the height change of the magnetic strip after it is installed in the casing is 0.120mm<△h≤0.200mm, a small number of motors will have the phenomenon that the magnetic strip is higher than the casing and touches the circuit board after long-term operation. When the height change of the magnetic strip after it is installed in the casing is △h>0.200mm, some motors will have faults such as magnetic strip breakage and jamming after long-term operation.
[0154] Test method: After the magnetic strip is installed in the housing of the micro motor, the micro motor is started and under the action of high-speed centrifugal force, if the tensile strength and temperature resistance of the magnetic strip are poor, the magnetic strip will be deformed or broken. By testing the deformation or cracking of the magnetic strip under high temperature and high speed for a long time after the magnetic strip is installed in the housing, the reliability difference of different magnetic strips can be compared. After a continuous test at 70℃×25000rpm×100 hours, if the height change of the magnetic strip after installation is less than 0.120mm and the magnetic strip does not break, it can be judged that it meets the requirements of high-speed motors.
[0155] From the test results in Table 1 above, it can be seen that the magnetic properties of the magnetic strip prepared in Example 1 are the same as those of conventional motor magnetic strips, and its bending performance is also better than that of conventional motor magnetic strips. From Comparative Example 3, it can be seen that increasing the ACM content will lead to poor processing performance and unqualified bending performance.
[0156] From the test results in Table 2, it can be seen that by adding high-temperature lamination and vulcanization process (Example 1), the physical properties of the rubber magnetic strip are significantly better than those of the rubber magnetic strip without vulcanization (Comparative Example 2) or normal temperature lamination process (Comparative Example 1).
[0157] From the high-speed test results in Table 3, it can be seen that the magnetic strip prepared in Example 1 has the smallest deformation under high temperature, high speed and long-term operation, △h is only 0.083mm, less than 0.120mm, and the magnetic strip has no cracking or damage. In Comparative Example 1, room temperature lamination and high-temperature vulcanization are adopted, and the vulcanization is uneven inside and outside. The magnetic strip will be greatly deformed at high temperature and high speed, △h>0.120mm. Comparative Example 2 was not vulcanized, and the deformation was large and cracking occurred. Comparative Example 3 adopts high-temperature lamination and then vulcanization. Although the magnetic strip has a small deformation under the high-speed test of installation, because the magnetic strip prepared in Comparative Example 3 is poorly bent, cracks appear when it is bent into a circle and installed in the casing, and it is actually not suitable for motors. Comparative Example 4 uses NBR alone as a binder, and the deformation is large and cracking occurs. Comparative Example 5 is not treated with a crushing coupling agent and then mixed twice. After cross-linking, expansion bubbles appear on the surface of the magnetic strip, and cracks appear after being installed in the casing, which cannot be actually used in motors. It can be concluded that the magnetic strip prepared in Example 1 can meet the use requirements of high-speed motor magnetic strips in all aspects.
[0158] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a rubber magnetic material, characterized in that: The steps include: The magnetic powder and the composite binder are mixed once to obtain a primary mixed material; the composite binder comprises, by mass percentage, 75% to 90% of nitrile rubber and 10% to 25% of acrylate rubber; The primary mixed material is mixed with a coupling agent and then subjected to secondary mixing to obtain a secondary mixed material; Calendering the secondary mixed material; Laminating the formed product; The lamination process is specifically as follows: the formed product is laminated by passing through five double-roll calenders in sequence, and the roller temperature of the first calender gradually increases to the roller temperature of the last calender; the roller temperature of the first calender is 50-60°C, the roller temperature of the second calender is 70-80°C, the roller temperature of the third calender is 80-90°C, the roller temperature of the fourth calender is 100-105°C, and the roller temperature of the fifth calender is 100-105°C; vulcanizing the laminated product to obtain the rubber magnetic material; The mass of the coupling agent is 0.5% to 1% of the primary mixed material; The coupling agent includes at least one of a titanate coupling agent and an aluminate compound; The vulcanization temperature is 150-180°C.
2. The preparation method according to claim 1, characterized in that: The composite adhesive comprises, by mass percentage, 80% to 90% of nitrile rubber and 10% to 20% of acrylate rubber.
3. The preparation method according to claim 2, characterized in that: The composite adhesive comprises, by mass percentage, 82% to 88% of nitrile rubber and 12% to 18% of acrylate rubber.
4. The preparation method according to claim 1, characterized in that: The primary mixing material includes the following components in percentage by mass: Magnetic powder 80%~95% Composite binder 4%~20% Additives 0.5%~3%.
5. The rubber magnetic material obtained according to the preparation method according to any one of claims 1 to 4.
6. Use of the rubber magnetic material according to claim 5 in manufacturing a motor.