A method and system for quickly calculating the moisture content distribution of wood fiber materials

The density distribution of ligno fiber materials is measured by an X-ray density meter and the moisture content distribution calculation equation is constructed, which solves the problem of moisture content distribution measurement error and real-time in the prior art, and realizes the rapid and accurate calculation of the moisture content distribution of ligno fiber materials. Suitable for monitoring the change of moisture content gradient during drying.

CN114993880BActive Publication Date: 2024-11-22SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210531088.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-16
Publication Date
2024-11-22
Estimated Expiration
2042-05-16

AI Technical Summary

Technical Problem

The existing methods for determining the moisture content distribution of wood fiber materials have large errors, cumbersomeness and cannot obtain continuous information in real time. Especially in the drying process, the deformation and error problems caused by changes in moisture content gradients have not been effectively solved.

Method used

X-ray density meter is used to measure the density distribution of wood fiber materials, combined with the density information before and after drying, the moisture content distribution calculation equation is constructed, the dry shrinkage rate in the direction of thickness, length and width is considered, and iterative discrete calculation and height constraints are used to reduce the Calculate complexity to achieve fast and accurate moisture content distribution calculation.

Benefits of technology

The rapid and accurate calculation of the moisture content distribution of wood fiber materials is achieved, the number of samples is taken out is reduced, deformation interference is avoided, calculation complexity is reduced, and measurement accuracy and real-timeness are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114993880B_ABST
    Figure CN114993880B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and system for quickly calculating the moisture content distribution of a wood fiber material. The method includes: preparing a first wood fiber material sample and a second wood fiber material sample and performing density measurement processing; drying the first wood fiber material sample to absolute dryness and combining the density information of the first wood fiber material sample before drying, calculating and discretely processing the moisture content distribution of the first wood fiber material sample, and constructing a moisture content distribution calculation equation; based on the moisture content distribution calculation equation, according to the density information of the second wood fiber material sample before and after drying, obtaining a moisture content distribution calculation result. By using the present invention, the moisture content distribution of a wood fiber material sample can be calculated more quickly and accurately. As a method and system for quickly calculating the moisture content distribution of a wood fiber material, the present invention can be widely used in the field of measuring the moisture content distribution of wood fiber materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of measuring and calculating the moisture content distribution of wood fiber materials, and in particular to a method and a system for quickly measuring and calculating the moisture content distribution of wood fiber materials. Background Art

[0002] Moisture content distribution is an important characteristic parameter of wood fiber materials. Almost all the physical and mechanical properties of wood fiber materials are related to moisture content and distribution. Moisture content distribution is also the main basis for the accurate implementation of wood fiber material drying process. If the moisture content gradient is too large during the drying process, it is easy to cause deformation and cracking of wood fiber materials, which will reduce the quality of wood fiber materials and cause economic losses. At present, the commonly used methods for determining moisture content distribution are mainly layered slicing method and electrical measurement method. The operation of layered slicing method is cumbersome and time-consuming. The evaporation of water during slicing will inevitably produce certain errors. At the same time, due to the limitation of slice thickness, the layered slicing method cannot obtain continuous moisture content distribution information of wood fiber materials. The measurement accuracy of the electrical measurement method is easily affected by factors such as the type of wood fiber material, texture direction, ambient temperature and humidity, and is generally only applicable to the range where the moisture content is below the fiber saturation point. The X-ray method is often used to measure the density of wood fiber materials. The basic principle is that the density of the material is calculated by measuring the attenuation change of the X-ray through the material, based on the relationship that the intensity attenuation rate of the X-ray through the material is proportional to the material density. The existing technical means include the X-ray method based on bulk density calculation to determine the moisture content distribution of wood fiber materials, but only considers the shrinkage of the wood fiber material in the thickness direction, ignoring the dimensional changes in the length and width directions, which will bring large errors to the calculation results. The X-ray scanning method for detecting the moisture content inside the wood fiber material during the drying process has a large moisture content gradient inside the wood fiber material during the actual drying process, and the shrinkage deformation of the wood fiber material is not uniform. Therefore, calculating the moisture content distribution of the wood fiber material according to the average thickness will produce certain errors. Therefore, the existing technical means and measurement methods have serious lags in obtaining moisture content distribution information. Therefore, it is necessary to seek a simple and effective method for detecting the moisture content distribution of wood fiber materials. Summary of the invention

[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a method and system for quickly measuring the moisture content distribution of wood fiber materials, which can more quickly and accurately measure the moisture content distribution of wood fiber material samples.

[0004] The first technical solution adopted by the present invention is: a method for quickly measuring the moisture content distribution of wood fiber materials, comprising the following steps:

[0005] preparing a first lignocellulosic material sample and a second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying;

[0006] The first wood fiber material sample is dried to absolute dryness and combined with the density information of the first wood fiber material sample before drying, the moisture content distribution of the first wood fiber material sample is calculated and discretized, and a moisture content distribution calculation equation is constructed;

[0007] Spin-coating the waterproof material and drying the second wood fiber material sample and measuring the density at preset time intervals to obtain density information of the second wood fiber material sample after drying;

[0008] Based on the moisture content distribution calculation equation, according to the density information of the second wood fiber material sample before drying and the density information of the second wood fiber material sample after drying, the moisture content distribution calculation result is obtained.

[0009] Furthermore, the step of preparing the first lignocellulosic material sample and the second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying specifically includes:

[0010] Selecting wood fiber materials;

[0011] preparing a wood fiber material sample on the wood fiber material and performing a division process on the thickness of the wood fiber material sample to obtain a first wood fiber material sample having a plurality of control units and a second wood fiber material sample;

[0012] Density measurement processing is performed on the first lignocellulosic material sample and the second lignocellulosic material sample respectively by an X-ray densitometer to obtain density information of the first lignocellulosic material sample before drying and density information of the second lignocellulosic material sample before drying.

[0013] Furthermore, the cross-sectional density calculation formula of the wood fiber material sample is expressed as follows:

[0014]

[0015]

[0016] In the above formula, J1 represents the number of density distribution values ​​measured by the X-ray method in the control unit of the wood fiber material sample before drying, J0 represents the number of density distribution values ​​measured by the X-ray method in the control unit of the wood fiber material sample after drying, P represents the density of the control unit of the wood fiber material sample before drying, ρ represents the density of the control unit of the wood fiber material sample after drying, P(X) represents the density distribution of the wood fiber material sample before drying, and ρ(X) represents the density distribution of the wood fiber material sample after drying.

[0017] Furthermore, the step of drying the first wood fiber material sample to absolute dryness and calculating and discretizing the moisture content distribution of the first wood fiber material sample in combination with the density information of the first wood fiber material sample before drying, and constructing a moisture content distribution calculation equation specifically includes:

[0018] Drying the first wood fiber material sample to obtain a completely dried first wood fiber material sample;

[0019] Performing density measurement on the completely dried first wood fiber material sample by an X-ray densitometer to obtain density information of the completely dried first wood fiber material sample;

[0020] Calculating the mass of the first lignocellulosic material sample according to the density information of the first lignocellulosic material sample and the length and width information of the first lignocellulosic material sample;

[0021] Calculating the first wood fiber material sample according to the shrinkage rate calculation formula of the wood fiber material and the density information of the first wood fiber material sample to obtain the shrinkage rate of the first wood fiber material sample;

[0022] Deducing the full-dry shrinkage rate of the first wood fiber material sample according to the shrinkage rate of the first wood fiber material sample and in combination with the characteristics of the wood fiber material, obtaining the full-dry shrinkage rate of the first wood fiber material sample;

[0023] The mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample are discretized to construct a moisture content distribution calculation equation.

[0024] Further, the shrinkage calculation formula is as follows:

[0025]

[0026]

[0027] In the above formula, β1 represents the shrinkage rate in the thickness direction of the first wood fiber material sample before drying, β2 represents the shrinkage rate in the thickness direction of the first wood fiber material sample after drying, and ΔZ green represents the thickness of the first wood fiber material sample in a saturated state, ΔZ represents the thickness of the first wood fiber material sample control unit before drying, Δz represents the thickness of the first wood fiber material sample control unit after drying, U represents the moisture content of the first wood fiber material sample before drying, and u represents the moisture content of the first wood fiber material sample after drying.

[0028] Furthermore, the step of performing discrete processing on the mass of the first lignocellulosic material sample, the shrinkage rate of the first lignocellulosic material sample and the fully dried shrinkage rate of the first lignocellulosic material sample to construct a moisture content distribution calculation equation specifically includes:

[0029] Performing discretization processing on the mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample to obtain a preliminary discrete calculation result;

[0030] Based on the iterative discrete calculation rule, it is determined that the preliminary discrete calculation result meets the preset threshold, the discrete calculation is stopped, and the discrete calculation result is output;

[0031] Based on the height constraint condition, the full-dry shrinkage rate of the first wood fiber material sample in the discrete calculation results is corrected and a moisture content distribution calculation equation is constructed.

[0032] Further, the moisture content distribution calculation equation is specifically as follows:

[0033]

[0034]

[0035] In the above formula, U i represents the moisture content of the first discrete wood fiber material sample before drying, u i represents the moisture content of the first wood fiber material sample after drying and discretization, M i represents the mass of the first discrete lignocellulosic material sample control unit before drying, m i represents the mass of the first lignocellulosic material sample control unit after drying and discretization, m 0,i represents the absolute dry mass of the first lignocellulosic material sample control unit after discretization.

[0036] Furthermore, the iterative discrete calculation rule is specifically as follows:

[0037]

[0038]

[0039] In the above formula, u′ i represents the moisture content value of the first wood fiber material sample calculated by the latest iteration, Δz′ i It represents the thickness of the first wood fiber material sample control unit calculated in the latest iteration.

[0040] Furthermore, the height constraint condition is specifically as follows:

[0041]

[0042]

[0043] In the above formula, β′ max represents the full-dry shrinkage of the first wood fiber material sample calculated by the latest iteration, β max represents the full-dry shrinkage of the first wood fiber material sample, ε represents the correction factor, z′ I+1 represents the thickness of the current first wood fiber material sample obtained by calculation, and h represents the actual thickness of the first wood fiber material sample obtained by measurement.

[0044] The second technical solution adopted by the present invention is: a rapid measurement system for moisture content distribution of wood fiber materials, comprising:

[0045] A measurement module, used for preparing a first lignocellulosic material sample and a second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying;

[0046] A construction module is used to dry the first wood fiber material sample to absolute dryness and calculate and discretize the moisture content distribution of the first wood fiber material sample based on the density information of the first wood fiber material sample before drying, so as to construct a moisture content distribution calculation equation;

[0047] A pre-processing module, used for spin-coating the second wood fiber material sample with a waterproof material and performing a drying process, and taking the sample out at preset time intervals to measure its density, so as to obtain density information of the dried second wood fiber material sample;

[0048] The calculation module obtains a moisture content distribution calculation result based on a moisture content distribution measurement equation and according to the density information of the second wood fiber material sample before drying and the density information of the second wood fiber material sample after drying.

[0049] The beneficial effects of the method and system of the present invention are as follows: during the drying process of wood fiber material samples, the present invention does not need to take out samples multiple times for drying and density measurement, but only needs to dry the samples to absolute dryness in the initial stage and dry multiple groups of adjacent samples and take out one of the groups at regular intervals, which is beneficial to regulating the drying process and avoiding deformation of the sample caused by taking out the same sample multiple times, which brings interference to the experimental results, and discretizes the constructed moisture content distribution calculation equation to reduce the complexity of the calculation, so that the moisture content distribution of the wood fiber material sample can be measured more quickly and accurately. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 It is a flowchart of the steps of a method for quickly calculating the moisture content distribution of wood fiber materials according to the present invention;

[0051] Figure 2 It is a structural block diagram of a rapid measurement system for moisture content distribution of wood fiber materials according to the present invention;

[0052] Figure 3 is a schematic diagram of a shrinkage model of a wood fiber material control unit of the present invention;

[0053] Figure 4 This is a moisture content distribution diagram of the Populus tomentosa wood drying process obtained by experimental simulation of the present invention;

[0054] Figure 5 This is a moisture content distribution diagram of the fir wood drying process obtained by experimental simulation of the present invention;

[0055] Figure 6 The present invention is a moisture content distribution diagram of the bamboo slice drying process obtained by experimental simulation. DETAILED DESCRIPTION

[0056] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The step numbers in the following embodiments are only provided for the convenience of explanation and description, and the order between the steps is not limited in any way. The execution order of each step in the embodiment can be adaptively adjusted according to the understanding of those skilled in the art.

[0057] Reference Figure 1 The present invention provides a method for quickly calculating the moisture content distribution of wood fiber materials, the method comprising the following steps:

[0058] S1, preparing a first lignocellulosic material sample and a second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying;

[0059] S11, selecting wood fiber material;

[0060] S12, preparing a wood fiber material sample on the wood fiber material and performing a division process on the thickness of the wood fiber material sample to obtain a first wood fiber material sample having a plurality of control units and a second wood fiber material sample;

[0061] Specifically, n groups of samples are prepared on the wood fiber material, each group of samples consists of two pieces of fiber-connected materials, marked as (A1, a1), (A2, a2), ..., (A n , a n ), the sample size is 20-50 mm (along the grain, length) × 20-50 mm (cross grain, width) × natural thickness is 3-100 mm (cross grain), and the number of groups ranges from 3 to 10.

[0062] S13, performing density measurement processing on the first lignocellulosic material sample and the second lignocellulosic material sample respectively by using an X-ray densitometer to obtain density information of the first lignocellulosic material sample before drying and density information of the second lignocellulosic material sample before drying;

[0063] Specifically, refer to Figure 3 , a one-dimensional coordinate system OZ is constructed in the thickness direction, assuming that the length, width and thickness of the wood fiber material before drying are L, W and H respectively, and the wood fiber material is divided into I control units along the thickness direction, and the thickness of the control unit is 0.5 mm to 5 mm, more precisely 1 mm to 2 mm, and further, the density of the first wood fiber material sample and the second wood fiber material sample is measured by an X-ray density meter, and the density calculation formula is specifically as follows:

[0064]

[0065]

[0066] In the above formula, J1 represents the number of density distribution values ​​measured by the X-ray method in the control unit of the wood fiber material sample before drying, J0 represents the number of density distribution values ​​measured by the X-ray method in the control unit of the wood fiber material sample after drying, P represents the density of the control unit of the wood fiber material sample before drying, ρ represents the density of the control unit of the wood fiber material sample after drying, P(X) represents the density distribution of the wood fiber material sample before drying, and ρ(X) represents the density distribution of the wood fiber material sample after drying.

[0067] S2, drying the first wood fiber material sample to absolute dryness and, based on the density information of the first wood fiber material sample before drying, calculating and discretizing the moisture content distribution of the first wood fiber material sample to construct a moisture content distribution calculation equation;

[0068] S21, drying the first wood fiber material sample to obtain a completely dried first wood fiber material sample;

[0069] Specifically, the first wood fiber material samples A1 to A n The first wood fiber material sample was placed in a constant temperature drying oven and the temperature was slowly increased from 40°C to 103°C at a rate of 10°C / h to dry the sample to absolute dryness. The absolute dryness condition is that the wood fiber material sample is dried in a constant temperature drying oven at 103°C to a constant weight, which is considered to be dried.

[0070] S22, measuring the density of the completely dried first wood fiber material sample by an X-ray densitometer to obtain density information of the completely dried first wood fiber material sample;

[0071] S23, calculating the mass of the first lignocellulosic material sample according to the density information of the first lignocellulosic material sample and the length and width information of the first lignocellulosic material sample;

[0072] Specifically, the mass of the control unit can be calculated based on the thickness of the control unit and the acquired length, width, and density. The mass calculation formula is as follows:

[0073] M=P·L·W·ΔZ

[0074] m=ρ·l·w·Δz

[0075] In the above formula, M represents the mass of the first lignocellulosic material sample control unit before drying, m represents the mass of the first lignocellulosic material sample control unit after drying, P represents the density of the first lignocellulosic material sample control unit before drying, ρ represents the density of the first lignocellulosic material sample control unit after drying, L represents the length of the first lignocellulosic material sample control unit before drying, l represents the length of the first lignocellulosic material sample control unit after drying, W represents the width of the first lignocellulosic material sample control unit before drying, w represents the width of the first lignocellulosic material sample control unit after drying, ΔZ represents the thickness of the first lignocellulosic material sample control unit before drying, and Δz represents the thickness of the first lignocellulosic material sample control unit after drying.

[0076] S24, calculating the first wood fiber material sample according to the shrinkage rate calculation formula of the wood fiber material and the density information of the first wood fiber material sample to obtain the shrinkage rate of the first wood fiber material sample;

[0077] Specifically, the shrinkage calculation formula is as follows:

[0078]

[0079]

[0080] In the above formula, β1 represents the shrinkage rate in the thickness direction of the first wood fiber material sample before drying, β2 represents the shrinkage rate in the thickness direction of the first wood fiber material sample after drying, and ΔZ green represents the thickness of the first lignocellulosic material sample in a saturated state, ΔZ represents the thickness of the control unit of the first lignocellulosic material sample before drying, Δz represents the thickness of the control unit of the first lignocellulosic material sample after drying, U represents the moisture content of the first lignocellulosic material sample before drying, and u represents the moisture content of the first lignocellulosic material sample after drying;

[0081] The wood fiber material does not shrink from the saturated state to the fiber saturation point, but the shrinkage from the fiber saturation point to the absolute dry state is linearly related to the moisture content. Assuming that the shrinkage rate of the wood fiber material is β max , the fiber saturation point is 30%.

[0082] S25, deriving the thickness of the control unit after the first lignocellulosic material sample is dried according to the shrinkage rate of the first lignocellulosic material sample and in combination with the characteristics of the lignocellulosic material;

[0083] Specifically, the calculation formula for controlling the thickness of the control unit after the first wood fiber material sample is dried is as follows:

[0084]

[0085] In the above formula, β max It indicates the full drying shrinkage rate;

[0086] Furthermore, the initial value of the full-dry shrinkage rate can be set to 0.01-0.2, and more precisely, can be set to 0.03-0.1.

[0087] S26. Discretely process the mass of the first lignocellulosic material sample, the density information of the first lignocellulosic material sample, and the full-dry shrinkage rate of the first lignocellulosic material sample to construct a moisture content distribution calculation equation.

[0088] Specifically, in order to develop an iterative algorithm for calculating the moisture content distribution of wood fiber materials, the density distribution measured by X-rays and the specific parameters of the first wood fiber material sample need to be discretized, thereby reducing the complexity of the calculation process, making the calculation process faster and the calculation results more accurate.

[0089] S261, performing discretization processing on the mass of the first wood fiber material sample, the density information of the first wood fiber material sample, and the full-dry shrinkage rate of the first wood fiber material sample to obtain a preliminary discrete calculation result;

[0090] S2611, firstly, performing discretization processing on the density distribution of the first wood fiber material sample;

[0091] Specifically, the discretization formula for the density of the first wood fiber material sample is as follows:

[0092]

[0093]

[0094] In the above formula, P i represents the density of the control unit of the wood fiber material sample before discrete processing and drying, ρ irepresents the density of the control unit of the wood fiber material sample after discrete processing and drying, F j+1 represents the upper boundary surface of the control unit of the first lignocellulosic material sample before drying, f j+1 represents the upper boundary surface of the control unit of the first lignocellulosic material sample after drying, F j represents the lower boundary surface of the control unit of the first lignocellulosic material sample before drying, f j represents the lower boundary surface of the first lignocellulosic material sample control unit after drying, P(X k ) represents the density distribution of the wood fiber material sample before discrete processing and drying, λ represents the scanning step of the X-ray;

[0095] If the boundary of the first lignocellulosic material sample control unit does not coincide with the X-ray density distribution position, the density distribution position closest to the lower boundary in the first lignocellulosic material sample control unit is taken, and the density of the first lignocellulosic material sample control unit before drying is calculated by taking the average density distribution in the unit, wherein the scanning step of the X-ray is 0.01mm~0.5mm, and more accurately can be 0.05mm~0.2mm.

[0096] S2612, performing discrete processing on the control unit after the first wood fiber material sample is dried;

[0097] Specifically, the formula for discrete processing performed by the control unit after the first wood fiber material sample is dried is as follows:

[0098]

[0099] In the above formula, ΔZ i represents the thickness of the first lignocellulosic material sample control unit before discrete drying, Δz i represents the thickness of the first lignocellulosic material sample control unit after discrete drying, U i represents the moisture content of the first lignocellulosic material sample before discrete drying, u i represents the moisture content of the first lignocellulosic material sample after discrete drying.

[0100] S2613, performing discrete processing on the mass calculation process of the first wood fiber material sample;

[0101] Specifically, the formula for performing discrete processing on the mass calculation process of the first lignocellulosic material sample is as follows:

[0102] M i =P i ·L·W·ΔZ i

[0103] m i =ρi ·l·w·Δz i

[0104] In the above formula, M i represents the mass of the first lignocellulosic material sample control unit before discrete drying, m i represents the mass of the first lignocellulosic material sample control unit after discrete drying, P i represents the density of the first lignocellulosic material sample control unit before discrete drying, ρ i represents the density of the first lignocellulosic material sample control unit after discrete drying, ΔZ i represents the thickness of the first lignocellulosic material sample control unit before discrete drying, Δz i represents the thickness of the first lignocellulosic material sample control unit after discrete drying.

[0105] S262, based on the iterative discrete calculation rule, determining that the preliminary discrete calculation result meets the preset threshold, stopping the discrete calculation, and outputting the discrete calculation result;

[0106] Specifically, assuming that the moisture content of the control unit after drying and the thickness of the control unit are calculated by the latest iteration u′ i and Δz′ i , set the convergence standard to the absolute value of the deviation between the two calculated values ​​less than 0.0001, and stop the iterative discretization of the parameters of the first wood fiber material sample, as shown below:

[0107]

[0108]

[0109] In the above formula, u′ i represents the moisture content value of the first wood fiber material sample calculated by the latest iteration, Δz′ i It represents the thickness of the first wood fiber material sample control unit calculated in the latest iteration.

[0110] S263. Based on the height constraint condition, the full-dry shrinkage rate of the first wood fiber material sample in the discrete calculation result is corrected and a moisture content distribution calculation equation is constructed.

[0111] Specifically, taking the actual thickness h of the first wood fiber material sample after drying as a constraint condition, the calculated thickness of the first wood fiber material sample is compared with the actual thickness, and the full drying shrinkage rate of the first wood fiber material sample is corrected. The correction process is as follows:

[0112]

[0113]

[0114] In the above formula, β′ max represents the full-dry shrinkage of the first wood fiber material sample calculated by the latest iteration, β max represents the full-dry shrinkage of the first wood fiber material sample, ε represents the correction factor, z′ I+1 represents the thickness of the current first wood fiber material sample obtained by calculation, and h represents the actual thickness of the first wood fiber material sample obtained by measurement;

[0115] The correction factor was introduced to correct the full-dry shrinkage rate, and the calculated sample thickness was completely consistent with the actual thickness, avoiding the calculation error caused by the large deviation between the introduced full-dry shrinkage rate and the actual full-dry shrinkage rate;

[0116] Further, the correction factor can be set to 0.001-0.1, and more precisely can be set to 0.005-0.05;

[0117] The moisture content distribution calculation equation is constructed based on the corrected full-dry shrinkage rate, as shown below:

[0118]

[0119]

[0120] In the above formula, U i represents the moisture content of the first discrete wood fiber material sample before drying, u i represents the moisture content of the first wood fiber material sample after drying and discretization, M i represents the mass of the first discrete lignocellulosic material sample control unit before drying, m i represents the mass of the first lignocellulosic material sample control unit after drying and discretization, m 0,i represents the absolute dry mass of the first lignocellulosic material sample control unit after discretization.

[0121] S3, spin-coating the second wood fiber material sample with a waterproof material, performing drying treatment, and measuring density at preset time intervals to obtain density information of the second wood fiber material sample after drying;

[0122] S4. Based on the moisture content distribution calculation equation, and according to the density information of the second wood fiber material sample before drying and the density information of the second wood fiber material sample after drying, a moisture content distribution calculation result is obtained.

[0123] Specifically, the moisture content distribution result calculated from the first wood fiber material sample is used as the initial moisture content distribution of the second wood fiber material sample, and the samples a1 to a1 are coated with a waterproof material. nOn the sides in the length and width directions, the waterproof material is spin-coated to simulate the actual drying process, so that moisture migrates only in one dimensional direction, namely the thickness direction. The waterproof material includes high-temperature paraffin, glass glue, epoxy resin and other substances, and is placed in a drying device for drying. A group of second wood fiber material samples are taken out from the drying device at regular intervals, and the cross-sectional density in the thickness direction is measured by an X-ray density meter. Combined with the density information of the second sample before drying measured in step S1, the moisture content distribution of the second wood fiber material sample is calculated by the constructed moisture content distribution measurement equation.

[0124] Reference Figure 2 , a rapid measurement system for moisture content distribution of wood fiber materials, comprising:

[0125] A measurement module, used for preparing a first lignocellulosic material sample and a second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying;

[0126] A construction module is used to dry the first wood fiber material sample to absolute dryness and calculate and discretize the moisture content distribution of the first wood fiber material sample based on the density information of the first wood fiber material sample before drying, so as to construct a moisture content distribution calculation equation;

[0127] A pre-processing module, used for spin-coating the second wood fiber material sample with a waterproof material and performing a drying process, and taking the sample out at preset time intervals to measure its density, so as to obtain density information of the dried second wood fiber material sample;

[0128] The calculation module obtains a moisture content distribution calculation result based on a moisture content distribution measurement equation and according to the density information of the second wood fiber material sample before drying and the density information of the second wood fiber material sample after drying.

[0129] The simulation experiment of the present invention is as follows:

[0130] Reference Figure 4, selected Populus tomentosa wood fiber material as the test material, with an initial moisture content of about 60%, and prepared 6 groups of wood fiber material samples of 50mm (length) × 50mm (width) × 25mm (thickness) at adjacent positions of the fibers. First, the cross-sectional density of A1~A6 was measured by an X-ray densitometer with a scanning step of 0.05mm, and then dried to absolute dryness, and the cross-sectional density was repeatedly measured; the cross-sectional density of samples a1~a6 was measured by an X-ray densitometer, and then placed in a drying device for drying, taken out at intervals, and then the cross-sectional density was measured. The moisture content distribution of Populus tomentosa wood fiber material in the drying process was calculated using the constructed moisture content distribution calculation equation, the cell thickness was 1mm, the calculation process was iterated 147 times, the initial value of the full-dry shrinkage rate was 0.15, the full-dry shrinkage rate correction factor was set to 0.005, and the full-dry shrinkage rate calculation result was 0.0652~0.0831;

[0131] Reference Figure 5 , selected fir wood fiber material as the test material, the initial moisture content is about 70%, prepared 7 groups of wood fiber material samples of 50mm (length) × 50mm (width) × 26mm (thickness) at the position adjacent to the fiber, first measured the cross-sectional density of A1~A7 by X-ray density meter, the scanning step length is 0.1mm, then dried to dry, and repeatedly measured its cross-sectional density; measured the cross-sectional density of samples a1~a7 by X-ray density meter, then put them into drying equipment to dry, took them out at intervals, and measured their cross-sectional density again, and calculated the moisture content distribution of fir wood fiber material in the drying process by using the constructed moisture content distribution calculation equation as follows Figure 2 As shown, the thickness of the control unit is 1mm, the calculation process is iterated 46 times, the initial value of the full-dry shrinkage rate is 0.1, the full-dry shrinkage rate correction factor is set to 0.008, and the full-dry shrinkage rate calculation result is 0.0613~0.0722;

[0132] Reference Figure 6 , selected bamboo chips as test materials, with an initial moisture content of about 50%, and prepared 6 groups of bamboo samples of 30mm (length) × 20mm (width) × 12mm (thickness) at positions adjacent to the fibers. First, the cross-sectional density of A1~A6 was measured by an X-ray density meter with a scanning step of 0.05mm, and then dried and repeatedly measured. The cross-sectional density of samples a1~a6 was measured by an X-ray density meter, and then placed in a drying device for drying, taken out at intervals, and then measured. The moisture content distribution of bamboo chips during the drying process was calculated using the constructed moisture content distribution calculation equation as shown in FIG. Figure 3 As shown, the thickness of the control unit is 0.5 mm, the calculation process is iterated 67 times, the initial value of the full-dry shrinkage rate is 0.1, the full-dry shrinkage rate correction factor is set to 0.01, and the calculation result of the full-dry shrinkage rate is 0.0427~0.0582.

[0133] The contents of the above method embodiments are all applicable to the present system embodiments. The functions specifically implemented by the present system embodiments are the same as those of the above method embodiments, and the beneficial effects achieved are also the same as those achieved by the above method embodiments.

[0134] The above is a specific description of the preferred implementation of the present invention, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.

Claims

1. A method for quickly calculating the moisture content distribution of wood fiber materials, characterized in that: The following steps are involved: preparing a first lignocellulosic material sample and a second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying; The first wood fiber material sample is dried to absolute dryness and combined with the density information of the first wood fiber material sample before drying, the moisture content distribution of the first wood fiber material sample is calculated and discretized, and a moisture content distribution calculation equation is constructed; Spin-coating the waterproof material and drying the second wood fiber material sample and measuring the density at preset time intervals to obtain density information of the second wood fiber material sample after drying; Based on the moisture content distribution calculation equation, according to the density information of the second wood fiber material sample before drying and the density information of the second wood fiber material sample after drying, a moisture content distribution calculation result is obtained; The step of drying the first wood fiber material sample to absolute dryness and calculating and discretizing the moisture content distribution of the first wood fiber material sample in combination with the density information of the first wood fiber material sample before drying, and constructing a moisture content distribution calculation equation specifically includes: Drying the first wood fiber material sample to obtain a completely dried first wood fiber material sample; Performing density measurement on the completely dried first wood fiber material sample by an X-ray densitometer to obtain density information of the completely dried first wood fiber material sample; Calculating the mass of the first lignocellulosic material sample according to the density information of the first lignocellulosic material sample and the length and width information of the first lignocellulosic material sample; Calculating the first wood fiber material sample according to the shrinkage rate calculation formula of the wood fiber material and the density information of the first wood fiber material sample to obtain the shrinkage rate of the first wood fiber material sample; Deducing the full-dry shrinkage rate of the first wood fiber material sample according to the shrinkage rate of the first wood fiber material sample and in combination with the characteristics of the wood fiber material, obtaining the full-dry shrinkage rate of the first wood fiber material sample; The mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample are discretized to construct a moisture content distribution calculation equation; The step of performing discrete processing on the mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample to construct a moisture content distribution calculation equation specifically includes: The mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample are discretized to obtain a preliminary discrete calculation result; Based on the iterative discrete calculation rule, it is determined that the preliminary discrete calculation result meets the preset threshold, the discrete calculation is stopped, and the discrete calculation result is output; Based on the height constraint condition, the full-dry shrinkage rate of the first wood fiber material sample in the discrete calculation result is corrected and a moisture content distribution calculation equation is constructed; The moisture content distribution calculation equation is specifically as follows: In the above formula, U i represents the moisture content of the first discrete wood fiber material sample before drying, u i represents the moisture content of the first wood fiber material sample after drying and discretization, M i represents the mass of the first discrete lignocellulosic material sample control unit before drying, m i represents the mass of the first lignocellulosic material sample control unit after drying and discretization, m 0,i represents the absolute dry mass of the first lignocellulosic material sample control unit after discretization.

2. A method for rapidly calculating the moisture content distribution of wood fiber materials according to claim 1, characterized in that: The step of preparing the first lignocellulosic material sample and the second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying specifically includes: Selecting wood fiber materials; Preparing a wood fiber material sample on the wood fiber material and performing a division process on the thickness of the wood fiber material sample to obtain a first wood fiber material sample having a plurality of control units and a second wood fiber material sample; Density measurement processing is performed on the first lignocellulosic material sample and the second lignocellulosic material sample respectively by an X-ray densitometer to obtain density information of the first lignocellulosic material sample before drying and density information of the second lignocellulosic material sample before drying.

3. A method for rapidly calculating the moisture content distribution of wood fiber materials according to claim 2, characterized in that: The cross-sectional density calculation formula of wood fiber material samples is as follows: In the above formula, J1 represents the number of density distribution values ​​measured by the X-ray method in the control unit of the wood fiber material sample before drying, J0 represents the number of density distribution values ​​measured by the X-ray method in the control unit of the wood fiber material sample after drying, P represents the density of the control unit of the wood fiber material sample before drying, ρ represents the density of the control unit of the wood fiber material sample after drying, P(X) represents the density distribution of the wood fiber material sample before drying, and ρ(X) represents the density distribution of the wood fiber material sample after drying.

4. A method for rapidly calculating the moisture content distribution of wood fiber materials according to claim 3, characterized in that: The shrinkage calculation formula is as follows: In the above formula, β1 represents the shrinkage rate in the thickness direction of the first wood fiber material sample before drying, β2 represents the shrinkage rate in the thickness direction of the first wood fiber material sample after drying, and ΔZ green represents the thickness of the first wood fiber material sample in a saturated state, ΔZ represents the thickness of the first wood fiber material sample control unit before drying, Δz represents the thickness of the first wood fiber material sample control unit after drying, U represents the moisture content of the first wood fiber material sample before drying, and u represents the moisture content of the first wood fiber material sample after drying.

5. A method for rapidly calculating the moisture content distribution of wood fiber materials according to claim 4, characterized in that: The iterative discrete calculation rules are specifically as follows: In the above formula, u' i Indicates the moisture content value of the first wood fiber material sample calculated by the latest iteration, Δz' i It represents the thickness of the first wood fiber material sample control unit calculated in the latest iteration.

6. A method for rapidly calculating the moisture content distribution of wood fiber materials according to claim 5, characterized in that: The height constraint conditions are as follows: In the above formula, β' max represents the full-dry shrinkage of the first wood fiber material sample calculated by the latest iteration, β max represents the full-dry shrinkage of the first wood fiber material sample, ε represents the correction factor, z' I+1 represents the thickness of the current first wood fiber material sample obtained by calculation, and h represents the actual thickness of the first wood fiber material sample obtained by measurement.

7. A rapid measurement system for moisture content distribution of wood fiber materials, characterized in that: Includes the following modules: A measurement module, used for preparing a first lignocellulosic material sample and a second lignocellulosic material sample and performing density measurement processing to obtain corresponding density information before drying; A construction module is used to dry the first wood fiber material sample to absolute dryness and calculate and discretize the moisture content distribution of the first wood fiber material sample based on the density information of the first wood fiber material sample before drying, so as to construct a moisture content distribution calculation equation; A pre-processing module, used for spin-coating the second wood fiber material sample with a waterproof material and performing a drying process, and taking the sample out at preset time intervals to measure its density, so as to obtain density information of the dried second wood fiber material sample; A calculation module, based on a moisture content distribution calculation equation, obtains a moisture content distribution calculation result according to the density information of the second wood fiber material sample before drying and the density information of the second wood fiber material sample after drying; The first wood fiber material sample is dried to absolute dryness and combined with the density information of the first wood fiber material sample before drying, the moisture content distribution of the first wood fiber material sample is calculated and discretized, and a moisture content distribution calculation equation is constructed, which specifically includes: drying the first wood fiber material sample to obtain a completely dried first wood fiber material sample; measuring the density of the completely dried first wood fiber material sample by an X-ray densitometer to obtain the density information of the completely dried first wood fiber material sample; calculating the mass of the first wood fiber material sample according to the density information of the first wood fiber material sample and the length and width information of the first wood fiber material sample; calculating the first wood fiber material sample according to the shrinkage rate calculation formula of the wood fiber material and the density information of the completely dried first wood fiber material sample to obtain the shrinkage rate of the first wood fiber material sample; deducing according to the shrinkage rate of the first wood fiber material sample and combined with the characteristics of the wood fiber material to obtain the completely dried shrinkage rate of the first wood fiber material sample; discretizing the mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the completely dried shrinkage rate of the first wood fiber material sample to construct a moisture content distribution calculation equation; The method of discretely processing the mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample to construct a moisture content distribution calculation equation specifically includes: discretely processing the mass of the first wood fiber material sample, the density information of the first wood fiber material sample and the full-dry shrinkage rate of the first wood fiber material sample to obtain a preliminary discrete calculation result; based on an iterative discrete calculation rule, judging that the preliminary discrete calculation result meets a preset threshold, stopping the discrete calculation, and outputting the discrete calculation result; based on a height constraint condition, correcting the full-dry shrinkage rate of the first wood fiber material sample in the discrete calculation result to construct a moisture content distribution calculation equation; The moisture content distribution calculation equation is specifically as follows: In the above formula, U i represents the moisture content of the first discrete wood fiber material sample before drying, u i represents the moisture content of the first wood fiber material sample after drying and discretization, M i represents the mass of the first discrete lignocellulosic material sample control unit before drying, m i represents the mass of the first lignocellulosic material sample control unit after drying and discretization, m 0,i represents the absolute dry mass of the first lignocellulosic material sample control unit after discretization.

Citation Information

Patent Citations

  • Method for oil deposit flow state digifax calculating with discrete fracture line processing

    CN103399970A

  • Moisture content measuring method for wood drying process and wood drying method

    CN108802352A

  • Method for detecting microscopic moisture content of wood

    CN109959577A

  • Method of wood strength and stiffness prediction

    US20050031158A1