Anti-skid yarn and method for preparing the same
By compounding polyester or nylon yarn with polyterephthalate and polyterephthalate and combining it with monocarboxyl-modified nanopowder, the problem of insufficient friction and discomfort in sports socks is solved. Yarns that achieve high friction coefficient and resilience are suitable for the production of complex textile structures.
Patent Information
- Application Number
- CN202210654786.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-10
AI Technical Summary
When improving friction, existing sports socks have problems such as insufficient friction, discomfort, and the inability to weave complex terry. Especially when exposed to water, the friction is greatly reduced, which affects the locking performance during exercise.
Polyester or nylon yarn is bonded with polyterephthalate and polyterephthalate composite fully stretched yarn through high-pressure air injection, combined with monocarboxylic modified polyterephthalate nanopowder Solution impregnation and dyeing treatment give the yarn high friction coefficient and resilience properties.
The anti-slip yarn produced has a high friction coefficient and good friction on both sides. The socks are soft to the touch and have resilience. It is suitable for weaving flat, terry and free terry structures, and the process parameters are simple and easy to operate.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to an anti-slip yarn and a preparation method of the anti-slip yarn. Background Art
[0002] At present, some sports socks need to use high-friction yarns on the soles of the socks. The conventional method is to apply silicone and use some yarns with increased twist coefficient to increase friction. While improving friction, its disadvantages are also very obvious. The glue application method can only apply glue on one side of the socks. Either the glue is applied on the outer layer of the socks, so the friction between the sole and the socks is not enough; or the glue is applied on the inner layer of the socks, so the friction between the socks and the soles is not enough. In addition, when silicone encounters water, especially sweat from exercise, the friction is greatly reduced, which affects the locking performance of the socks during exercise.
[0003] The use of high-twist yarns increases friction and makes the socks harder, which makes the soles of the feet feel very uncomfortable when wearing them for a long time. In addition, high-twist yarns have no free rebound performance and can only be woven into flat sheets, which are not suitable for weaving terry and semi-terry. They will make the terry uneven, with poor layering, and the finished product will be unstuck, with missed stitches, and sometimes even impossible to weave. Summary of the invention
[0004] The purpose of the present invention is to solve the above problems and provide an anti-skid yarn and a method for preparing the anti-skid yarn, so that the yarn has a high friction coefficient and resilience at the same time, and the socks made are soft and comfortable.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing an anti-slip yarn, characterized in that it comprises the following steps:
[0007] Step (1) prepares polyester or nylon yarn, polyterephthalate and polyterephthalate composite fully drawn yarn, and bonds the two yarns together by high pressure air spraying to form a composite yarn;
[0008] Step (2) preparing a monocarboxyl-modified poly(terephthalate) nanopowder solution, adding an additive to form a mixed solution, and stirring;
[0009] In step (3), the composite yarn is immersed in a tank containing the mixed solution and then pulled out, dried in a dryer, and then wound on a yarn bobbin of a rewinding machine.
[0010] Furthermore, in step (1), polyester yarn is selected; in step (2), the auxiliary agents are dispersants and chelating agents; the components in the solution are calculated by weight percentage: monocarboxyl-modified polyester terephthalate nanopowder accounts for 10%-20%, dispersant accounts for 2%-5%, chelating agent accounts for 1%-2%, and the rest is water at room temperature.
[0011] The anti-slip yarn preparation method also includes:
[0012] Step (4) is to process the yarn tubes in the dyeing plant, and the processing steps are as follows:
[0013] Step (41), putting the yarn into the dyeing vat, adding water at room temperature, adding sodium carbonate, adjusting the pH to 9-11, and then adding 3%-5% sodium sulfonate saturated fatty acid soap detergent, 1%-3% cationic quaternary ammonium salt degreasing agent, the bath ratio is 1:10-1:8;
[0014] Step (42), heating up to 90-100°C at a rate of 2°C / min, running for 30-40 minutes, and draining;
[0015] Step (43), after cleaning, add water, add 1-3g / L caustic soda, 0.5-1.5g / L thiourea dioxide, raise the temperature to 90-100°C at a rate of 1-2°C / min, keep warm for 30-50 minutes, and drain;
[0016] Step (44): Wash with clean water, add 1-3g / L citric acid, adjust the pH of the dye solution to between 4-6, drain the water, and remove the yarn from the tank;
[0017] In step (45), the yarn is dehydrated, dried, and wound again.
[0018] Furthermore, in step (3), the temperature of the drying machine is set to 185-200°C, the drying process is reciprocating drying, the winding speed of the rewinding machine is adjusted to 130-150m / min, and the produced yarn is wound on the yarn drum for dyeing for standby use.
[0019] Furthermore, in step (1), nylon yarn is selected; in step (2), the auxiliary agents are propylene glycol crosslinking agent, dispersant, and water-soluble vinyl thickener; the components in the solution are calculated by weight percentage: monocarboxyl modified polyester terephthalate nanopowder accounts for 10%-20%, propylene glycol crosslinking agent accounts for 1%-2%, dispersant accounts for 1%-2%, water-soluble vinyl thickener accounts for 1%-3%, and the rest is water at room temperature.
[0020] The anti-slip yarn preparation method also includes:
[0021] Step (4) is to process the yarn tubes in the dyeing plant, and the processing steps are as follows:
[0022] Step (41), putting the yarn into the dyeing vat, adding water at room temperature, adding sodium carbonate, adjusting the pH to 9-11, and then adding 3-5% sodium sulfonate saturated fatty acid soap detergent, 1-3% cationic quaternary ammonium salt degreasing agent, the bath ratio is 1:12-1:8;
[0023] Step (42), heating up to 90-100°C at a rate of 2°C / min, running for 30-40 minutes, and draining;
[0024] Step (43), after cleaning, add water, add 0.5-1.5g / L citric acid, adjust the pH to 5-6, heat up to 90-100℃ at a rate of 1-2℃ / min, run for 40-50 minutes, then cool down and drain;
[0025] Step (44): Wash with clean water, add 0.5-1.5g / L citric acid, adjust the pH of the dye solution to between 4-6, drain the water, and remove the yarn from the tank;
[0026] In step (45), the yarn is dehydrated, dried, and wound again.
[0027] Furthermore, in step (3), the temperature of the drying machine is set to 120-130°C, the drying process is reciprocating drying, the winding speed of the rewinding machine is adjusted to 80-110m / min, and the produced yarn is wound on the yarn drum for dyeing for standby use.
[0028] Furthermore, in the step (1), the fineness of the composite FDY of polyterephthalate and polyterephthalate is 20D.
[0029] Furthermore, in step (2), stirring is carried out at room temperature for 30-40 minutes.
[0030] The invention discloses an anti-skid yarn prepared by a method for preparing the anti-skid yarn.
[0031] Furthermore, the fiber crystal region of the composite yarn is embedded with monocarboxyl-modified polyethylene terephthalate nanoparticles.
[0032] The beneficial effects of the present invention are:
[0033] (1) The yarn produced has a high coefficient of friction, which makes the textile product have great friction on both sides;
[0034] (2) The manufactured socks have friction on both sides, locking the sole of the foot and the sock, as well as the sock and the sole of the shoe from moving relative to each other;
[0035] (3) The socks are soft to the touch, comfortable to wear, do not damage the skin, and have a certain resilience. They can be woven into flat, loop, semi-loop and free loop structures;
[0036] (4) The yarn preparation method has simple process parameters and the preparation process is easy to control and operate. DETAILED DESCRIPTION
[0037] The specific implementation methods of the anti-slip yarn and the method for preparing the anti-slip yarn of the present invention are described in detail below.
[0038] The anti-slip yarn of the present invention uses polyester or nylon fiber as a carrier, and the fiber surface is loaded with a high friction coefficient material that is resistant to washing and friction through micro-embedding and chemical reaction. Specifically, the yarn is processed through an air-changing yarn processing process, and a composite fully stretched monofilament of polyterephthalate and polyterephthalate is added.
[0039] After further high temperature treatment, the composite fully drawn yarn of polyterephthalate and polyterebutyrate has good elastic recovery performance when bent. After being made into socks, it has good elastic recovery performance when weaving positive terry, half terry and free jacquard terry.
[0040] Embodiment 1
[0041] Use polyester yarn carrier to carry out compounding. The specific steps are as follows:
[0042] S1: Prepare a polyester yarn for carrier, the fineness of which is 20D polyterephthalate and polyterephthalate composite FDY (fully drawn yarn), and bond the two yarns together by blowing with high-pressure air.
[0043] S2: Prepare monocarboxyl-modified polyethylene terephthalate nanopowder, a dispersant, a chelating agent, and room temperature water, mix them in a ratio of 15%:3%:1.5%:70.5%, and stir them at room temperature for 30 minutes for later use.
[0044] S3: Pour the prepared solution into the tank, pull out one end of the yarn, pass it through the solution tank, go through the dryer for multiple reciprocating cycles (increasing the drying time), wind it on the reeling machine, set the dryer temperature to 200 degrees, adjust the reeling machine speed to 150m / min, and wind the produced yarn on the dyeing yarn tube for use. After 1 minute at a high temperature of 200 degrees, the lattice cracks in the crystallization area of the polyester fiber open and are embedded with nanoparticles, thus giving the fiber a high friction coefficient.
[0045] S4: The yarn cones produced in S3 are treated in a cone yarn dyeing plant to remove impurities, monocarboxyl-modified polyethylene terephthalate remaining on the surface, and by-products generated by high temperature decomposition.
[0046] S4.1: Bath ratio 1:10, put the yarn into the dye vat, add water at room temperature, add sodium carbonate, adjust the pH to 9-11, then add 3% sodium sulfonate saturated fatty acid soap detergent and 1% cationic quaternary ammonium salt degreasing agent.
[0047] S4.2: Heat up to 100 degrees at a rate of 2 degrees / minute, operate for 30 minutes, and drain.
[0048] S4.3: After washing with clean water once, drain the water. Add 3g / L caustic soda and 1g / L thiourea dioxide into the water, heat up to 100 degrees at a rate of 2 degrees / minute, keep warm for 30 minutes, and drain the water.
[0049] S4.4: Wash with clean water, add 3g / L citric acid, adjust the pH of the dye solution to between 4-6, drain the water, and take the yarn out of the tank
[0050] S4.5: The yarn out of the cylinder is dehydrated, dried, and wound again.
[0051] The yarn made in Example 1 has good anti-slip properties and a high friction coefficient. It was tested by Zhejiang Light Industrial Product Quality Inspection Institute and National Textile and Garment Product Quality Inspection and Testing Center under the conditions of "pressure: 150cN, speed: 100mm / min, abrasive: cotton lining cloth", and the test results were "longitudinal static friction coefficient: 1.311, longitudinal dynamic friction coefficient: 0.765, transverse static friction coefficient: 1.425, transverse dynamic friction coefficient: 0.948".
[0052] By performing Martindale pilling on the yarn 5,000 times, better anti-slip performance can be achieved, with the results being: "Longitudinal static friction coefficient: 1.420, longitudinal dynamic friction coefficient: 0.910, transverse static friction coefficient: 1.350, transverse dynamic friction coefficient: 1.021."
[0053] Under the same testing conditions, the test results of pure cotton thread are "longitudinal static friction coefficient: 1.047, longitudinal dynamic friction coefficient: 0.745, transverse static friction coefficient: 0.976, transverse dynamic friction coefficient: 0.684", and the test results of pure nylon thread are: "longitudinal static friction coefficient: 0.678, longitudinal dynamic friction coefficient: 0.543, transverse static friction coefficient: 1.022, transverse dynamic friction coefficient: 0.710".
[0054] In addition, the socks made of the yarn of this patent also have good anti-slip performance. Under the same test conditions, the test results are "longitudinal static friction coefficient: 0.413, transverse static friction coefficient: 0.626, longitudinal dynamic friction coefficient: 0.339, transverse dynamic friction coefficient: 0.500".
[0055] It can be seen that the anti-skid yarn made by the present invention has good anti-skid performance, which is about 50% higher than that of ordinary pure cotton material and nylon material. The textile finished product also has good anti-skid performance.
[0056] Embodiment 2
[0057] Using nylon yarn carrier, compounding is carried out, and the specific steps are as follows:
[0058] S1: Prepare nylon yarn for carrier, the fineness is 20D polyterephthalate and polyterephthalate composite FDY, and bond the two yarns together by high-pressure air spray.
[0059] S2: Prepare monocarboxyl modified polyester terephthalate nano solution, propylene glycol crosslinker, dispersant, water-soluble vinyl thickener, and room temperature water: mix in the ratio of 13%:1%:1.5%:2%:72.5%, then adjust the pH to between 4-5 with citric acid, stir at room temperature for 30 minutes and set aside.
[0060] S3: Pour the prepared solution into the tank, pull out one end of the yarn, pass it through the solution tank, go through the dryer for multiple reciprocating cycles (increase the drying time), wind it on the reeling machine, set the dryer temperature to 130 degrees, adjust the reeling machine speed to 100m / min, and wind the produced yarn on the dyeing yarn tube for use. After 3 minutes at a high temperature of 160 degrees, the nylon amino group and the carboxyl group in the monocarboxyl-modified polyethylene terephthalate solution undergo an amidation reaction, thereby giving the fiber a high friction coefficient.
[0061] S4: The yarn cones produced in S3 are treated in a cone yarn dyeing plant to remove impurities, monocarboxyl-modified polyethylene terephthalate remaining on the surface, and by-products generated by high temperature decomposition.
[0062] S4.1: Bath ratio 1:10, put the yarn into the dye vat, add water at room temperature, add sodium carbonate, adjust the pH to 9-11, then add 3% sodium sulfonate saturated fatty acid soap detergent and 1% cationic quaternary ammonium salt degreasing agent.
[0063] S4.2: Heat up to 100 degrees at a rate of 2 degrees / minute, operate for 30 minutes, and drain.
[0064] S4.3: After washing once with clean water, drain the water. Add 1g / L citric acid to adjust the pH to 5-6, heat up to 100 degrees at a rate of 2 degrees / minute, and run for 40 minutes. Cool down and drain the water.
[0065] S4.4: Wash with clean water, add 1g / L citric acid, adjust the pH of the dye solution to between 4-6, drain the water, and take the yarn out of the tank.
[0066] S4.5: The yarn out of the cylinder is dehydrated, dried, and wound again.
[0067] Likewise, the yarn produced in the second embodiment also has similar anti-slip performance parameters as those in the first embodiment.
[0068] The present invention also claims to protect the anti-skid yarn directly prepared by the preparation method of the above embodiment. The fiber crystal region of the anti-skid yarn of the present invention is embedded with monocarboxyl-modified polyethylene terephthalate nanoparticles.
[0069] The above are only preferred embodiments of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principles of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing an anti-slip yarn, characterized in that: The steps include: Step (1) preparing polyester yarn, poly(terephthalate) and poly(terephthalate) composite fully drawn yarn, and bonding the two yarns together by high pressure air spraying to form a composite yarn; Step (2) preparing a monocarboxyl-modified polyethylene terephthalate nanopowder solution, adding an auxiliary agent to form a mixed solution, and stirring the solution. The auxiliary agent is a dispersant and a chelating agent. The components in the solution are calculated by weight percentage: the monocarboxyl-modified polyethylene terephthalate nanopowder accounts for 10%-20%, the dispersant accounts for 2%-5%, the chelating agent accounts for 1%-2%, and the rest is water at room temperature; In step (3), the composite yarn is immersed in a tank containing the mixed solution and then pulled out, dried in a dryer, and then wound on a yarn bobbin of a rewinding machine; Step (4) is to process the yarn tubes in the dyeing plant, and the processing steps are as follows: Step (41), putting the yarn into the dyeing vat, adding water at room temperature, adding sodium carbonate, adjusting the pH to 9-11, and then adding 3%-5% sodium sulfonate saturated fatty acid soap detergent, 1%-3% cationic quaternary ammonium salt degreasing agent, the bath ratio is 1:10-1:8; Step (42), heating up to 90-100°C at a rate of 2°C / min, running for 30-40 minutes, and draining; Step (43), after cleaning, add water, add 1-3g / L caustic soda, 0.5-1.5g / L thiourea dioxide, raise the temperature to 90-100°C at a rate of 1-2°C / min, keep warm for 30-50 minutes, and drain; Step (44): Wash with clean water, add 1-3g / L citric acid, adjust the pH of the dye solution to between 4-6, drain the water, and remove the yarn from the tank; In step (45), the yarn is dehydrated, dried, and wound again.
2. The method for preparing the anti-slip yarn according to claim 1, characterized in that: In the step (3), the temperature of the drying machine is set to 185-200°C, the drying process is reciprocating drying, the winding speed of the rewinding machine is adjusted to 130-150m / min, and the produced yarn is wound on the yarn drum for dyeing for standby use.
3. A method for preparing an anti-slip yarn, characterized in that: The steps include: Step (1) preparing nylon yarn, polyterephthalate and polyterephthalate composite fully drawn yarn, and bonding the two yarns together by high pressure air spraying to form a composite yarn; Step (2) prepares a monocarboxyl modified polyester terephthalate nanopowder solution, adds an auxiliary agent to form a mixed solution, and stirs the solution. The auxiliary agent is a propylene glycol crosslinking agent, a dispersant, and a water-soluble vinyl thickener. The components in the solution are calculated by weight percentage: the monocarboxyl modified polyester terephthalate nanopowder accounts for 10%-20%, the propylene glycol crosslinking agent accounts for 1%-2%, the dispersant accounts for 1%-2%, the water-soluble vinyl thickener accounts for 1%-3%, and the rest is water at room temperature; In step (3), the composite yarn is immersed in a tank containing the mixed solution and then pulled out, dried in a dryer, and then wound on a yarn bobbin of a rewinding machine; Step (4) is to process the yarn tubes in the dyeing plant, and the processing steps are as follows: Step (41), putting the yarn into the dyeing vat, adding water at room temperature, adding sodium carbonate, adjusting the pH to 9-11, and then adding 3-5% sodium sulfonate saturated fatty acid soap detergent, 1-3% cationic quaternary ammonium salt degreasing agent, the bath ratio is 1:12-1:8; Step (42), heating up to 90-100°C at a rate of 2°C / min, running for 30-40 minutes, and draining; Step (43), after cleaning, add water, add 0.5-1.5g / L citric acid, adjust the pH to 5-6, heat up to 90-100℃ at a rate of 1-2℃ / min, run for 40-50 minutes, then cool down and drain; Step (44): Wash with clean water, add 0.5-1.5g / L citric acid, adjust the pH of the dye solution to between 4-6, drain the water, and remove the yarn from the tank; In step (45), the yarn is dehydrated, dried, and wound again.
4. The method for preparing the anti-slip yarn according to claim 3, characterized in that: In the step (3), the temperature of the drying machine is set at 120-130°C, the drying process is reciprocating drying, the winding speed of the rewinding machine is adjusted to 80-110m / min, and the produced yarn is wound on the yarn drum for dyeing for standby use.
5. The method for preparing the anti-slip yarn according to any one of claims 1 to 4, characterized in that: In the step (1), the fineness of the composite FDY of polyterephthalate and polyterephthalate is 20D.
6. The method for preparing the anti-slip yarn according to any one of claims 1 to 4, characterized in that: In the step (2), stirring is carried out at room temperature for 30-40 minutes.
7. An anti-slip yarn prepared by the anti-slip yarn preparation method according to any one of claims 1 to 6, wherein the fiber crystal region of the composite yarn is embedded with monocarboxyl-modified polyethylene terephthalate nanoparticles.
Citation Information
Patent Citations
Production process of weft-elastic peach skin fabric
CN109763241A
Modified polyester fiber product and preparing method thereof
CN111647998A