Delayed fracture evaluation method for metallic materials

By using a chloride solution with a pH of 3.5 or above and an appropriate liquid film thickness in the stress-load part of the metal material, simulating the snow and precipitation environment at a specific temperature, the problem of difficulty in evaluating the delayed fracture characteristics of metal materials in the prior art is solved. , and the evaluation of high-precision delay fracture characteristics of automotive parts materials has been achieved.

CN115023600BActive Publication Date: 2024-11-26JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180012074.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-14
Filing Date
2021-02-09
Publication Date
2024-11-26
Estimated Expiration
2041-02-09

AI Technical Summary

Technical Problem

The prior art is difficult to evaluate the delayed fracture characteristics of the stress-loaded portion of the metal material with high precision in the corrosion environment in the wet state of snow, precipitation, and splashing water. Especially in the manufacturing of automobile parts, the existing methods have not been effectively considered. Corrosion conditions in various environments.

Method used

A solution containing chloride is supplied to the stress-loaded portion of the metal material by spraying, spraying, droplet addition or impregnation at a test temperature of -50 to 60°C, and the liquid film is maintained. In a state with a thickness of more than 10 μm and less than 2500 μm, corrosion continues to simulate the actual environment.

Benefits of technology

The evaluation of the high-precision delayed fracture characteristics of metal materials in corrosion environments in snow, precipitation, and splashing states is achieved, and the severity of delayed fracture in snow-melting salt environment is clarified, and a more accurate material use boundary is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115023600B_ABST
    Figure CN115023600B_ABST
Patent Text Reader

Abstract

A method for evaluating delayed fracture characteristics of a metal material is provided in which a solution containing a chloride having a pH of 3.5 or higher is placed on the stress loading portion of the metal material to maintain the state of deliquescent humidity of the chloride, thereby corroding the stress loading portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a delayed fracture evaluation method for evaluating the delayed fracture characteristics of a metal material used in a non-drying corrosive environment at a stress loading portion such as a bent portion of the metal material. Background Art

[0002] As the strength of automotive parts materials increases, the so-called "delayed fracture" phenomenon occurs, in which mechanical properties such as elongation deteriorate when hydrogen intrudes into the material. It is known that the occurrence of delayed fracture is caused by an increase in the amount of hydrogen intrusion into the material, and the delayed fracture sensitivity increases with the increase in the strength and load stress of the material. In particular, in the manufacture of automotive parts, steel plates as raw materials (plate materials) are usually used for bending or stretching using stamping machines and sheet metal machines, but at this time, delayed fracture is likely to become a problem in the stress load part that is subjected to stress.

[0003] Conventionally, delayed fracture evaluation methods have been performed by introducing hydrogen in acid immersion tests, cathode filling tests, corrosion tests, etc. Non-patent document 1 describes a technique for evaluating delayed fracture characteristics by introducing hydrogen into a material by immersing the material in a hydrochloric acid aqueous solution. Patent document 1 describes a technique for simply evaluating delayed fracture characteristics by introducing hydrogen into a stressed thin steel sheet in a cathode filling test.

[0004] Patent Document 2 describes a technique for evaluating delayed fracture characteristics of materials associated with corrosion by simulating the day and night wet and dry processes occurring in an atmospheric corrosion environment as a method for simply evaluating delayed fracture characteristics of metal materials used in an atmospheric corrosion environment. In addition, Patent Document 3 describes a laboratory corrosion resistance evaluation method for reducing the influence of surface irregularities by using a muddy aqueous material as an electrochemical corrosion resistance evaluation method using a water-containing material focusing on the shape of a test object as an automotive part.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2005-134152

[0008] Patent Document 2: Japanese Patent Application Publication No. 2016-180658

[0009] Patent Document 3: Japanese Patent Application Publication No. 2019-32173

[0010] Non-patent literature

[0011] Non-patent document 1: Iron and Steel, Vol. 79, No. 2, pp. 227-232 Summary of the invention

[0012] Problems to be solved by the invention

[0013] As mentioned above, delayed fracture often occurs during bending and bulging of metal materials, and it is necessary to evaluate the delayed fracture of the stress load part of the metal material after such processing. The evaluation methods described in Non-Patent Document 1, Patent Document 1, and Patent Document 3 can also test the stress load part at the same time. However, the tests in Non-Patent Document 1 and Patent Document 1 are not tests that take into account the corrosive environment of the wet state of snow, precipitation, and splashing water, so it is difficult to judge the delayed fracture characteristics in the actual environment.

[0014] The premise of Patent Document 2 is to conduct the test in an environment where wet and dry behavior occurs during the day and night, thereby directly evaluating the delayed fracture characteristics of the material. However, automobiles are used in a variety of environments, and Patent Document 2 does not envision the use in snowy areas or in environments where wading occurs. The purpose of Patent Document 3 is to use a water-containing material to penetrate the surface treatment film, and its concept is different from the liquid film thickness maintenance of the present invention.

[0015] The present invention has been made in view of the above situation, and an object of the present invention is to provide a delayed fracture evaluation method for metal materials that can accurately evaluate the delayed fracture characteristics of a stress-loaded portion of a metal material in a corrosive environment such as snow, precipitation, or splashing water.

[0016] Means for solving problems

[0017] The present invention has been made to achieve the above-mentioned object, and the gist of the present invention is as follows.

[0018] [1] A method for evaluating the delayed fracture characteristics of a metal material, which is a method for evaluating the delayed fracture characteristics of a stress-loaded portion of a metal material.

[0019] Here, a solution holding substance containing a solution having a pH of 3.5 or higher and containing chloride is arranged on the stress loading portion, and a state of holding the solution with deliquescent humidity of the chloride is continued to corrode the stress loading portion.

[0020] [2] The method for evaluating delayed fracture characteristics of a metal material according to [1], wherein corrosion is continued while maintaining a film thickness of the solution in a range of 10 μm to 2500 μm.

[0021] [3] The method for evaluating delayed fracture characteristics of a metal material according to [1] or [2], wherein the corrosion is carried out at a test temperature of -50 to 60°C.

[0022] [4] A method for evaluating delayed fracture characteristics of a metal material according to any one of [1] to [3], wherein after supplying a solution having a pH of 3.5 or more and containing chloride to the stress load portion, the solution retaining substance is arranged on the stress load portion.

[0023] [5] The method for evaluating delayed fracture characteristics of a metal material according to [4], wherein the solution is supplied by any one of spraying, showering, dripping, or immersion for less than 15 minutes.

[0024] [6] The method for evaluating delayed fracture characteristics of a metal material according to any one of [1] to [5], wherein the metal material is a steel plate having a tensile strength of 1180 MPa or more.

[0025] Effects of the Invention

[0026] According to the present invention, it is possible to evaluate with high accuracy the delayed fracture characteristics of a stress-loaded portion of a metal material in a corrosive environment in a wet state such as snow, precipitation, or splashing water. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram showing an example of a test piece used in the delayed fracture evaluation method.

[0028] Figure 2 This is a schematic diagram showing an example of a test piece used in the delayed fracture evaluation method. DETAILED DESCRIPTION

[0029] The following describes an embodiment of the present invention. The following description of the preferred embodiment is essentially illustrative and is not intended to limit its application or use. The inventors of the present application evaluated the delayed fracture characteristics of high-strength steel plates for automobiles under various actual environments. As a result, it was clarified that delayed fracture is prone to occur particularly in an environment where de-icing salt is dispersed. The reason is known to be that the surface of the steel plate is kept wet due to the adhesion of snow and mud stirred up by the running of the car, resulting in the most severe corrosion conditions.

[0030] It is known that when the surface of a metal material and a stress load part to which bending stress is applied are placed in the same corrosive environment, the stress load part remains wetted due to the adhesion of snow and mud even though it is curved, which is a severe delayed fracture environment. Therefore, it is confirmed that in addition to the evaluation of the delayed fracture characteristics of the surface of the metal material, it is necessary to conduct a test to evaluate the delayed fracture characteristics of the stress load part in a corrosive environment of a wet state in snow, precipitation, or splashing water.

[0031] Furthermore, it is known that not only the surface of the metal material but also the stress load portion is kept wet due to the adhesion of snow and mud. Based on this result, it is known that a uniform wet state must be maintained in the stress load portion during the evaluation test.

[0032] As described above, the delayed fracture evaluation method of the metal material of the present invention is performed as follows: a solution holding substance containing a solution having a pH of 3.5 or more and containing chloride is arranged on the stress load portion of the metal material, and the state of being maintained at the deliquescent humidity of the chloride is continued, thereby corroding the stress load portion. In the following embodiment, an example of the evaluation is performed by the following steps: (1) a supply step, which supplies a solution having chloride ions having a pH of 3.5 or more to the stress load portion of the metal material; and (2) a corrosion step, which maintains the state of a liquid film of the solution in an environment having a deliquescent humidity of the chloride at a test temperature of -50 to 60°C or more, thereby corroding the metal material.

[0033] First, in order to specifically evaluate the delayed fracture characteristics, it is necessary to make the metal material have a stress load portion. As a processing method for the metal material, bending, bulging, stretching, etc. can be cited. In addition, as a method of applying stress to the metal material, for example, a method of fixing it in a shape to which stress is applied using bolts, a method of evaluating using residual stress existing after processing, etc. can be cited. It should be noted that although the case where bending stress is applied as the stress load portion is illustrated, axial load stress, torsional stress, etc. based on tensile load or compression load other than this can also be applied.

[0034] In particular, the metal material to be evaluated is a steel material such as a steel plate having a tensile strength TS of 1180 MPa or more, but is not limited thereto and may be other metal materials such as Ti, Al, etc. In addition, metal materials subjected to plating are also included.

[0035] (1) Supply process

[0036] The supply process is a process of supplying a solution containing chloride with a pH of 3.5 or more to the stress load portion of the metal material. If the pH of the solution is lower than 3.5, the dissolution of the metal material is promoted, so that the hydrogen ions in the solution accompanying the dissolution of the metal material are reduced, thereby promoting the intrusion of hydrogen into the metal material. In other words, if the pH of the solution is lower than 3.5, the test becomes an environment more harsh than the actual environment, and the delayed fracture characteristics test in the actual environment cannot be performed with high precision. Therefore, a solution with a pH of 3.5 or more is used. It should be noted that since the solution is neutral in the corrosive environment of the actual environment, the pH of the solution is preferably 5 to 9.

[0037] As a corrosive environment in an actual environment, chloride is a common factor, so chloride is contained in the solution. It should be noted that, when the stress load portion of the metal material is only covered with snow, the snow does not contain chloride, but it is considered that even if the stress load portion of the metal material is covered with snow, it will be affected by snow-melting salt. Therefore, the solution contains chloride. At this time, chloride is contained in the solution in the form of chloride ions.

[0038] Chloride ions refer to Cl ions in salts containing Cl ions, such as NaCl, MgCl2, and CaCl2, and the solution contains one or more components of the above chlorides. The solvent may contain only chlorides such as NaCl, MgCl2, and CaCl2 in water, or may contain multiple chlorides, or may contain components other than chlorides. As components other than chlorides, sulfides, nitric acid compounds, urea mixed and dispersed in snow melting agents, etc. contained in the environment can be cited, but are not limited to these. Considering the actual environment, it is preferred that the solution attached to the metal material is mainly NaCl, such as salt water.

[0039] A solution is a mixture in a liquid state composed of two or more substances, and an aqueous solution can be used, for example, with a liquid component containing water as a solvent and the above-mentioned chloride as a solute. In particular, with respect to the solution used in the delayed fracture test, the chloride accounts for 50 to 100% by weight of the solute, preferably more than 70%. In this way, by increasing the weight ratio of the chloride, the management of the deliquescent humidity described later can be simplified. In addition, with respect to the weight % of the solute and the solvent, the concentration is arbitrary as long as there is no obstacle in the operation. For example, when NaCl accounts for more than half of the volume of the solution, NaCl produces precipitation due to being higher than the saturation amount. In such a case, it is not suitable for the present invention because the solution cannot be supplied evenly.

[0040] The method of supplying the solution to the stress load portion of the metal material is not particularly limited. As specific examples, there can be cited a method of immersing the test piece in the solution and then taking it out to adhere the solution to the surface of the test piece (less than 15 minutes, preferably less than 10 minutes), a method of applying the solution to the metal material by spraying or showering, a method of adhering the solution by spraying, a method of adding a prescribed amount of solution droplets using a pipette, etc. If the solution adhesion based on immersion exceeds 15 minutes, corrosion proceeds in the solution, which is different from the corrosion method of the present invention and is not suitable. It should be noted that spraying means spraying a solution with droplets of 50μm or more, and spraying means spraying a solution with droplets less than 50μm.

[0041] In addition, the solution supply in the supply process can also be performed by placing a solution retaining material such as a gauze containing the solution used in the corrosion process on the stress load part. In this case, the corrosion process described later is performed using the solution retaining material configured in the supply process. In this way, the actual corrosion environment that remains unchanged from the supply process to the corrosion process can be reproduced, and the accuracy of the test can be improved.

[0042] (2) Etching process

[0043] The etching step is a step of placing a solution-retaining substance containing a solution on the stress loading portion of the metal material and maintaining the state of being retained in a deliquescent humidity of the chloride to thereby corrode the stress loading portion of the metal material.

[0044] In the corrosion process, the solution must be continuously maintained on the stress load part of the metal material. Since the thickness of the liquid film has a great influence on the delayed fracture characteristics, it is an important factor. The delayed fracture characteristics when the thickness of the liquid film is actually changed and the delayed fracture characteristics when each liquid film thickness is evaluated, it can be seen that as long as at least the liquid film exists in the stress load part (greater than 0μm), the delayed fracture characteristics can be evaluated. It should be noted that the thickness of the liquid film is obtained by converting the value obtained from the ACM sensor (made by Syrinx Co., Ltd.) into the liquid film. In particular, it is preferred that the liquid film thickness is maintained at a state of 10μm to 2500μm. When the liquid film thickness is less than 10μm, the liquid film is not fully formed, and no corrosion occurs compared to the actual environment test. Therefore, there is a situation where the limit load stress is consistent with the actual environment, but the corrosion mode (corrosion type) is different from the actual environment. Similarly, even if the liquid film thickness exceeds 2500μm, the limit load stress is consistent with the actual environment due to the excessive thickness of the liquid film, but the corrosion mode (corrosion type) is different from the actual environment. Therefore, the thickness of the liquid film is preferably 10 μm to 2500 μm. It should be noted that the thickness of the liquid film in the etching step is mainly based on the supply amount of the solution in the supply step and the management of the chloride amount described later.

[0045] The test temperature in the corrosion process is not particularly limited, and is carried out in an environment with a test temperature of -50 to 60°C, for example. The test temperature is determined based on measurements in an actual environment. In an environment where deicing salt is spread, an environment reaching -50°C has been confirmed. In addition, when a car is parked in direct sunlight, the body parts become as high as 60°C, so the temperature range of the present invention is set to -50 to 60°C. As a range that can be implemented by a general-purpose device, the preferred test temperature is -20 to 40°C.

[0046] In the corrosion process, the relative humidity of the test environment is one of the important factors. According to multiple experiments, in the corrosion process, the solution on the stress load part must be kept in a non-dry state. The non-drying wet state means that a liquid film is formed uninterruptedly on the stress load part of the metal material (preferably the thickness of the liquid film is 10μm or more). If the liquid film is interrupted, the amount of chloride in the test object part will be uneven, which is not preferred due to the large difference from the actual environment. In addition, in order for the liquid film to form a liquid film uninterruptedly, the wetting condition must be continuous and the shaking must be small.

[0047] Therefore, the etching process is carried out in an environment above the deliquescent humidity of the chloride. The deliquescent humidity is the humidity that produces wetting on the surface of the test piece due to moisture absorption (deliquesce) of the chloride. As a result, the solution of the stress load unit mentioned above can be maintained in a non-dry state. The deliquescent humidity is determined by the type of chloride supplied to the stress load unit, that is, the chloride in the solution. For example, in the case of using a salt mainly composed of NaCl, the relative humidity is above 75% RH, in the case of using a salt mainly composed of MgCl2, the relative humidity is above 33% RH, and in the case of using a salt mainly composed of KCl, the relative humidity is above 84% RH, and it is uniformly managed in a manner without humidity changes. It should be noted that the change in the thickness of the liquid film in the etching process can be allowed to be ±10% of the set value. If this value is exceeded, the results will be uneven and inappropriate.

[0048] As mentioned above, the amount of chloride in the solution and the relative humidity of the test environment are the amounts that can maintain the liquid film thickness without interruption. That is, the liquid film thickness is determined by the relative humidity of the test environment and the amount of chloride. Too much or too little chloride is difficult to reproduce the actual environment. As the amount of chloride to ensure the above-mentioned liquid film thickness, 1000 to 200000 mg / m 2 .

[0049] For example, in an environment with a temperature of 25°C and a humidity of 95% RH, the amount of chloride is 0.1 g / m 2 When the film thickness is about 10μm, the chloride content is 1g / m 2 The thickness of the liquid film is about 100 μm. It should be noted that, from the perspective of the amount of chloride supplied and the management of relative humidity, the thickness of the liquid film in the etching process is preferably 40 to 1500 μm in consideration of the thickness of the liquid film. In addition, it is more preferred that the relative humidity of the test environment is above 90% RH, so that even if the relative humidity of the test environment changes by ±5% RH, it will not affect the experimental results.

[0050] Furthermore, in the corrosion process, a solution retaining substance containing a solution is arranged on the stress load portion of the metal material in such a manner that the state of the solution supplied in the supply process can be maintained. Thus, a state in which wetting is continued in the stress load portion of the metal material can be reliably maintained. The solution retaining substance can be any substance such as cotton gauze, mud, etc., which has gaps in the substance and can maintain the state of the solution by capillary phenomenon. Preferably, the solution retaining substance is a substance that allows oxygen to pass through without hindering corrosion. It should be noted that in order to maintain a constant wetting state of the stress load portion of the metal material, it is preferred that the solution retaining substance is inactive during the test. In addition, the supply process may be implemented only once initially, or the supply process and the corrosion process may be repeated. In the case of repeatedly performing the supply process and the corrosion process, it is preferred that the corrosion process be performed for more than 100 hours.

[0051] Example 1

[0052] First, whether the delayed fracture test method of the present invention simulates actual corrosion was verified by the following Example 1. First, as metal materials forming test pieces, steel types A, B, C, and D having the components shown in Table 1 were used.

[0053] [Table 1]

[0054]

[0055] Figure 1 Schematic diagram showing an example of a test piece for delayed fracture evaluation. Figure 1 As shown, a steel plate with a thickness of 1.4 mm formed by steel types A, B, C, and D is cut into a width of 35 mm × a length of 100 mm. In order to remove the residual stress during shearing, the two ends are ground to a width of 30 mm, and a test piece 1 is made in which a hole for bolts is opened away from the evaluation part.

[0056] The steel plate for the test was immersed in toluene for 5 minutes, and after ultrasonic cleaning, it was bent 180°. The test piece 1 after rebound was constrained with bolts BN and nuts NN to make test piece 1. The test piece 1 for delayed fracture evaluation has a stress load part 2 formed by a bending part with a bending radius R=7mm. An arbitrary stress is supplied to the stress load part 2 by adjusting the tightening amplitude of the bolts BN and the nuts NN. Under the condition of more tightening, the load stress becomes larger, which is a harsh condition. The stress of the stress load part 2 generated by tightening is recorded as the tightening stress. In this embodiment, it is set to five levels of 800, 1000, 1200, 1400, and 1600 MPa. The tightening stress is determined by estimating the tightening amplitude based on the CAE analysis based on the SS curve of each material.

[0057] The test pieces 1 using steel types A and B were subjected to both actual environmental tests in actual deicing salt spreading areas and tests based on the delayed fracture evaluation method of metal materials of the present invention. On the other hand, the test pieces 1 using steel types C and D were subjected to tests based on the delayed fracture evaluation method of metal materials described later.

[0058] <Actual environment test>

[0059] In the actual environment test, each test piece 1 was set at the bottom of the moving body that was traveling on a road with deicing salt sprinkled on it every day, and was collected on the 60th day after the start of the test. The reason why it was set at the bottom of the moving body is that the bottom of the moving body is affected by the deicing salt. The results are shown in the following Table 2. It should be noted that the minimum load stress at which cracking occurred during the test period was set as the boundary of cracking, which was used as the limit load stress in the actual environment.

[0060] [Table 2]

[0061]

[0062] In Table 2, the condition of the test piece in which a crack of 1 mm or more appeared on the test piece 1 was defined as cracked (symbol: ×), and the condition of crack less than 1 mm or no crack was defined as no crack (symbol: 0). In addition, when the stress with the smallest load stress in the test piece 1 in which cracking occurred was defined as the limit load stress, the limit load stress of steel A was 1400 MPa, and the limit load stress of steel B was 1200 MPa.

[0063] <Delayed fracture characteristics test>

[0064] Next, if Figure 2 As shown, the delayed fracture evaluation method of the above-mentioned metal material is implemented by using the same test piece 1 as the above-mentioned actual environmental test, and arranging the solution retaining component 10 on the stress load part 2 during the corrosion process. At this time, the test period is set to a maximum of 60 days, and the minimum load stress at which cracking occurs during the test period is set as the boundary of cracking, which is used as the limit load stress. In addition, by comparing the limit load stress and corrosion mode (corrosion type) obtained in the delayed fracture characteristic test with the limit load stress and corrosion mode (corrosion type) obtained in the above-mentioned actual environmental test, it is determined whether the delayed fracture characteristic test is appropriate. It should be noted that the relative humidity in the atmospheric atmosphere is within the range of ±5% of the set value as the test range.

[0065] Table 3 shows the test conditions and results of the delayed fracture evaluation test.

[0066] [Table 3]

[0067]

[0068] It should be noted that in Table 3, the case based on the test conditions of one embodiment of the present invention is taken as an example, the case that does not meet the test conditions is taken as a comparative example, and the part outside the numerical range of the present application is underlined. In addition, for the condition that no test piece cracks, the limit load stress is recorded as 1600MPa or more. The conditions that are inconsistent with the actual environmental test are set as × (comparative example), the conditions that are consistent with the results are set as "B", and the more preferred results are set as "A". Specifically, as described above, from the perspective of the limit load stress and the corrosion mode (corrosion type), the evaluation of the compatibility with the actual environment is performed. And, when the limit load stress and the corrosion mode (corrosion type) are consistent with the actual environment, it is set as "A". In addition, when the limit load stress is consistent but the corrosion mode is different, it is set as "B" because it is established as a delayed fracture evaluation test. On the other hand, when the limit load stress and the corrosion mode (corrosion type) are inconsistent with the actual environment, it is set as "×" as not suitable for the delayed fracture evaluation test.

[0069] No.3, 5, 13, 23, and 26 are examples of using steel type A, and changing the liquid film thickness by fixing conditions other than the chloride amount and changing the chloride amount. In the environment of No.3, since the amount of chloride supplied is small, the liquid film is not fully formed, and the corrosion is less than that in the actual environment test. Therefore, the cracking result (limit load stress) is consistent with the actual environment but slow. In addition, in No.26, the chloride amount is large and the liquid film thickness is too thick, so the limit load stress is consistent with the actual environment, but the corrosion mode is different from that in the actual environment. No.30, 32, 40, 50, and 53 are examples of using steel type B, showing the same tendency.

[0070] No. 1, 2, 4, 13, 28-29, 31, 40 are examples and comparative examples of using steel types A and B and changing the amount of chloride and the relative humidity of the test environment to change the film thickness. The film thickness formed is determined by the relationship between the relative humidity of the test environment and the amount of chloride. In No. 4 and 31, the humidity is 75% RH, the chloride amount is 10000 mg / m 2 , so it is possible to maintain a state where the liquid film exists uninterruptedly (the liquid film thickness is 10 μm or more). In No. 1 and 28 as comparative examples, the relative humidity of the test environment is low and the relative humidity is lower than the relative humidity at which the chloride contained in the solution absorbs moisture, so the liquid film is basically not formed and corrosion does not proceed, so the environment is different from the actual environment. In addition, in the examples No. 13 and 40 where the relative humidity of the test environment is 90% or more, the water film thickness is within the appropriate range and the corrosion condition is also similar to the actual environment, so a more preferable result is obtained.

[0071] No. 13, 22, 27, 40, 49, 54 are examples and comparative examples in which the types of solutions are changed. No. 13, 22, 40, 49 in the examples are solutions containing chloride, so the results are consistent with the actual environment. Comparative examples No. 27 and 54 are solutions that do not contain chloride ions. Since they do not contain chloride ions, uniform liquid films are not formed and the results are inconsistent with the actual environment.

[0072] No.8-10, 13, 19-21, 35-37, 40, 46-48 are examples in which the test temperature is changed. No.9, 10, 13, 19, 20, 36, 37, 40, 46, and 47 in the examples show a high degree of consistency with the actual environment. On the other hand, in No.8 and 35, the solution freezes due to the excessively low temperature, and corrosion no longer proceeds from the middle. Therefore, although the cracking results (limit load stress) are consistent with the actual environment, the corrosion mode is inconsistent. Like No.21 and 48, if the temperature is too high, corrosion proceeds above the actual environment. Therefore, although the cracking results (limit load stress) are consistent with the actual environment, the corrosion mode is inconsistent.

[0073] No. 11 to 13, 18, 38 to 40, 45 are examples and comparative examples when the pH of the solution is changed. Examples No. 12 to 13, 18, 39 to 40, 45 are highly consistent with the actual environment. In Comparative Examples No. 11 and 38, the results are harsher than the actual environment. This is because the low pH of the solution promotes the dissolution of iron, and the hydrogen ions in the solution are reduced with the dissolution of iron, which promotes the intrusion of hydrogen into the steel. Therefore, it is expected to be harsher than the actual environment and inconsistent with the actual environment.

[0074] No. 5, 7, 13, 16-17, 23, 25, 32, 34, 40, 43-44, 50, 52 are examples and comparative examples in which the solution-retaining substance is changed. No. 5, 7, 13, 16, 23, 25, 32, 34, 40, 43, 50, 52 are cases in which the solution-retaining substance is changed. In these examples, the thickness of the liquid film is maintained by configuring a substance that retains the solution, thereby being consistent with the results of the actual environment. Since the solution cannot be retained if a substance with water-retaining ability is not configured like No. 17 and 44, the progress of corrosion is different and inconsistent with the actual environment.

[0075] No. 5 to 6, 13 to 15, 23 to 24, 32 to 33, 40 to 42, 50 to 51 are examples in which the supply method of the solution is changed. No. 5 to 6, 13 to 15, 23 to 24, 32 to 33, 40 to 42, 50 to 51 are examples that are consistent with the actual environment while satisfying the condition of the liquid film thickness even if the supply method is changed.

[0076] Example 2

[0077] In the hydrochloric acid immersion, which is a conventional delayed fracture evaluation method, only materials under the same conditions can be compared. It was verified whether the use limit of the material itself can be determined by performing this evaluation. Specifically, the delayed fracture characteristics of steel C and steel D were evaluated based on the limit load stress. The results are shown in Table 4.

[0078] [Table 4]

[0079]

[0080] As shown in Table 4, for steel C, only the test piece with the largest load stress of 1600 MPa cracked. According to this embodiment, it can be seen that the limit load stress of steel C is large, so the delayed fracture characteristics are excellent. On the other hand, the limit load stress of steel D is 1000 MPa, and cracking occurs at a stress lower than YS. Therefore, the limit load stress of steel D is smaller than that of this test, so it can be judged that the delayed fracture characteristics are low. In this way, by using the technology of the present invention, it is also possible to evaluate the use limit of the material itself.

[0081] The embodiment of the present invention is not limited to the above embodiment, and various modifications can be implemented. For example, the metal material to be evaluated is usually a steel material such as a steel plate, but is not limited thereto, and may also be a metal material such as Ti, Al, etc. The delayed fracture characteristic evaluation method of the present invention can accurately evaluate the delayed fracture characteristics of a metal material, thereby evaluating that the selected metal material (particularly a steel material such as a steel plate) has excellent delayed fracture characteristics.

[0082] Description of Reference Numerals

[0083] 1 Test piece

[0084] 2 Stress load part

[0085] BN Bolts

[0086] NN Nut

[0087] 10 Solution retention material

Claims

1. A method for evaluating delayed fracture characteristics of a metal material, the method comprising evaluating delayed fracture characteristics of a stress-loaded portion of a metal material, in, In the stress load portion, a solution retaining material containing a solution with a pH of 3.5 or higher and containing chloride is arranged on the stress load portion, and the liquid film thickness of the solution is maintained at 10 μm or more and 2500 μm or less, so that the state of being maintained at the deliquescent humidity of the chloride is continued, thereby corroding the stress load portion.

2. The method for evaluating delayed fracture characteristics of a metal material according to claim 1, wherein: The corrosion was carried out at a test temperature of -50 to 60°C.

3. The method for evaluating delayed fracture characteristics of a metal material according to claim 1, wherein: After supplying a solution having a pH of 3.5 or more and containing chloride to the stress loading portion, the solution retaining substance is disposed on the stress loading portion.

4. The method for evaluating delayed fracture characteristics of a metal material according to claim 2, wherein: After supplying a solution having a pH of 3.5 or more and containing chloride to the stress loading portion, the solution retaining substance is disposed on the stress loading portion.

5. The method for evaluating delayed fracture characteristics of a metal material according to claim 3, wherein: The solution is supplied by any of spraying, showering, dripping, or immersion for less than 15 minutes.

6. The method for evaluating delayed fracture characteristics of a metal material according to claim 4, wherein: The solution is supplied by any of spraying, showering, dripping, or immersion for less than 15 minutes.

7. The method for evaluating delayed fracture characteristics of a metal material according to any one of claims 1 to 6, wherein: The metal material is a steel plate having a tensile strength of 1180 MPa or more.