Silicon-carbon-metal composite negative electrode material and preparation method thereof

The silicon-carbon-metal composite material modified by the metal organic framework solves the problems of volume changes in silicon-based batteries and unstable electrode interfaces, improves electrochemical activity and conductivity, and realizes the high energy density of the negative electrode materials of lithium-ion batteries and Long cycle stability.

CN115064687BActive Publication Date: 2024-11-01TN CORE ENERGY TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210918396.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-01
Publication Date
2024-11-01
Estimated Expiration
2042-08-01

AI Technical Summary

Technical Problem

The volume change of the negative electrode material of silicon-based lithium-ion battery during charging and discharging leads to performance attenuation, the electrode interface is unstable, and the conductivity is low, which limits its application prospects.

Method used

Silicon-carbon-metal composite material modified with metal organic framework is prepared by mixing metal salt, organic carbon source, silicon source and elemental carbon source, and stirring, reaction, drying and high-temperature carbonization to form a porous carbon framework structure and uniformly dispersed. Silicon and silicon oxide improve electrochemical activity and electrical conductivity.

Benefits of technology

The electrochemical activity of silicon and silicon oxides is improved, and the rapid ion diffusion channel is provided, long cycle stability and high conductivity are ensured, and the energy density and cycling performance of the negative electrode material of lithium-ion battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115064687B_ABST
    Figure CN115064687B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon-carbon-metal composite negative electrode material and a preparation method thereof. The method comprises the following steps: mixing a metal salt, an organic carbon source, a silicon source, an elemental carbon source and a solvent, and stirring them thoroughly until they are completely dissolved to obtain a first precursor; reacting the first precursor at a certain temperature for a period of time, drying, and obtaining a second precursor; carbonizing the second precursor at a high temperature to obtain a silicon-carbon-metal composite negative electrode material. The material includes a composite negative electrode material prepared by the method for preparing a silicon-carbon-metal composite negative electrode material. The beneficial effects of the present invention include: avoiding the problem of agglomeration of silicon and silicon oxides, improving the catalytic activity of the electrode reaction of silicon and silicon oxides, and ensuring the long-cycle stability of silicon and silicon oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for lithium ion batteries, and in particular to a silicon-carbon-metal composite negative electrode material and a preparation method thereof. Background Art

[0002] At present, rechargeable lithium-ion batteries are widely used in the fields of portable electronic products and electric vehicles. However, commercial lithium-ion batteries mainly use carbon materials such as artificial graphite and natural graphite as negative electrodes. Their theoretical specific capacity is relatively low, only 372mAh / g. When used with commercial lithium iron phosphate and ternary composite positive electrode materials, the energy density of a single cell is 220-270Wh / kg. Further improving the energy density of single cells requires positive and negative electrode materials with higher specific capacity. Therefore, developing high-energy-density, long-cycle-life, and highly-safe lithium-ion battery electrode materials and constructing new electrode structure systems have important research significance and application prospects.

[0003] Among the negative electrode materials for lithium-ion batteries, silicon-based materials have the highest theoretical specific capacity (4200mAh / g), which is 10 times higher than that of traditional graphite electrodes (372mAh / g). In addition, they have the advantages of abundant natural resources and less environmental pollution, and are considered to be one of the negative electrode materials for lithium-ion batteries with great development prospects. However, there are many problems with silicon in commercial applications: first, during the charge and discharge process, large silicon particles undergo huge volume changes, and the stress inside the particles causes the particles to break and pulverize, resulting in performance degradation. Second, due to the change in particle morphology, it is difficult to form a stable solid electrolyte membrane (SEI membrane) on the surface of the negative electrode material, resulting in reduced cycle stability. In addition, the low conductivity of silicon electrodes also limits their application in lithium-ion negative electrode materials. In response to the current problems of silicon-based negative electrodes, the main research ideas include (1) designing nano-silicon structures to inhibit the volume change of silicon during the cycle and improve the cycle stability; (2) compounding with carbon materials to improve their interface stability and conductivity at the same time; (3) actively exploring and researching new electrolyte systems and binder systems.

[0004] Metal organic framework materials are ordered structural materials synthesized by self-assembly bridging of metal centers and organic ligands. After carbonization, they can obtain carbon-metal composite materials with ordered porous structures. They have the advantages of low density, adjustable specific surface area, nitrogen-modified functional groups and uniform metal centers, and are widely used in batteries, catalysis, adsorption and other fields. In the study of improving silicon-based negative electrodes, Han et al. (ACS Applied Materials & Interfaces, 2015, 7(48): 26608) used MOFs to prepare a sandwich-like coating structure, coating a zinc ZIF-8 on the silicon surface and directly using it as an electrode. After 50 charge and discharge cycles, the capacity loss was nearly half. Wu et al. (Applied Surface Science, 2020, 510: 145477) used cobalt MOF-67 by pyrolysis to prepare Si@ZIF-67 silicon-carbon negative electrode material. The capacity of the silicon-carbon negative electrode pyrolyzed at 600°C was 1180 mAh / g, but the polyhedral structure of ZIF-67 could not be well maintained during the expansion and contraction of silicon during the cycle.

[0005] Improving the electrochemical properties of silicon negative electrode by using multiple carbon sources can utilize the synergistic protection of silicon by carbon of different dimensions, thereby improving the electrochemical performance of silicon negative electrode. For example, Chinese patent No. CN105098160A discloses a graphene-doped hollow porous carbon / silicon nanofiber lithium battery negative electrode material and a preparation method thereof. The negative electrode material is composed of graphene and silicon nanoparticles uniformly dispersed in a hollow porous carbon nanofiber matrix, with a mass ratio of carbon / graphene / silicon of 80:15 to 25:2. The carbon nanofiber is in the form of a non-woven fiber felt with a diameter of 300 to 500 nm. The carbon fiber contains cavities and pores with a porosity of 800 to 1000 g / cm 3 , the size of the silicon nanoparticles is 15 to 30 nm.

[0006] Metal modification can improve the conductivity of silicon and the electrochemical performance of silicon negative electrode. For example, the patent with publication number CN114122336A discloses a hollow structure silicon-carbon composite material modified with ultrafine metal nanoparticles and a preparation method thereof. An organic polymer template is prepared, and a template / silicon dioxide core-shell structure composite material is prepared with the template as the core. The core template is then removed by high-temperature pyrolysis to obtain a hollow structure silicon dioxide nanomaterial. Magnesium powder is then added for reduction reaction to obtain a hollow structure silicon nanomaterial. Finally, a hollow structure silicon-carbon composite material modified with ultrafine metal particles is obtained in a nickel salt solution and an additive.

[0007] The above methods improve the electrochemical performance of silicon negative electrodes through a variety of schemes. However, the above methods all have problems such as complex preparation process, difficulty in morphology control, severe volume expansion, and unstable electrode interface. Summary of the invention

[0008] The object of the present invention is to solve at least one of the above-mentioned deficiencies in the prior art. One of the objects of the present invention is to provide a material that can enhance the electrochemical activity of silicon and silicon oxide.

[0009] To achieve the above objectives, the present invention provides a method for preparing a silicon-carbon-metal composite negative electrode material.

[0010] The method comprises the following steps: mixing a metal salt, an organic carbon source, a silicon source, an elemental carbon source and a solvent, and stirring them fully until they are completely dissolved to obtain a first precursor; reacting the first precursor at a certain temperature for a period of time, drying, and obtaining a second precursor; and carbonizing the second precursor at a high temperature to obtain a silicon-carbon-metal composite negative electrode material. The molar mass ratio of the metal salt, the organic carbon source, the silicon source, the elemental carbon source and the solvent is 1:0.3-2.0:1.8-12:0.1-3.5:130-1800.

[0011] According to an exemplary embodiment of the present invention, the metal salt may include one or two of copper sulfate, copper acetate, copper chloride, vanadium pentoxide, vanadium trichloride, vanadyl sulfate, vanadyl acetylacetonate, ferric nitrate, ferric chloride and ferric sulfate.

[0012] According to an exemplary embodiment of the present invention, the organic carbon source may include one or more of 2-methylimidazole, terephthalic acid, trimesic acid and hexamethylenetetramine; the elemental carbon source may include one or more of acetylene black, carbon nanotubes and graphene.

[0013] According to an exemplary embodiment of the present invention, the silicon source may include one or more of nano-silicon and silicon oxide compounds; the solvent may include one or more of water, methanol, ethanol and N,N-dimethylformamide.

[0014] According to an exemplary embodiment of the present invention, the sufficient stirring may include ultrasonic stirring, and the time of ultrasonic stirring is 0.5 to 8 hours.

[0015] According to an exemplary embodiment of the present invention, the reaction temperature may be room temperature to 240°C; the reaction time may be 6 to 72 hours; the drying may include freeze drying or vacuum drying; wherein the drying temperature of freeze drying is -120°C to -50°C, and the drying time is 24 to 96 hours; the drying temperature of vacuum drying is 60 to 170°C, and the drying time is 6 to 48 hours.

[0016] According to an exemplary embodiment of the present invention, the carbonization temperature may be 200-1100° C., and the carbonization time may be 1-12 hours. Inert gas protection is introduced during the carbonization process, and the inert gas may include one or more of nitrogen, argon and helium.

[0017] In another aspect, the present invention provides a silicon-carbon-metal composite negative electrode material, which includes a composite negative electrode material prepared by the method for preparing a silicon-carbon-metal composite negative electrode material.

[0018] According to an exemplary embodiment of the present invention, the material has a metal content of 0.1-10%, a silicon content of 0.1%-99.7%, a carbon content of 0.1-99.7%, and a simple carbon source content of 0.1-20% by mass.

[0019] According to an exemplary embodiment of the present invention, the electrochemical properties of the silicon-carbon-metal composite material may include: the first discharge specific capacity is 1205-2006 mAh / g; the first charge specific capacity is 680-1156 mAh / g; the first coulombic efficiency is 47%-62%; and the reversible specific capacity after 100 cycles is 670-1052 mAh / g.

[0020] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:

[0021] (1) In the composite negative electrode material, the metal organic framework acts as a precursor of metal and a porous carbon, and introduces a second phase elemental carbon source. The composite structure has silicon and silicon oxide compounds uniformly dispersed in the carbon framework constructed by the porous carbon and the elemental carbon source, avoiding the problem of silicon and silicon oxide agglomeration.

[0022] (2) The metal in the composite negative electrode material is evenly dispersed in the carbon skeleton structure, which enhances the catalytic activity of the electrode reaction of silicon and silicon oxide.

[0023] (3) The porous carbon in the composite negative electrode material provides a fast ion diffusion channel, improving the rate performance of silicon and silicon oxide.

[0024] (4) The elemental carbon source in the composite negative electrode material combines with porous carbon to construct a stable three-dimensional skeleton structure, ensuring the long-term cycle stability of silicon and silicon oxide.

[0025] (5) The metal element in the composite negative electrode material combines with the two carbon sources to improve the conductivity of the composite material, and the metal element improves the electrochemical activity of silicon and silicon oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and other objects and features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:

[0027] Figure 1 A flow chart of a method for preparing a silicon-carbon-metal composite negative electrode material according to an exemplary embodiment of the present invention is shown;

[0028] Figure 2 The scanning electron microscope image of the silicon-carbon-graphene-copper composite material prepared in Example 1 of the present invention is shown;

[0029] Figure 3 The graph shows the cyclic stability performance of the silicon-carbon-graphene-copper composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention.

[0031] Aiming at the problems of poor conductivity, severe volume expansion, unstable electrode interface and the like of silicon-based negative electrode materials, the present invention provides a metal-organic framework-modified silicon-carbon-metal composite negative electrode material and a preparation method thereof.

[0032] Exemplary Embodiment 1

[0033] The present exemplary embodiment provides a method for preparing a silicon-carbon-metal composite negative electrode material. Figure 1 The method flow of preparing a silicon-carbon-metal composite negative electrode material of this exemplary embodiment is shown. The method uses a metal organic framework material as a precursor of metal modification and ordered porous carbon, and introduces a single carbon source to prepare a metal organic framework modified silicon-carbon-metal composite negative electrode material.

[0034] The method comprises the following steps:

[0035] S1. Mix an organic metal salt, an organic carbon source, a silicon source, an elemental carbon source and a solvent, and stir them thoroughly until they are completely dissolved to obtain a first precursor.

[0036] In this embodiment, the silicon source is one or more of nano-silicon and silicon oxide compounds. Silicon oxide compounds include silicon dioxide, silicon monoxide or SiO X (X<1).

[0037] In this embodiment, the metal salt may include one or two of copper sulfate, copper acetate, copper chloride, vanadium pentoxide, vanadium trichloride, vanadyl sulfate, vanadyl acetylacetonate, ferric nitrate, ferric chloride and ferric sulfate.

[0038] Metal salts can be divided into two categories: organic metal salts and inorganic metal salts. The present invention can select one of them. For example, the metal salt can be an organic metal salt, and the organic metal salt can include vanadium acetylacetonate or cupric acetate.

[0039] Metal salts can be used to form metal organic framework materials, which can be used as precursors for metal modification and ordered porous carbon. The metal is evenly dispersed in the carbon framework structure, which improves the catalytic activity of the electrode reaction of silicon and silicon oxide. The metal ions in the metal salt are reduced to metal elements, which combine with two carbon sources to improve the conductivity of the composite material. The metal elements can improve the electrochemical activity of silicon and silicon oxide.

[0040] In this embodiment, the organic carbon source may include one or more of 2-methylimidazole, terephthalic acid, trimesic acid and urotropine. After the organic carbon source and the metal salt are combined to form a metal organic framework material, porous carbon is formed by high temperature carbonization. Porous carbon is an organic framework material that provides a fast ion diffusion channel and improves the rate performance of silicon and silicon oxide.

[0041] In this embodiment, the single carbon source is one or more of acetylene black, carbon nanotubes and graphene. The single carbon source is combined with porous carbon to construct a stable three-dimensional skeleton structure to ensure the long-term cycle stability of silicon and silicon oxide.

[0042] In this embodiment, the solvent may be one or more of water, methanol, ethanol and N,N-dimethylformamide.

[0043] The metal organic framework in the composite material acts as a precursor of metal and a porous carbon, and introduces a second phase elemental carbon source. The composite structure has silicon and silicon oxide compounds uniformly dispersed in the carbon skeleton constructed by porous carbon and elemental carbon source, avoiding the problem of silicon and silicon oxide agglomeration.

[0044] In this embodiment, sufficient stirring includes ultrasonic stirring, and the ultrasonic stirring time is 0.5 to 8 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, and 7.5 hours. Further, the ultrasonic stirring time is 1 to 6 hours. During the stirring process, the metal salt will dissociate into metal cations, which will combine with the organic carbon source to form a ligand complex. At the same time, the hydroxyl groups on the surface of the silicon source and the oxygen-containing functional groups on the surface of the carbon source can combine with the metal cations to promote their uniform dispersion in the ligand complex, ensuring that the subsequent formation is a silicon-carbon-metal composite negative electrode material in which silicon and elemental carbon sources are uniformly dispersed.

[0045] In this embodiment, the molar mass ratio of the metal salt, the organic carbon source, the silicon source, the elemental carbon source and the solvent is 1:0.3-2.0:1.8-12:0.1-3.5:130-1800. For example, 1:0.4:1.9:0.2:140, 1:1.5:10:3:1000, 1:1:5:2:1500, 1:1.9:2:0.2:1799, 1:0.8:11:3.4:150.

[0046] S2. Allow the first precursor to react at a certain temperature for a period of time, and dry to obtain a second precursor.

[0047] In this embodiment, the reaction may include a room temperature reaction and a hydrothermal reaction.

[0048] In this embodiment, the reaction temperature is room temperature to 240° C., for example, 30° C., 50° C., 65° C., 70° C., 90° C., 120° C., 150° C., 180° C., 190° C., 210° C., 230° C., 235° C.; further, the reaction temperature is 80 to 200° C. This temperature range promotes the orderly growth of metal organic ligands according to a certain structure.

[0049] In this embodiment, the reaction time is 6 to 72 hours, for example, 6.5 hours, 7 hours, 10 hours, 20 hours, 30 hours, 40 hours, 50 hours, 60 hours, 70 hours, and 71 hours; further, the reaction time is 8 to 48 hours. As the reaction time increases from 6 hours to 72 hours, different ligand complexes will gradually grow, and the particle size can increase from nanometers to micrometers. Therefore, the reaction time can be used to control the size of the reaction particles.

[0050] In this embodiment, drying may include freeze drying and vacuum drying. The drying temperature of freeze drying is -120°C to -50°C, for example, -110°C, -100°C, -90°C, -80°C, -70°C, -60°C, -55°C. The drying time is 24 to 96 hours, for example, 25 hours, 30 hours, 36 hours, 40 hours, 50 hours, 60 hours, 70 hours, 80 hours, 85 hours, 90 hours, 95 hours; more preferably, the drying time is 48 to 72 hours; the drying temperature and drying time can ensure that ethanol, methanol and water are completely sublimated, and N, N-methylformamide solvent is solidified and completely sublimated. The drying temperature of vacuum drying is 60-170°C, for example, 61°C, 65°C, 70°C, 80°C, 90°C, 100°C, 110°C, 115°C, 119°C; the drying time is 6-48h, for example, 7h, 10h, 15h, 24h, 30h, 36h, 40h, 45h, 47h; more preferably, the drying temperature is 60-100°C, and the drying time is 12-48h; the drying temperature and drying time can ensure the evaporation of water, ethanol, methanol and N,N-methylformamide solvents.

[0051] S3. Carbonizing the second precursor at high temperature to obtain a silicon-carbon-metal composite negative electrode material.

[0052] In this embodiment, the carbonization temperature is 200-1100°C, for example, 250°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1050°C, and more preferably, the carbonization temperature is 300-800°C. The carbonization time is 1-12h, for example, 1.5h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 11.5h, and further, 3-10h. The carbonization temperature and carbonization time can ensure that the metal organic ligand is cracked and carbonized to form porous carbon.

[0053] In this embodiment, the carbonization atmosphere is an inactive gas, including one or more of nitrogen, argon and helium.

[0054] Exemplary Embodiment 2

[0055] This exemplary embodiment provides a silicon-carbon-metal composite negative electrode material. The silicon-carbon-metal composite negative electrode material includes a material prepared by the method for preparing a silicon-carbon-metal composite negative electrode material.

[0056] In this embodiment, the silicon-carbon-metal composite negative electrode material includes the following materials by mass percentage: 0.1-10% metal, 0.1-99.7% silicon, 0.1-99.7% carbon, and 0.1-20% single carbon source.

[0057] In this embodiment, the electrochemical properties of the silicon-carbon-metal composite negative electrode material include a first discharge specific capacity of 1205 to 2006 mAh / g; a first charge specific capacity of 680 to 1156 mAh / g; a first coulombic efficiency of 47% to 62%; and a reversible specific capacity of 670 to 1052 mAh / g after 100 cycles.

[0058] In order to better understand the exemplary embodiments of the present invention, they are further described below in conjunction with specific embodiments.

[0059] Example 1

[0060] Weigh 1mmol of trimesic acid and 0.5mmol of urotropine and add them to 30ml of deionized water, mix and dissolve, stir until evenly dispersed to obtain a mixed solution, then add 0.5g of nano silicon powder and continue stirring to form a yellow mixed solution. Prepare 5mg / ml, 10ml of graphene oxide solution and add it to the yellow mixed solution, ultrasonically disperse for 3 hours to form a yellow-brown mixed solution. Weigh 1.5mmol of copper sulfate solid and add it to 20ml of deionized water to form a copper sulfate solution, pour the copper sulfate solution into the above mixed solution, continue stirring to form a uniform mixed solution, and obtain the first precursor.

[0061] The first precursor was stirred and reacted at 80° C. for 6 hours to obtain a blue flocculent hydrogel, and the hydrogel was placed in a freeze dryer and dried at −50° C. for 48 hours to obtain a second precursor.

[0062] The second precursor obtained above was heated to 600° C. at a rate of 2° C. / min in a tube furnace under inert atmosphere protection, and was kept warm for 4 hours and then naturally cooled to obtain a copper-modified silicon-carbon-graphene-copper composite material. Figure 2 This is a scanning electron microscope image with a scale of 10μm of the silicon-carbon-graphene-copper composite material obtained in this embodiment. It can be seen that the porous structure of the metal organic framework is well maintained. The silicon-carbon-graphene-copper composite material prepared in this embodiment was subjected to a constant current charge and discharge test. The active material, CMC, and acetylene black were configured in an 8:1:1 ratio to form a slurry, which was coated on a copper foil. The electrode piece was dried and made into a disc with a diameter of 1cm. Metal lithium was used as the counter electrode. 1MLiPF6 was dissolved in a volume ratio of 1:1:1 EC:DEC:DMC and 5% by mass of FEC was added as the electrolyte. The electrode pieces were assembled into R2032 button cells for testing. The test current density was 1000A / g, and the test results are as follows. Figure 3 As shown, the first discharge specific capacity of the silicon-carbon-graphene-copper composite material is 1507 mAh / g, the first charge specific capacity is 817 mAh / g, and the reversible specific capacity after 100 cycles is 900 mAh / g.

[0063] Example 2

[0064] Weigh 1 mmol of 2-methylimidazole and add it to 30 ml of methanol, mix and dissolve, stir until evenly dispersed to obtain a mixed solution, then add 0.1 g of nano silicon powder and continue stirring to form a yellow mixed solution. Add 0.01 g of carbon nanotubes to the yellow mixed solution and ultrasonically disperse for 3 hours to form a yellow-brown mixed solution. Weigh 3 mmol of copper acetate solid and add it to 30 ml of methanol to form a copper acetate solution. Pour the copper acetate solution into the above mixed solution and continue stirring to form a uniform mixed solution to obtain the first precursor.

[0065] The first precursor was transferred to a hydrothermal reactor at 100° C., and stirred for reaction at 180° C. for 10 hours to obtain a precipitate. The precipitate was washed with water, filtered, and dried in a vacuum oven at 120° C. for 12 hours to obtain a second precursor.

[0066] The second precursor obtained above was heated to 700° C. at a rate of 2° C. / min in a tube furnace under inert atmosphere protection, and was kept warm for 5 hours and then naturally cooled to obtain a copper-modified silicon-carbon-graphene-copper composite material.

[0067] Example 3

[0068] Weigh 4 mmol of terephthalic acid and dissolve it in 40 mL of dimethylformamide, mix and dissolve, stir evenly, then add 0.5 g of silicon oxide and continue stirring to form a mixed solution, add 0.05 g of carbon nanotubes to the mixed solution, and ultrasonically disperse for 6 hours to form a uniform gray solution. Weigh 2 mmol of vanadyl sulfate solid and add it to 20 mL of dimethylformamide, evenly disperse it, then add the vanadyl sulfate solution to the mixed solution, continue stirring to form a uniform mixed solution, and obtain a first precursor.

[0069] The first precursor was transferred to a 100 mL high pressure reactor and reacted in an oven at 180° C. for 48 hours to obtain a yellow-brown solid, which was the second precursor.

[0070] The second precursor obtained above was heated to 350° C. at a rate of 2° C. / min in a tube furnace under nitrogen atmosphere protection, and kept at this temperature for 6 hours and then naturally cooled to obtain a vanadium-modified silicon-carbon-carbon nanotube-vanadium composite material.

[0071] Example 4

[0072] 3 mmol of trimesic acid was weighed and dissolved in 40 mL of ethanol, mixed and dissolved, stirred evenly, and then 0.3 g of nano silicon was added and stirred to form a mixed solution, and 0.05 g of acetylene black was added to the mixed solution, and ultrasonic dispersion was performed for 6 hours to form a uniform yellow solution. 6 mmol of acetylacetonato vanadium solid was weighed and added to 30 mL of ethanol solution, and after uniform dispersion, the acetylacetonato vanadium solution was added to the mixed solution, and stirring was continued to form a uniform mixed solution to obtain a first precursor.

[0073] The first precursor was transferred to a 100 mL autoclave and reacted in an oven at 200° C. for 8 hours to obtain a yellow-green solid. The product was washed with deionized water and dried in a vacuum oven at 80° C. for 16 hours to obtain a second precursor.

[0074] The second precursor obtained above was heated to 500° C. at a rate of 2° C. / min in a tube furnace under the protection of argon atmosphere, and was kept warm for 6 hours and then naturally cooled to obtain a vanadium-modified silicon-carbon-acetylene black-vanadium composite material.

[0075] Example 5

[0076] Weigh 4 mmol of trimesic acid and dissolve it in 40 mL of aqueous solution, mix and dissolve, stir evenly, then add 0.3 g of nano silicon and continue stirring to form a mixed solution, add 0.08 g of acetylene black to the mixed solution, and ultrasonically disperse for 2 hours to form a uniform gray solution. Weigh 2 mmol of ferric chloride solid and add it to 40 mL of aqueous solution, add the ferric chloride solution to the mixed solution after uniform dispersion, and continue stirring to form a uniform mixed solution to obtain a first precursor.

[0077] The first precursor was transferred to a 100 mL high pressure reactor and reacted in an oven at 160° C. for 18 hours to obtain a yellow-brown solid, which was the second precursor.

[0078] The second precursor obtained above was heated to 700° C. at a rate of 5° C. / min in a tubular furnace under nitrogen atmosphere protection, kept at this temperature for 3 hours and then naturally cooled to obtain an iron-modified silicon-carbon-acetylene black-iron composite material.

[0079] Example 6

[0080] Weigh 6 mmol of trimesic acid and dissolve it in 40 mL of methanol solution, mix and dissolve, stir evenly, then add 0.5 g of silicon oxide and continue stirring to form a mixed solution, prepare 1 mg / ml of graphene methanol solution, take 10 mL of the solution and add it to the above mixed solution, and ultrasonically disperse for 5 hours to form a uniform gray solution. Weigh 6 mmol of ferric nitrate solid and add it to 20 mL of methanol solution, add the ferric nitrate solution to the above mixed solution after uniform dispersion, and continue stirring to form a uniform mixed solution to obtain the first precursor.

[0081] The first precursor was transferred to a 100 mL autoclave and reacted in an oven at 180°C for 18 hours to obtain a black solid. The product was washed with deionized water three times and placed in a freeze dryer and dried at -80°C for 72 hours to obtain a second precursor.

[0082] The second precursor obtained above was heated to 800° C. at a rate of 2° C. / min in a tubular furnace under nitrogen atmosphere protection, and was kept warm for 5 hours and then naturally cooled to obtain an iron-modified silicon-carbon-graphene-iron composite material.

[0083] The electrochemical performance of the silicon-carbon-metal composite materials prepared in Examples 1-6 was tested. The test results are shown in Table 1.

[0084] Table 1 Electrochemical performance test results of silicon-carbon-metal composites

[0085]

[0086] Table 1 shows the electrochemical properties of the silicon-carbon-metal composite materials obtained in the above six embodiments. It can be seen that the composite materials can obtain relatively excellent electrochemical properties, indicating that the porous structure in the composite material is conducive to the full infiltration of the electrolyte and the active material, shortening the diffusion path of ions in the bulk material. In addition, the two carbon sources combined with metal modification can ensure that the composite material has good conductivity. The silicon-carbon-metal composite materials prepared in each example maintain good cycle stability.

[0087] In summary, the silicon-carbon-metal composite material prepared by the present invention has excellent electrochemical properties, good electrical conductivity and good cycle stability, and is a good negative electrode material for lithium-ion batteries.

[0088] Although the present invention has been described above by combining with exemplary embodiments, it will be apparent to those skilled in the art that various modifications and changes may be made to the exemplary embodiments of the present invention without departing from the spirit and scope defined in the claims.

Claims

1. A method for preparing a silicon-carbon-metal composite negative electrode material, characterized in that: The method comprises the following steps: Mixing a metal salt, an organic carbon source, a silicon source, an elemental carbon source and a solvent, and stirring them thoroughly until they are completely dissolved to obtain a first precursor; The first precursor is allowed to react at a certain temperature for a period of time, and dried to obtain a second precursor; the reaction temperature is room temperature to 240° C.; the reaction time is 6 to 72 hours; Carbonizing the second precursor at high temperature to obtain a silicon-carbon-metal composite negative electrode material; The molar mass ratio of the metal salt, the organic carbon source, the silicon source, the elemental carbon source and the solvent is 1: 0.3-2.0: 1.8-12: 0.1-3.5: 130-1800; The metal salt includes one or two of copper sulfate, copper acetate, copper chloride, vanadium pentoxide, vanadium trichloride, vanadyl sulfate, vanadyl acetylacetonate, ferric nitrate, ferric chloride and ferric sulfate; The elemental carbon source includes one or more of acetylene black, carbon nanotubes and graphene; The silicon source includes one or more of nano-silicon and silicon-oxygen compounds; The organic carbon source includes one or more of 2-methylimidazole, terephthalic acid, trimesic acid and hexamethylenetetramine; After the organic carbon source and the metal salt are combined to form a metal organic framework material, porous carbon is formed through high temperature carbonization; the silicon source is evenly dispersed in the carbon framework constructed by the porous carbon and the elemental carbon source; and the metal element is evenly dispersed in the carbon framework.

2. The method for preparing a silicon-carbon-metal composite negative electrode material according to claim 1, characterized in that: The solvent includes one or more of water, methanol, ethanol and N,N-dimethylformamide.

3. The method for preparing a silicon-carbon-metal composite negative electrode material according to claim 1, characterized in that: The sufficient stirring includes ultrasonic stirring, and the ultrasonic stirring time is 0.5 to 8 hours.

4. The method for preparing a silicon-carbon-metal composite negative electrode material according to claim 1, characterized in that: The drying includes freeze drying or vacuum drying; wherein, The drying temperature of freeze drying is -120℃~-50℃, and the drying time is 24~96h; The drying temperature of vacuum drying is 60-170°C, and the drying time is 6-48h.

5. The method for preparing a silicon-carbon-metal composite negative electrode material according to claim 1, characterized in that: The carbonization temperature is 200-1100° C., and the carbonization time is 1-12 hours. Inert gas protection is introduced during the carbonization process, and the inert gas includes one or more of nitrogen, argon and helium.

6. A silicon-carbon-metal composite negative electrode material, characterized in that: The material includes a composite negative electrode material prepared by the method for preparing a silicon-carbon-metal composite negative electrode material according to any one of claims 1 to 5.

7. The silicon-carbon-metal composite negative electrode material according to claim 6, characterized in that: Calculated by mass percentage, the metal content of the material is 0.1-10%, the silicon content is 0.1-99.7%, the carbon content is 0.1-99.7%, and the elemental carbon source content is 0.1-20%.

8. The silicon-carbon-metal composite negative electrode material according to claim 6, characterized in that: The electrochemical properties of the silicon-carbon-metal composite material include: The first discharge specific capacity is 1205~2006mAh / g; the first charge specific capacity is 680~1156mAh / g; The first coulombic efficiency is 47% to 62%; the reversible specific capacity after 100 cycles is 670 to 1052 mAh / g.