Electrochemical device and electronic device

The electrochemical device's optimized electrolyte composition addresses lithium deposition issues in lithium-ion batteries, enhancing cycle performance and safety through balanced kinetic and high temperature stability.

CN115066778BActive Publication Date: 2024-12-06NINGDE AMPEREX TECHNOLOGY LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180013415.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-03
Publication Date
2024-12-06
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

Lithium-ion batteries face issues with increased lithium deposition affecting cycle performance and safety as charging speed increases.

Method used

An electrochemical device with a specific composition of fluoroethylene carbonate and a trinitrile compound in the electrolyte, along with controlled ratios and contents of these components, is used to improve the negative electrode's kinetic performance and balance high temperature stability, enhancing cycle performance, energy density, and safety.

Benefits of technology

The proposed electrolyte composition improves lithium-ion battery performance by preventing lithium precipitation, ensuring good cycle performance, energy density, and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003786584860000111
    Figure BDA0003786584860000111
  • Figure BDA0003786584860000121
    Figure BDA0003786584860000121
  • Figure BDA0003786584860000131
    Figure BDA0003786584860000131
Patent Text Reader

Abstract

The present application provides an electrochemical device and an electronic device, including a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte includes fluoroethylene carbonate and a trinitrile compound, based on the mass of the electrolyte, the mass percentage of fluoroethylene carbonate is A%, 2≤A≤6, the mass percentage of the trinitrile compound is B%, 2≤B≤5, and A and B satisfy: 4≤A×B≤20; the defect degree of the negative electrode is Id / Ig, satisfying: 0.07<Id / Ig≤0.13, and the mass percentage of fluoroethylene carbonate A% and Id / Ig satisfy: 1.5≤A / (10×Id / Ig)≤8.6. The present application improves the energy density, cycle performance and safety performance of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in various fields such as power storage, portable electronic devices and electric vehicles. As the scope of use of lithium-ion batteries continues to expand, the market has put forward higher requirements for lithium-ion batteries, such as requiring lithium-ion batteries to have faster charging speed and longer service life.

[0003] However, as the charging speed of lithium-ion batteries increases, lithium deposition becomes more likely, affecting the cycle performance and safety of lithium-ion batteries. Summary of the invention

[0004] The purpose of this application is to provide an electrochemical device and an electronic device to improve the cycle performance of the electrochemical device. The specific technical solution is as follows:

[0005] The first aspect of the present application provides an electrochemical device, which includes a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte includes fluoroethylene carbonate and a trinitrile compound, based on the mass of the electrolyte, the mass percentage of fluoroethylene carbonate is A%, 2≤A≤6, for example, A can be 2, 3, 4, 5, 6 or any range therebetween; the mass percentage of the trinitrile compound is B%, 2≤B≤5, for example, B can be 2, 2.5, 3, 3.5, 4, 4.5, 5 or any range therebetween. A and B satisfy: 4≤A×B≤20, for example, A×B can be 4, 5, 6, 8, 10, 12, 15, 17, 20 or any range therebetween. The defect degree of the negative electrode is Id / Ig, which satisfies: 0.07<Id / Ig≤0.13, for example, Id / Ig can be 0.07, 0.08, 0.09, 0.10, 0.12, 0.13 or any range therebetween, and the mass percentage content A% of fluoroethylene carbonate and Id / Ig satisfy: 1.5≤A / (10×Id / Ig)≤8.6, for example, A / (10×Id / Ig) can be 1.5, 2, 3, 3.5, 4, 5, 6, 7, 8, 8.6 or any range therebetween. Without being limited to any theory, by adjusting A×(10×Id / Ig) within the above range, a lithium-ion battery with good cycle performance, energy density and safety performance can be obtained. The positive electrode of the present application may refer to the positive electrode sheet, and the negative electrode may refer to the negative electrode sheet.

[0006] The inventors of the present application have found that by adjusting A×B and A / (10×Id / Ig) within the above ranges, the energy density and cycle performance of lithium-ion batteries can be improved. Without being limited to any theory, this may be because when the electrolyte of the present application contains trinitrile compounds in the above content range, although the trinitrile compounds can improve the stability of the positive electrode interface, the kinetic performance of the lithium-ion battery also needs to be improved to obtain a higher charging speed. Based on this, the present application can improve the kinetic performance of lithium-ion batteries while improving lithium precipitation by adjusting the content of fluoroethylene carbonate, a negative electrode film-forming additive; by synergistically adjusting A / (10×Id / Ig), the negative electrode kinetic performance and high temperature stability of lithium-ion batteries can be balanced, so that the lithium-ion battery has good cycle performance, energy density and safety performance as a whole.

[0007] In one embodiment of the present application, the positive electrode includes a positive electrode active material, the positive electrode active material includes a metal element M, the metal element M includes at least one of Ti, Mg or Al, the content of the metal element M in the positive electrode active material is C ppm, and C and B satisfy: 8≤C×B / 1000≤30, for example, C×B / 1000 can be 8, 10, 13, 15, 18, 20, 22, 25, 27, 30 or any range therebetween. The present application can improve the structural stability of the positive electrode active material by adjusting C×B / 1000 within the above range, thereby improving the energy density and cycle performance of the lithium-ion battery.

[0008] In one embodiment of the present application, Id / Ig satisfies C / (1000×Id / Ig)≥20, preferably 20≤C / (1000×Id / Ig)≤70. C / (1000×Id / Ig) can be 20, 25, 30, 35, 50, 55, 60, 70 or any range therebetween. Not limited to any theory, if C / (1000×Id / Ig) is too small (for example, less than 20), it is not conducive to improving the cycle stability of the lithium-ion battery. By adjusting A×(10×Id / Ig) within the above range, a lithium-ion battery with good cycle performance, energy density and safety performance can be obtained.

[0009] In the present application, in the defect degree of the negative electrode Id / Ig, Id refers to the peak intensity of the D peak in the Raman spectrum of the negative electrode active material, and Ig refers to the peak intensity of the G peak in the Raman spectrum of the negative electrode active material. Id / Ig represents the density of defects in the negative electrode active material. The greater the Id / Ig ratio, the greater the defect degree. The present application does not particularly limit the method for adjusting the defect degree of the negative electrode, such as surface coating of the negative electrode active material. The defect degree of the negative electrode active material generally decreases with the increase of the ratio of the surface coating layer to the substrate coating area. Therefore, the defect degree of the negative electrode active material can be adjusted by adjusting the ratio of the surface coating layer to the substrate coating area.

[0010] In one embodiment of the present application, the content C of the metal element M in the positive electrode active material satisfies: 2000ppm≤C≤6500ppm. For example, C can be 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm or any range therebetween. Not limited to any theory, when C is too low (for example, less than 2000ppm), the improvement in the cycle performance of the lithium-ion battery is limited; when C is too high (for example, greater than 6500ppm), the relative content of the positive electrode active material decreases, which is not conducive to the improvement of its energy density. By adjusting C within the above range, a lithium-ion battery with good cycle performance, energy density and safety performance can be obtained.

[0011] In one embodiment of the present application, the electrolyte further includes ethylene carbonate and propylene carbonate. Based on the mass of the electrolyte, the mass percentage of ethylene carbonate is D%, and the mass percentage of propylene carbonate is E%, and D and E satisfy: 15≤D+E≤40, and D / E≥1.2, preferably 1.2≤D / E≤3.5. For example, D+E can be 15, 20, 25, 30, 35, 40 or any range therebetween, and E / D can be 1.2, 1.3, 1.4, 1.5, 2, 2.5, 3, 3.5 or any range therebetween. Without being limited to any theory, by synergistically adjusting D+E and E / D within the above range, the energy density and cycle performance of lithium-ion batteries can be further improved, lithium plating of lithium-ion batteries can be reduced, and the safety of lithium-ion batteries can be improved.

[0012] In one embodiment of the present application, the mass percentage content D% of ethylene carbonate and the mass percentage content A% of fluoroethylene carbonate satisfy: D×A≥35, preferably 35≤D×A≤150. For example, D×A is 35, 50, 70, 80, 100, 110, 130, 150 or any range therebetween. Without being limited to any theory, by adjusting D×A within the above range, a lithium-ion battery with good cycle performance, energy density and safety performance can be obtained.

[0013] In one embodiment of the present application, the mass percentage B% of the trinitrile compound, the mass percentage D% of the ethylene carbonate, and the mass percentage E% of the propylene carbonate satisfy the following conditions: B×(D+E)≤150, preferably 40≤B×(D+E)≤150. For example, B×(D+E) may be 40, 50, 60, 80, 100, 110, 130, 140, 150, or any range therebetween. Without being limited to any theory, by adjusting B×(D+E) within the above range, a lithium ion battery with good cycle performance, energy density, and safety performance can be obtained.

[0014] In one embodiment of the present application, the electrolyte further comprises a dinitrile compound, and based on the mass of the electrolyte, the mass percentage of the dinitrile compound is F%, 1≤F≤6, and F and B satisfy: 4≤F+B≤9. For example, F can be 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6 or any range therebetween. F+B can be 4, 4.5, 5, 5.5, 6.5, 7, 8, 8.5, 9 or any range therebetween. Without being limited to any theory, by synergistically adjusting F and F+B within the above range, the positive electrode can be effectively protected, and the cycle performance and energy density of the lithium-ion battery can be further improved.

[0015] In one embodiment of the present application, the electrolyte further includes at least one of 1,3-propane sultone, vinyl sulfate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate or γ-butyrolactone. The electrochemical device satisfies at least one of the following conditions: a) based on the mass of the electrolyte, the mass percentage of the 1,3-propane sultone is 0.5% to 5%, b) based on the mass of the electrolyte, the mass percentage of the vinyl sulfate is 0.1% to 1%, c) based on the mass of the electrolyte, the mass percentage of the vinylene carbonate is 0.1% to 1%, d) based on the mass of the electrolyte, the mass percentage of the dimethyl carbonate is 0.1% to 30%, e) based on the mass of the electrolyte, the mass percentage of the diethyl carbonate is 0.1% to 30%, f) based on the mass of the electrolyte, the mass percentage of the ethyl methyl carbonate is 0.1% to 30%, g) based on the mass of the electrolyte, the mass percentage of the γ-butyrolactone is 0.01% to 5%. Without being limited to any theory, by adjusting the above electrolyte additives within the scope of this application, the cycle performance and energy density of the lithium-ion battery can be further improved.

[0016] The present application has no particular restrictions on the trinitrile compound, as long as the purpose of the present application can be achieved. For example, the trinitrile compound includes at least one of 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,2,4-tris(2-cyanoethoxy)butane or 1,2,5-tris(cyanoethoxy)pentane.

[0017] The electrolyte of the present application includes a lithium salt, and the present application has no particular restrictions on the lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, or lithium difluorophosphate.

[0018] The present application has no particular restrictions on the dinitrile compound, as long as the purpose of the present application can be achieved. For example, the dinitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanooctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile or 2,2,4,4-tetramethylglutaronitrile.

[0019] A second aspect of the present application provides an electronic device comprising the electrochemical device described in the above embodiments of the present application.

[0020] The present application provides an electrochemical device and an electronic device, wherein the electrolyte in the electrochemical device comprises fluoroethylene carbonate and a trinitrile compound, wherein the mass percentage of the fluoroethylene carbonate is A%, 2≤A≤6, the mass percentage of the trinitrile compound is B%, 2≤B≤5, A and B satisfy: 4≤A×B≤20, the defect degree of the negative electrode is Id / Ig, satisfying: 0.07<Id / Ig≤0.13, the mass percentage of the fluoroethylene carbonate A% and Id / Ig satisfy: 1.5≤A / (10×Id / Ig)≤8.6, thereby improving the cycle performance, energy density and safety performance of the electrochemical device. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical scheme, and advantages of the present application more clearly understood, the present application is further described in detail with reference to the embodiments below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other technical schemes obtained by ordinary technicians in the field belong to the scope of protection of the present application.

[0022] It should be noted that in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.

[0023] The present application does not particularly limit the preparation method of the positive electrode active material containing the metal element M (hereinafter referred to as the modified positive electrode active material), and the preparation method of those skilled in the art can be adopted. For example, an aluminum-containing compound (such as Al2O3, Al(OH)3, AlF3), a magnesium-containing compound (such as MgO) or a Ti-containing compound (such as TiO2) can be added to the positive electrode active material LiCoO2 to obtain the above-mentioned modified positive electrode active material. In addition, the present application can achieve the change of the metal element M in the positive electrode active material layer by adjusting the content of the metal element M in the modified positive electrode active material, such as adjusting the amount of the compound containing the metal element M. The present application does not specifically limit the adjustment process, as long as the purpose of the present application can be achieved.

[0024] The positive electrode current collector in the present application is not particularly limited and can be any positive electrode current collector in the art, such as aluminum foil, aluminum alloy foil or composite current collector.

[0025] The negative electrode current collector in the present application is not particularly limited, and materials such as metal foil or porous metal plate can be used, such as foil or porous plate of metals such as copper, nickel, titanium or iron or their alloys, such as copper foil. The negative electrode active material layer includes a negative electrode active material, a conductive agent, a binder and a thickener. The binder can be at least one of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin or carboxymethyl cellulose (CMC); the thickener can be carboxymethyl cellulose (CMC).

[0026] The substrate of the isolation film of the present application includes, but is not limited to, at least one selected from polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyimide (PI) or aramid. For example, polyethylene includes at least one component selected from high-density polyethylene, low-density polyethylene and ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have excellent effects on preventing short circuits and can improve the stability of electrochemical devices through the shutdown effect. The substrate can be a single-layer structure or a multi-layer composite structure of a plurality of mixtures, with a thickness of 3μm to 20μm.

[0027] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0028] The preparation process of the electrochemical device is well known to those skilled in the art and is not particularly limited in this application. For example, a lithium-ion battery can be manufactured by overlapping the positive electrode and the negative electrode via a separator, and placing them in a housing after winding, folding, etc. as required, injecting an electrolyte into the housing and sealing it. In addition, an overcurrent protection element, a guide plate, etc. can also be placed in the housing as required to prevent the pressure inside the lithium-ion battery from rising and overcharging and discharging.

[0029] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0030] Test methods and equipment:

[0031] Cathode active material metal element M content test:

[0032] The active material of the positive electrode sheet washed with DMC (dimethyl carbonate) is scraped off with a scraper, dissolved with a mixed solvent (for example, 0.4 g of positive electrode active material uses 10 ml of aqua regia (nitric acid and hydrochloric acid mixed in a ratio of 1:1) and 2 ml of HF mixed solvent), the volume is fixed to 100 ml, and then the content of metal elements M such as Ti, Mg, and Al in the solution is tested using an ICP analyzer in ppm.

[0033] Negative electrode defect degree test:

[0034] The dried negative electrode sheet is kept flat on the sample stage of the Raman test instrument (JobinYvonLabRAM HR) for testing to obtain a Raman spectrum. The peak intensity of the D peak and the peak intensity of the G peak are determined in the Raman spectrum, and Id / Ig is calculated, which is the degree of defect of the negative electrode.

[0035] Lithium-ion battery cycle performance test:

[0036] At 25°C, the lithium-ion battery is charged to 4.5V at a constant current of 0.7C (rate), then charged to a current of 0.05C at a constant voltage, and then discharged to 3.0V at a constant current of 1C. This is a charge and discharge cycle, which is the first cycle. The discharge capacity of the lithium-ion battery in the first cycle is recorded. The lithium-ion battery is charged and discharged according to the above method, and the discharge capacity of each cycle is recorded until the discharge capacity of the lithium-ion battery decays to 80% of the discharge capacity of the first cycle. The number of charge and discharge cycles is recorded.

[0037] Capacity test of lithium-ion battery:

[0038] In a constant temperature box at 25±0.5℃, the lithium-ion battery is charged at a constant current of 0.5C (rate) to a voltage of 4.5V, then charged at a constant voltage of 4.5V to a current of 0.05C, and then discharged at a constant current of 0.2C rate to a voltage of 3V. The discharge capacity obtained is the battery capacity of the lithium-ion battery.

[0039] Lithium ion battery lithium deposition degree test:

[0040] 1) Place the lithium-ion battery in a 10°C high and low temperature box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature;

[0041] 2) Discharge the lithium-ion battery that has reached a constant temperature at a constant current of 0.5C until the voltage reaches 3.0V;

[0042] 3) After standing for 10 minutes, charge at a constant current of 0.1C to a voltage of 4.5V, and then charge at a constant voltage of 4.5V to a current of 0.05C (record the charge capacity C1);

[0043] 4) After standing for 10 minutes, discharge at a constant current of 0.5C to a voltage of 3.0V. After standing for 10 minutes, discharge at a constant current of 0.025C to a voltage of 3.0V. After standing for another 10 minutes, discharge at a constant current of 0.005C to a voltage of 3.0V. The discharge capacity after the completion of this step is recorded as D1.

[0044] 5) After standing for 10 minutes, charge at 0.7C constant current to 4.5V, then charge at 4.5V constant voltage to 0.05C;

[0045] 6) After standing for 10 minutes, discharge at a constant current of 0.5C to a voltage of 3.0V. After standing for 10 minutes, discharge at a constant current of 0.025C to a voltage of 3.0V. After standing for another 10 minutes, discharge at a constant current of 0.005C to a voltage of 3.0V.

[0046] 7) Repeat step 5) and step 6) 12 times, and record the last complete discharge capacity as D12. Calculate the amount of lithium deposition as the basis for judging the charging performance (the lower the amount of lithium deposition, the milder the degree of lithium deposition; when the amount of lithium deposition is less than 0.3, it is difficult to see lithium deposition with the naked eye), where the amount of lithium deposition is calculated as follows:

[0047] Lithium deposition amount = (C1-D12) / C1.

[0048] Example 1

[0049] <Preparation of Modified Positive Electrode Active Material>

[0050] Commercially available lithium cobalt oxide (LiCoO2) and oxide containing metal element M (a mixture of magnesium oxide (MgO), titanium dioxide (TiO2), and aluminum oxide (Al2O3)) are mixed, mixed in a high-speed mixer at 300r / min for 20min, placed in an air kiln, heated to 820°C at 5°C / min, maintained for 24h, taken out after natural cooling, and sieved through a 300-mesh sieve to obtain a modified positive electrode active material (i.e., modified LiCoO2). In the modified positive electrode active material, the total content of metal element M (Mg, Ti, Al) in the positive electrode active material is 4000ppm, and the molar ratio of Mg element, Ti element, and Al element is 1:1:1.

[0051] <Preparation of positive electrode sheet>

[0052] The prepared modified LiCoO2, conductive agent carbon nanotube (CNT), and binder polyvinylidene fluoride are mixed in a mass ratio of 95:2:3, and N-methylpyrrolidone (NMP) is added as a solvent. The system is stirred under the action of a vacuum mixer until it becomes a uniform positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on a positive electrode current collector aluminum foil with a thickness of 12μm, dried at 85℃, and cold pressed to obtain a positive electrode sheet with a positive electrode active material layer thickness of 100μm, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use.

[0053] <Preparation of negative electrode sheet>

[0054] The negative electrode active material artificial graphite, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) are mixed in a mass ratio of 95:2:3, and then deionized water is added as a solvent to prepare a slurry with a solid content of 70wt%, and stirred evenly. The slurry is evenly coated on one surface of a copper foil with a thickness of 8μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a single-sided negative electrode active material layer coated with a negative electrode active material layer with a thickness of 150μm, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a double-sided negative electrode active material layer. The negative electrode sheet is cut into a specification of (74mm×867mm) and welded to the pole ear for standby use. Among them, the defect degree Id / Ig of the negative electrode sheet is 0.1.

[0055] <Preparation of Electrolyte>

[0056] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were uniformly mixed in a weight ratio of 1:1:1 as a base solvent, and LiPF6, trinitrile compound 1,3,6-hexane trinitrile and fluoroethylene carbonate were added and stirred evenly to form an electrolyte, wherein the concentration of LiPF6 was 12.5wt%, and the mass percentages of the trinitrile compound 1,3,6-hexane trinitrile and fluoroethylene carbonate were as shown in Table 1.

[0057] <Preparation of Separator Film>

[0058] A polyethylene (PE) porous polymer film with a thickness of 15 μm was used as the isolation membrane.

[0059] <Preparation of lithium-ion batteries>

[0060] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the moisture is removed at 80°C, and the prepared electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.

[0061] Example 2 to Example 5

[0062] Except for adjusting the content of fluoroethylene carbonate in the electrolyte and adjusting the defect degree Id / Ig of the negative electrode sheet by adjusting the ratio of the negative electrode coating layer to the substrate coating area, the changes in relevant preparation parameters and performance are shown in Table 1, and the rest is the same as Example 1.

[0063] Example 6 to Example 8

[0064] Except for adjusting the content of fluoroethylene carbonate and the content of trinitrile compound in the electrolyte, the changes of relevant preparation parameters and performance are shown in Table 1, and the rest is the same as Example 1.

[0065] Example 9 to Example 20

[0066] Except for adjusting the type of trinitrile compound, the content of fluoroethylene carbonate, the content of trinitrile compound, and the total content of metal element M in the electrolyte, the changes in relevant preparation parameters and performance are shown in Table 2, and the rest is the same as Example 1.

[0067] Embodiment 21

[0068] Except that in <Preparation of modified positive electrode active material>, the oxide containing metal element M is a mixture of MgO and Al2O3, the molar ratio of Mg element to Al element is 1:1, and the changes in relevant preparation parameters and performance are shown in Table 2, the rest is the same as Example 18.

[0069] Embodiment 22

[0070] Except that in <Preparation of modified positive electrode active material>, the oxide containing the metal element M is Al2O3, and the changes in relevant preparation parameters and performance are shown in Table 2, the rest is the same as Example 18.

[0071] Embodiment 23

[0072] Except for the fact that <Preparation of electrolyte> is different from Example 1, the rest is the same as Example 1.

[0073] <Preparation of Electrolyte>

[0074] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were uniformly mixed in a weight ratio of 9:7:64.5 as a base solvent, and LiPF6, trinitrile compound 1,3,6-hexanetrinitrile and fluoroethylene carbonate were added and stirred to form an electrolyte, wherein the concentration of LiPF6 was 12.5wt%, and the mass percentage of the trinitrile compound 1,3,6-hexanetrinitrile and fluoroethylene carbonate and the changes in related preparation parameters and properties are shown in Table 3.

[0075] Embodiment 24

[0076] Except for the fact that <Preparation of electrolyte> is different from Example 1, the rest is the same as Example 1.

[0077] <Preparation of Electrolyte>

[0078] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were uniformly mixed in a weight ratio of 20:8:52.5 as a base solvent, and LiPF6, trinitrile compound 1,3,6-hexanetrinitrile and fluoroethylene carbonate were added and stirred to form an electrolyte, wherein the concentration of LiPF6 was 12.5wt%, and the mass percentage of the trinitrile compound 1,3,6-hexanetrinitrile and fluoroethylene carbonate and the changes in related preparation parameters and properties are shown in Table 3.

[0079] Embodiment 25

[0080] Except for the fact that <Preparation of electrolyte> is different from Example 1, the rest is the same as Example 1.

[0081] <Preparation of Electrolyte>

[0082] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were uniformly mixed in a weight ratio of 30:10:40.5 as a base solvent, and LiPF6, trinitrile compound 1,3,6-hexanetrinitrile and fluoroethylene carbonate were added and stirred to form an electrolyte, wherein the concentration of LiPF6 was 12.5wt%, and the mass percentage of the trinitrile compound 1,3,6-hexanetrinitrile and fluoroethylene carbonate and the changes in related preparation parameters and properties are shown in Table 3.

[0083] Embodiment 26

[0084] Except for the fact that <Preparation of electrolyte> is different from Example 13, the rest is the same as Example 13.

[0085] <Preparation of Electrolyte>

[0086] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were uniformly mixed in a weight ratio of 1:1:1 as a base solvent, and LiPF6, a trinitrile compound 1,3,6-hexanetrinitrile, fluoroethylene carbonate and a dinitrile compound succinonitrile were added and stirred evenly to form an electrolyte, wherein the concentration of LiPF6 was 12.5wt%, and the mass percentages of the trinitrile compound 1,3,6-hexanetrinitrile, fluoroethylene carbonate and a dinitrile compound succinonitrile and the changes in related preparation parameters and properties are shown in Table 4.

[0087] Example 27 to Example 31

[0088] Except that the type and content of the dinitrile compound were adjusted as shown in Table 4 in <Preparation of electrolyte>, the rest was the same as Example 26.

[0089] Embodiment 32

[0090] Except for the fact that <Preparation of electrolyte> is different from Example 13, the rest is the same as Example 13.

[0091] <Preparation of Electrolyte>

[0092] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were uniformly mixed in a weight ratio of 1:1:1 as a base solvent, and LiPF6, a trinitrile compound 1,3,6-hexane trinitrile, fluoroethylene carbonate and an additive 1,3-propane sultone were added and stirred evenly to form an electrolyte, wherein the concentration of LiPF6 was 12.5wt%, and the mass percentages of the trinitrile compound 1,3,6-hexane trinitrile, fluoroethylene carbonate and the additive 1,3-propane sultone and the changes in related preparation parameters and properties are shown in Table 4.

[0093] Example 33 to Example 34

[0094] Except for adjusting the type and content of additives as shown in Table 5 in <Preparation of electrolyte>, the rest is the same as Example 32.

[0095] Comparative Example 1, Comparative Example 2

[0096] Except for adjusting the content of fluoroethylene carbonate and the content of trinitrile compound in the electrolyte, the changes of relevant preparation parameters and performance are shown in Table 1, and the rest is the same as Example 1.

[0097] Comparative Examples 3 to 6

[0098] Except for adjusting the type of trinitrile compound, the content of fluoroethylene carbonate, the content of trinitrile compound, and the total content of metal element M in the electrolyte, the changes in relevant preparation parameters and performance are shown in Table 2, and the rest is the same as Example 1.

[0099]

[0100]

[0101]

[0102] Table 5

[0103]

[0104] In Table 5, “ / ” means not contained or not measured.

[0105] It can be seen from Table 1 that by adjusting A×B and A / (10×Id / Ig) within the scope of the present application, the battery capacity and capacity retention rate of the lithium-ion battery are significantly improved, and lithium plating does not occur in the lithium-ion battery, indicating that the lithium-ion battery of the present application has good cycle performance, capacity performance and safety performance.

[0106] It can be seen from Examples 9 to 14 and Comparative Examples 3 to 4 in Table 2 that, on the basis of satisfying A×B and A / (10×Id / Ig) within the scope of this application, by adjusting C×B / 1000 within the scope of this application, the battery capacity and capacity retention rate of the lithium-ion battery are significantly improved, and lithium plating does not occur in the lithium-ion battery, indicating that the lithium-ion battery of the present application has good cycle performance, capacity performance and safety performance.

[0107] It can be seen from Examples 15 to 18 and Comparative Examples 5 to 6 in Table 2 that when the content of the metal element M is too high (e.g., Comparative Example 5), the battery capacity and capacity retention rate of the lithium-ion battery are significantly reduced, and slight lithium precipitation occurs; when the content of the metal element M is too low (e.g., Comparative Example 6), the battery capacity and capacity retention rate of the lithium-ion battery are also significantly reduced, and slight lithium precipitation occurs. It can be seen that on the basis of satisfying A×B and A / (10×Id / Ig) within the scope of this application, by controlling the content of the metal element M and C×B / 1000 within the scope of this application, a lithium-ion battery with good cycle performance, capacity performance and safety performance can be obtained.

[0108] It can be seen from Example 12, Example 19 and Example 20 in Table 2 that, on the basis of satisfying A×B, A / (10×Id / Ig) within the scope of this application, as long as the type of trinitrile compound is within the scope of this application, a lithium ion battery with good cycle performance and safety performance can be obtained.

[0109] It can be seen from Example 18, Example 21 and Example 22 that, on the basis of satisfying A×B, A / (10×Id / Ig) within the scope of this application, as long as the type of metal element M is within the scope of this application, a lithium-ion battery with good cycle performance and safety performance can be obtained.

[0110] It can be seen from Examples 9 to 22 in Table 2 that, on the basis of satisfying A×B and A / (10×Id / Ig) within the scope of this application, by adjusting C / (1000×Id / Ig) within the scope of this application, a lithium-ion battery with good battery capacity, capacity retention rate and safety performance can be obtained.

[0111] It can be seen from Examples 13 and 23 to 25 in Table 3 that, on the basis of satisfying A×B and A / (10×Id / Ig) within the scope of this application, a lithium ion battery with good cycle performance can be obtained by adjusting the content of ethylene carbonate and propylene carbonate.

[0112] It can be seen from Example 13 and Example 26 to Example 31 in Table 4 that, on the basis of satisfying A×B and A / (10×Id / Ig) within the scope of this application, when the electrolyte further includes a dinitrile compound, and the sum of the contents of the dinitrile compound and the trinitrile compound is within the scope of this application, the cycle performance of the lithium-ion battery can be further improved.

[0113] It can be seen from Example 13 and Example 32 to Example 34 in Table 5 that, on the basis of satisfying A×B, A / (10×Id / Ig) within the scope of this application, when the electrolyte further includes at least one additive of 1,3-propane sultone, vinyl sulfate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate or γ-butyrolactone, the cycle performance of the lithium ion battery can be further improved.

[0114] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. An electrochemical device comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein: The electrolyte includes fluoroethylene carbonate and a trinitrile compound. Based on the mass of the electrolyte, the mass percentage of the fluoroethylene carbonate is A%, 2≤A≤6, the mass percentage of the trinitrile compound is B%, 2≤B≤5, A and B satisfy: 4≤A×B≤20, the defect degree of the negative electrode is Id / Ig, satisfying: 0.07<Id / Ig≤0.13, and the mass percentage of the fluoroethylene carbonate A% and Id / Ig satisfy: 1.5≤A / (10×Id / Ig)≤8.

6.

2. The electrochemical device according to claim 1, wherein: The positive electrode includes a positive electrode active material, the positive electrode active material includes a metal element M, the metal element M includes at least one of Ti, Mg or Al, the content of the metal element M in the positive electrode active material is C ppm, and C and B satisfy: 8≤C×B / 1000≤30.

3. The electrochemical device according to claim 2, wherein: C / (1000×Id / Ig)≥20.

4. The electrochemical device according to claim 1, wherein The content C of the metal element M in the positive electrode active material satisfies: 2000ppm≤C≤6500ppm.

5. The electrochemical device according to claim 1, wherein The electrolyte also includes ethylene carbonate and propylene carbonate. Based on the mass of the electrolyte, the mass percentage of ethylene carbonate is D%, and the mass percentage of propylene carbonate is E%. D and E satisfy: 15≤D+E≤40, and D / E≥1.

2.

6. The electrochemical device according to claim 5, wherein: The mass percentage content D% of ethylene carbonate and the mass percentage content A% of fluoroethylene carbonate satisfy: D×A≥35.

7. The electrochemical device according to claim 5, wherein: The mass percentage content B% of the trinitrile compound, the mass percentage content D% of the ethylene carbonate, and the mass percentage content E% of the propylene carbonate satisfy: B×(D+E)≤150.

8. The electrochemical device according to claim 1, wherein The electrolyte further includes a dinitrile compound. Based on the mass of the electrolyte, the mass percentage of the dinitrile compound is F%, 1≤F≤6, and F and B satisfy the following: 4≤F+B≤9.

9. The electrochemical device according to claim 1, wherein: The electrolyte further includes at least one of 1,3-propane sultone, vinyl sulfate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate or γ-butyrolactone.

10. The electrochemical device according to claim 9, wherein: The electrochemical device satisfies at least one of the following conditions: a) based on the mass of the electrolyte, the mass percentage of the 1,3-propane sultone is 0.5% to 5%; b) based on the mass of the electrolyte, the mass percentage of the vinyl sulfate is 0.1% to 1%; c) based on the mass of the electrolyte, the mass percentage of the vinylene carbonate is 0.1% to 1%; d) based on the mass of the electrolyte, the mass percentage of dimethyl carbonate is 0.1% to 30%; e) based on the mass of the electrolyte, the mass percentage of diethyl carbonate is 0.1% to 30%; f) based on the mass of the electrolyte, the mass percentage of the ethyl methyl carbonate is 0.1% to 30%; g) Based on the mass of the electrolyte, the mass percentage of the γ-butyrolactone is 0.01% to 5%.

11. The electrochemical device according to claim 1, wherein The trinitrile compound includes at least one of 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,2,4-tris(2-cyanoethoxy)butane or 1,2,5-tris(cyanoethoxy)pentane.

12. The electrochemical device according to claim 1, wherein The electrolyte includes a lithium salt, and the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate or lithium difluorophosphate.

13. The electrochemical device according to claim 8, wherein: The dinitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanooctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile or 2,2,4,4-tetramethylglutaronitrile.

14. An electronic device comprising the electrochemical device according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Lithium secondary cell

    CN103493276A

  • Electrochemical device and electronic equipment

    CN113097433A

  • Electrochemical device and electronic device

    CN113097438A

  • Lithium ion secondary battery

    JP2017199547A