Method for removing contaminants from diffusion coated components

Using laser beam pulse technology to remove contaminants and additive layers on gas turbine engine components, combined with high-temperature aluminide coating regeneration, solves the problems of substrate damage and high cost in diffusion coating removal in the existing technology, achieving efficient and safe Coating regeneration and protective coating formation.

CN115069681BActive Publication Date: 2024-10-29GENERAL ELECTRIC CO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210231769.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-09
Publication Date
2024-10-29
Estimated Expiration
2042-03-09

AI Technical Summary

Technical Problem

When the existing technology removes diffusion coating contaminants from gas turbine engine components, it is easy to damage the substrate surface, resulting in thin component walls or changes in airflow characteristics, and the use of acid stripping and other methods has safety hazards and high costs.

Method used

Laser beam pulse technology is used to remove contaminants on the coated component, selectively removing the additive layer and oxide layer without damaging the diffusion zone, and then applying an aluminide coating at high temperature to form a protective coating.

Benefits of technology

Effectively reduces recoating time and cost, maintains the chemical composition and microstructure of the coating, meets dimensional and airflow requirements, increases the yield of repair hardware, and reduces the consumption of wall thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115069681B_ABST
    Figure CN115069681B_ABST
Patent Text Reader

Abstract

A method of removing contaminants from a surface of a gas turbine engine component protected by a diffusion coating, the diffusion coating comprising an additive layer on the component surface and a diffusion zone in the component surface. The method comprises: subjecting the surface containing the contaminants to laser beam pulses to remove the contaminants from the component, such that the contaminants on the component surface are removed without damaging or removing the diffusion zone of the diffusion coating. A method for controlled removal of at least a portion of the thickness of a diffusion coating from a coated superalloy component is also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority information

[0002] This application claims priority from European patent application No. 21461524.7 filed on March 10, 2021. Technical Field

[0003] The present disclosure relates generally to methods for repairing gas turbine engine components protected by diffusion coatings, and more particularly, to methods for removing contaminants from diffusion coatings. Background Art

[0004] When turbines are used in aircraft or for power generation, they are typically run at the highest possible temperature to achieve maximum operating efficiency. Because high temperatures can damage the alloys used for the components, a variety of methods have been used to increase the operating temperature of metal components.

[0005] Nickel-based superalloys are used in many of the highest temperature material applications in gas turbine engines. For example, nickel-based high-temperature alloys are used to manufacture components such as high-pressure and low-pressure gas turbine blades, impellers or nozzles, stators and shrouds. These components are subject to extreme pressure and environmental conditions. The composition of nickel-based superalloys is carefully designed to withstand the stresses imposed on the components. Protective coatings are often applied to components to protect them from the environmental impact of hot, corrosive combustion gases.

[0006] A widely used protective coating is an aluminum-containing coating known as a diffusion aluminide coating. The diffusion process generally requires that the surface of the component react with an aluminum-containing gas component to form two distinct regions, the outermost of which is an additive layer containing an environmentally resistant intermetallic compound represented by MAl, where M is iron, nickel, or cobalt, depending on the substrate. MAl intermetallic compounds are the result of aluminum deposition and diffusion of iron, nickel, and / or cobalt from the substrate. During high temperature exposure in air, MAl intermetallic compounds form a protective aluminum oxide (alumina) scale or oxide layer, thereby inhibiting oxidation of the diffusion coating and the underlying substrate. The chemical properties of the additive layer can be altered by the presence of additional elements (e.g., platinum, chromium, silicon, rhodium, hafnium, yttrium, and zirconium) in the aluminum-containing composition. Diffusion aluminide coatings containing platinum, known as platinum aluminide coatings, are particularly widely used for gas turbine engine components.

[0007] The second zone of the diffusion aluminide coating is formed in the surface region of the component below the additive layer. The diffusion zone contains various intermetallic and metastable phases that are formed during the coating reaction due to diffusion gradients and changes in element solubility in localized regions of the substrate. The intermetallic compounds in the diffusion zone are the product of various alloying elements of the substrate and the diffusion coating.

[0008] Although significant advances have been made in environmental coating materials and methods of forming such coatings, the need to repair or replace these coatings is unavoidable in certain circumstances. For example, removal may be necessary due to corrosion or thermal degradation of the diffusion coating, refurbishment of the component to which the coating is formed, or in-process repair of the diffusion coating or the thermal barrier coating (if present) adhered to the component by the diffusion coating. The current state-of-the-art repair process is to completely remove the diffusion aluminide coating by combining mechanical and chemical treatments. For example, the diffusion aluminide coating can be removed by sandblasting followed by treatment with an acidic solution that is capable of interacting with and removing the additives and the diffusion layer.

[0009] Removal of the entire aluminide coating including the diffusion zone results in removal of a portion of the substrate surface. For components such as gas turbine engine blades and impeller airfoils, removal of the diffusion zone may result in alloy loss from the substrate surface, and for air-cooled components, removal of the diffusion zone may result in excessively thin walls and drastic changes in airflow characteristics, necessitating the component being scrapped.

[0010] Most current methods for removing diffusion coatings to expose the surface of superalloy components or completely remove the additive layer involve the use of acid stripping, multiple grit blasting, and subsequent heat coloring processes to verify that the aluminide is completely removed from the surface of the superalloy component. Acid stripping uses harsh chemicals such as phosphoric acid, nitric acid, or hydrochloric acid that require special equipment to remove the additive and diffusion layers.

[0011] Therefore, there is a need for an improved method for cleaning, inspecting and rejuvenating coated articles. Summary of the invention

[0012] In one aspect, embodiments of the present disclosure are directed to a method of removing contaminants from a coated superalloy component having a diffusion coating including an additive layer on a surface of the component and a diffusion zone in the surface of the component. The method includes providing a coated superalloy component having one or more contaminants on a surface of the component; and subjecting the surface of the component containing the contaminants to a laser beam pulse to remove the contaminants from the component, such that the one or more contaminants are removed without damaging or removing the diffusion zone of the diffusion coating.

[0013] In another aspect, embodiments of the present disclosure relate to a method for regenerating a coated superalloy component having a surface that has been subjected to high temperature service. The method includes providing a coated superalloy component having a diffusion coating, the diffusion coating including an additive layer on the component surface and a diffusion zone in the component surface; removing one or more contaminants from the component by subjecting the component to laser beam pulses to remove the contaminants from the component, such that the contaminants are removed without damaging or removing the diffusion zone of the diffusion coating, resulting in an exposed portion of the diffusion zone or an exposed portion of the additive layer; optionally, selectively removing at least a portion of the additive layer using laser beam pulses; applying an aluminide coating to the exposed portion of the diffusion zone or the exposed portion of the additive layer; performing a diffusion heat treatment at a preselected high temperature to form a regenerated protective aluminide coating on the superalloy component. Optionally, the method may also include repairing the coated superalloy component prior to applying the aluminide coating thereon. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] The above and other aspects, features and advantages of the present disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings, in which:

[0015] Figure 1 is a perspective view of an assembly used at high temperature according to the present disclosure;

[0016] Figure 2 is a used component according to an exemplary embodiment of the present disclosure along Figure 1 A schematic cross-sectional view in the direction 2-2;

[0017] Figure 3 According to the exemplary embodiment of the present disclosure, after removing the pollutants Figure 2 A schematic diagram of the components;

[0018] Figure 4 According to an exemplary embodiment of the present disclosure, after removing part of the additive layer Figure 2 A schematic diagram of the components;

[0019] Figure 5 is a flow chart of an exemplary method of removing contaminants from a coated superalloy component according to an exemplary embodiment of the present disclosure; and

[0020] Figure 6 is a flow chart of a method of regenerating a coated superalloy component used at high temperature according to an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION

[0021] One or more embodiments of the present disclosure will be described below. Unless otherwise defined, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0022] The terms "a" and "an" do not denote a limitation of quantity, but rather denote the presence of at least one of the referenced item. Approximate language, as used throughout the specification and claims, may be used to modify any quantitative representation that may be permissibly varied without resulting in a change in the basic function to which it is associated. Therefore, a value modified by one or more terms such as "about" is not limited to the precise value specified. In addition, when the expression "first value - second value" is used, it is intended to modify both values. At least in some cases, the approximate language may correspond to the precision of the instrument used to measure the value.

[0023] Here, in the entire specification and claims, range limits can be combined and / or interchanged, unless the context or language indicates otherwise, such ranges are determined and include all sub-ranges contained therein. Any numerical value cited herein includes all values ​​from a lower value to a higher value in increments of one unit, provided that there is an interval of at least 2 units between any lower value and any higher value. As an example, if the value of the amount of the component or the process variable (such as temperature, pressure, time, etc.) is, for example, from 1 to 90, it is intended that 15 to 85, 22 to 68, 43 to 51, 30 to 32, etc. are clearly listed in this specification. For values ​​less than 1, one unit is considered to be 0.0001, 0.001, 0.01 or 0.1 (as the case may be). These are only examples of specific intent, and all possible numerical combinations between the lowest and highest values ​​listed will be considered to be clearly stated in a similar manner in this application.

[0024] The methods of the present disclosure may include, consist essentially of, or consist of the components of the present disclosure as well as other materials described herein. As used herein, "consisting essentially of" means that the composition or component may include additional materials, but only if the additional materials do not materially change the basic and novel characteristics of the claimed composition or method.

[0025] The present disclosure provides a method for removing contaminants from an article having a diffusion coating thereon. In addition, a method for regenerating a coated superalloy component that has been used at high temperatures is provided. The present disclosure is generally applicable to components that are protected from thermal and chemical adverse environmental effects by diffusion coatings (e.g., diffusion aluminide coatings or diffusion chromide coatings). Notable examples of such components include high-pressure and low-pressure turbine nozzles, blades, shrouds, combustor liners, and enhancer hardware of gas turbine engines. Although the advantages of the present disclosure are particularly applicable to gas turbine engine components, the teachings of the present disclosure are generally applicable to any component on which a diffusion coating can be used to protect the component from its environment.

[0026] One advantage of the embodiments of the present disclosure includes reducing the time and labor used to re-coat or regenerate superalloy components after use in a turbine. Another advantage of the embodiments of the present disclosure is reducing the cost of re-coating and regenerating components after use in a turbine. Another advantage of the embodiments of the present disclosure is that the regenerated coating on the superalloy component has a chemical composition that is substantially the same as the original manufactured superalloy component having a protective aluminide coating before any use in the turbine. Another advantage of the embodiments of the present disclosure is that the coating microstructure and chemical properties of the regenerated coating meet the technical requirements. Another advantage of the embodiments of the present disclosure is that the method and the regenerated coating maintain the size and airflow requirements and increase the yield of the repair hardware. Another advantage of the embodiments of the present disclosure is that the method consumes less wall thickness than a full stripping repair using acid.

[0027] Figure 1 A coated superalloy component 10 is depicted after use in a turbine, which may be used in the method of the present disclosure, and in this illustration is an airfoil 11. As shown, cooling holes 18 are present in the airfoil 11 through which bleed air is forced to transfer heat from the airfoil 11. Particularly suitable materials for the component 10 include nickel-based superalloys, although it is contemplated that other materials may be used. Although described as an airfoil 11, the component 10 includes, but is not limited to, high pressure and low pressure gas turbine blades, impellers or nozzles, stators, and shrouds. As shown in FIG. Figure 1 As shown, component 10 may have contaminants 12 thereon after a useful life of 12,000 to 24,000 hours at temperatures exceeding 800°C (1500°F).

[0028] The contaminants 12 may include any hot corrosion products, dirt, dust, oxides, and combinations thereof. For example, hot corrosion of gas turbine engine components typically occurs when sulfur and sodium react to form sodium sulfate (Na2SO4) during combustion, which condenses and subsequently corrodes the surface of the component. The sources of sulfur and sodium for hot corrosion reactions include impurities in the fuel being burned and the inhalation of sodium-containing dust and / or the inhalation of sea salt. In the latter case, hot corrosion typically occurs on hot section turbine blades and impellers under conditions where salt is deposited on the surface of the component in solid or liquid form. Salt deposits can damage the aluminum oxide scale on the aluminide coating, causing rapid corrosion of the coating. Hot corrosion produces a loosely adhered outer scale, and various internal oxides and sulfides penetrate beneath the outer scale. These products are typically compounds of sulfur and sodium, elements present in the alloy, and other elements that may come from the environment, such as calcium, magnesium, chlorine, etc. Therefore, hot corrosion products can be distinguished from oxides that are typically formed or deposited on gas turbine engine components due to exposure to an oxidizing environment. The terms "a contaminant" and "contaminant" are used interchangeably herein to refer to any contaminant in any form that is present on the diffusion coating after the component has been used (ie, in operational use) and is removed prior to further use of the component.

[0029] Figure 2 After 12,000 to 24,000 hours of use in the turbine Figure 1 1 is a cross-sectional view of a coated superalloy component 10. The coated superalloy component 10 includes a diffusion coating 20 on a superalloy substrate 70. The diffusion coating 20 includes an additive layer 50 formed on the superalloy substrate 70 and a diffusion zone 60 formed in the surface of the superalloy substrate 70. In one embodiment, the diffusion coating 20 also includes an oxide layer 40 formed on the additive layer 50 by exposure to an oxidizing environment.

[0030] Further Figure 2As shown, the typical thickness 22 of the diffusion coating 20 is 38 microns (1.5 milli-inches or mils) to 102 microns (4.0 mils), or 45 microns to 90 microns, or 50 microns to 80 microns. The thickness 22 of the diffusion coating 20 includes the thickness of the oxide layer 40, the thickness of the additive layer 50, and the thickness of the diffusion zone 60. The oxide layer 40 is typically very thin and is 5 microns to 10 microns, or 6 microns to 9 microns, or alternatively 7 microns to 8 microns. For some diffusion coatings 20, the oxide layer 40 may not be present. The additive layer 50 is located between the oxide layer 40 and the diffusion zone 60. The thickness 54 of the additive layer 50 is typically 12.7 microns (0.5 mils) to 63.5 microns (2.5 mils), or 17.8 microns (0.7 mils) to 50.8 microns (2.0 mils), or 22.9 microns (0.9 mils) to 43.1 microns (1.7 mils). The additive layer 50 comprises an environmentally resistant intermetallic phase MA1, where M is iron, nickel or cobalt, depending on the substrate material (primarily β(NiAl) if the substrate is nickel-based). A diffusion zone 60 is formed on and in a portion of the substrate between the additive layer 50 and the bulk superalloy substrate 70 of the coated superalloy component 10. The thickness of the diffusion zone 60 typically varies from 7.6 microns (0.3 mils) to 17.8 microns (0.7 mils) thick, or 8 microns to 16 microns, or 9 microns to 15 microns. The superalloy substrate 70 typically includes nickel-based, iron-based, and cobalt-based superalloys, but other superalloys are possible. The diffusion coating 20 may include, for example, an aluminide diffusion coating or a chromide diffusion coating.

[0031] Further Figure 2 As shown, contaminants 12 are present on the surface of the component. For example, contaminants such as thermal corrosion products, dirt, dust, or oxides may be present on the oxide layer 40, within the oxide layer 40, or within the additive layer 50. Contaminants 12 may be selectively removed from the coated superalloy component 10 by exposure to laser beam pulses. For example, Figure 3 As shown, the contaminant 12 has been removed from the substrate 70. The removal of the contaminant 12 may also remove portions of the oxide layer 40 and the additive layer 50, depending on the location of the contaminant 12 within the structure. The removal of the contaminant 12 may create an exposed portion 61 of the diffusion zone 60 or an exposed portion 56 of the additive layer 50. The laser beam pulses used in the current method allow for visual inspection and removal of contaminants from the diffusion coating 20. The laser beam pulses used to remove the contaminant 12 remove little or no diffusion zone 60, nor any portion of the underlying superalloy substrate 70.

[0032] Subjecting the surface of the component to laser beam pulses includes directing a pulsed laser beam to the surface of the component, wherein each pulse of the laser has sufficient energy to melt or evaporate a portion of the contaminant or coating. Various operating parameters of pulsed lasers will be further discussed herein, wherein "pulsed laser" refers to a laser that emits a pulsed laser beam. In addition, pulsed lasers can produce heat-affected zones, and various parameters can be changed or modified to control the size of the heat-affected zones, thereby reducing unwanted thermal effects and microcracks. The pulsed laser beam and controlled laser parameters as provided herein allow for the selective removal of contaminants 12 and / or additive layers 50 from the component 10. For example, highly selective, controlled removal of portions of the contaminants 12 is possible. In addition, by means of a pulsed laser beam, the contaminants 12 can be removed without damaging the underlying diffusion zone 60 of the coating.

[0033] like Figure 4 As shown, the oxide layer 40 of the diffusion coating 20 and a portion 52 of the additive layer 50 may also be selectively removed from the coated superalloy component 10 by the laser beam pulses. Removing the portion 52 of the additive layer 50 creates an exposed portion 56 of the additive layer 50. Figure 4 5. Although not described herein, removing a portion 52 may also produce an exposed portion of the diffusion region 60 in addition to the exposed portion 56 of the additive layer 50 (e.g., Figure 3 The exposed portion 61 described in Figure 4 As described in the foregoing, the portion 52 removed may include the entire additive layer 50, or substantially all of the additive layer 50, leaving the diffusion zone 60 substantially or completely exposed. The portion 52 of the additive layer 50 removed accounts for 25% to 100%, or 25% to 80%, or 30% to 50% of the thickness 54 of the additive layer 50. In addition, the thickness removed may vary at locations along the surface. A pulsed laser capable of generating laser beam pulses is used to remove a portion of the additive layer 50. The pulsed laser parameters make it possible to selectively remove a portion of the additive layer 50 or the entirety of the additive layer 50. The laser beam pulses used in the current method allow for visual inspection of the removal of a portion 52 of the additive layer 50. The laser beam pulses used to remove the additive layer 50 remove little or no diffusion zone 60, and do not remove any portion below the superalloy substrate 70.

[0034] Figure 5 is described for use in coating superalloy components 10 (see Figure 3) is a flow chart of a method 300 for removing contaminants from a diffusion coating 20 of a coated superalloy component 10. The contaminants present on the coated superalloy component 10 are a result of use in a turbine. The diffusion coating 20 includes an optional oxide layer 40, an additive layer 50, and a diffusion zone 60 on a superalloy substrate 70 of the coated superalloy component 10. At 302, the method 300 includes selectively removing the contaminant 12 by subjecting the component to laser beam pulses. Optionally, at 304, a portion of the oxide layer 40 and a portion of the additive layer 50 may also be removed by subjecting the component to laser beam pulses. The method 300 may also optionally include inspecting the component 10 for continued presence of contaminants at 306. At 308, the removal of contaminants (302), the optional removal of the oxide layer and the additive layer 50 (304), and the inspection (306) may be repeated, alternating between removal and inspection until all contaminants are removed. In other embodiments, the component is subjected to continuous, uninterrupted laser beam pulses at 302 until the removal of the contaminants is complete. The inspection may be omitted or performed simultaneously. Inspection may be visual or by other than visual means.

[0035] Various operating parameters of the pulsed laser are provided to allow for selective removal of contaminants 12 from the component 10. For example, the frequency of the pulsed laser can be from 10 kHz to 250 kHz, such as from 25 to 200, such as from 50 to 150. In an embodiment, the frequency of the pulsed laser can be 20 kHz. The energy per pulse of the laser beam pulse can be equal to or less than 1 millijoule (mJ). The pulse length of each pulse is typically from 10 to 500 nanoseconds, such as from 20 to 100 nanoseconds. The laser beam pulse provides a laser spot beam with a diameter of 75 μm to 95 μm, such as 85 μm. The energy density of the laser beam pulse is between 17,000 mJ / cm 2 Up to 18,00mJ / cm 2 Range, for example 17,200mJ / cm 2 Up to 17,800mJ / cm 2 , for example 17,600mJ / cm 2 Up to 17,700mJ / cm 2. The output power of the pulsed laser used to deliver the laser beam pulses can be 50W to 1000W, for example 100W. The method can be performed with any suitable pulsed laser, including an Nd:YAG laser. The parameters provided are such that the diffusion zone 60 is hardly removed or not removed. In addition, the parameters provided effectively remove the contaminant 12 without removing any portion below the superalloy substrate 70. In addition, the parameters provided can be used to remove a portion of the oxide layer 40 and the additive layer 50 from the component 10. In one embodiment, various parameters can be pre-selected based on the type, degree, and location of the contaminant to achieve the target result. In addition, various parameters can be controlled during the implementation of the method to affect the results, such as by adjusting one or more of the parameters to increase or decrease the parameter value. For example, adjustments can be made to reduce the heat affected zone, increase or decrease the material removal rate, or increase or decrease the diameter or pulse length of the laser spot beam.

[0036] Prior to selectively removing the contaminants (302), the coated superalloy component 10 may be degreased or hot water washed to remove any residual oil and grease from the surface of the coated superalloy component 10. Optionally, prior to selectively removing the contaminants 12, the component 10 may be subjected to an aqueous cleaning process. Once the contaminants 12 have been removed, the component 10 itself or the diffusion coating may be repaired. For example, once the contaminants 12 have been removed, the component 10 may be repaired as needed. For example, repairing the coated superalloy component 10 includes, but is not limited to, spot welding, MIG welding, TIG welding, and brazing. In addition, a diffusion coating may be applied to an area where the contaminants 12 have been removed to provide a regenerated coated component. In an embodiment, the method 300 is applicable to a coated superalloy component 10 from which at least a portion of the aluminide coating needs to be removed. The coated superalloy component 10 includes, for example, but is not limited to, blades, impellers, nozzles, stators, shrouds, buckets, and combinations thereof.

[0037] Figure 6Flowchart describing method 500 for regenerating coated superalloy component 10 after coated superalloy component 10 is used at high temperature above about 800°C. As used herein, regenerated coating refers to forming a new coating, including the remaining portion of the existing diffusion coating and the newly applied vapor deposited or gel aluminide coating, wherein the new regenerated coating has the same microstructure and chemical composition as the OEM diffusion coating before use, which means that the microstructure and chemical composition are substantially similar to the same. Contamination present on (or within) the diffusion coating of superalloy component 10 is caused by use in a turbine. Diffusion coating 20 includes an optional oxide layer 40, an additive layer 50, and a diffusion zone 60 on a superalloy substrate 70 of coated superalloy component 10. At 502, method 500 includes removing contaminants 12 from superalloy component 10 using laser beam pulses. Removal of contaminants produces exposed portions 61 of diffusion zone 60 and / or exposed portions 56 of additive layer 50.

[0038] Various operating parameters of the pulsed laser are provided to allow for selective removal of contaminants 12 from the component 10. For example, the frequency of the pulsed laser can be from 10 kHz to 250 kHz, such as from 25 to 200, such as from 50 to 150. In an embodiment, the frequency of the pulsed laser can be 20 kHz. The energy per pulse of the laser beam pulse can be equal to or less than 1 millijoule (mJ). The pulse length of each pulse is typically from 10 to 500 nanoseconds, such as from 20 to 100 nanoseconds. The laser beam pulse provides a laser spot beam with a diameter of 75 μm to 95 μm, such as 85 μm. The energy density of the laser beam pulse is between 17,000 mJ / cm 2 Up to 18,00mJ / cm 2 Range, for example 17,200mJ / cm 2 Up to 17,800mJ / cm 2 , for example 17,600mJ / cm 2 Up to 17,700mJ / cm 2. The output power of the pulsed laser used to deliver the laser beam pulses can be 50W to 1000W, such as 100W. The method can be performed with any suitable pulsed laser, including Nd:YAG lasers. In one embodiment, the various pulsed laser beam parameters described above are controlled to produce the desired results. In one embodiment, the parameters are controlled to achieve the target results by preselecting the parameters based on the type, degree and location of the contaminants. In addition, various parameters can be controlled during the implementation of the method to affect the results, such as by adjusting one or more of the parameters to increase or decrease the parameter value. For example, adjustments can be made to reduce the heat affected zone, increase or decrease the material removal rate, or increase or decrease the diameter or pulse length of the laser spot beam. Adjustments can be made during the laser beam pulse (i.e., in operation) or between laser beam pulse repetitions (i.e., after inspection and before repeating the laser beam pulse).

[0039] At 503, optionally, method 500 includes selectively removing oxide layer 40 (if present) and a portion 52 of additive layer 50 by further subjecting the assembly to laser beam pulses. Removing oxide layer 40 and a portion 52 of additive layer 50 results in an exposed portion 56 of additive layer 50. Removing the entire thickness of additive layer 50 anywhere on the surface results in an exposed portion 61 of diffusion zone 60. Removing portion 52 of additive layer 50 may include removing 25% to 100% of the thickness 54 of additive layer 50. Exposure to laser beam pulses of the present method removes little or no diffusion zone 60, and does not remove any portion of the underlying superalloy substrate 70. Visual inspection may be used to determine whether the desired portion of additive layer 50 has been removed. Diffusion zone 60 is typically a brighter gray metal than additive layer 50, which has more of a matte or dull gray metal finish, such that the remaining thickness of additive layer 50 may be seen without the use of special tools. Inspection methods other than visual inspection may also be used. If desired, subjecting the component to laser beam pulses (502 and 503) and inspecting the component (e.g., Figure 5 The laser beam pulse parameters may be adjusted between the repeated steps as described above.

[0040] At 505, method 500 includes applying an aluminide coating to exposed portion 61 and / or exposed portion 56. The aluminide coating may be applied by any suitable process, such as a vapor deposition or gel aluminide coating process.

[0041] At 507, method 500 includes performing a heat treatment at a preselected elevated temperature to form a regenerated protective aluminide coating on superalloy component 10. Heat treatment includes using a furnace or other heat source to increase the temperature of superalloy component 10 to open the metal of substrate 70, thereby allowing material from diffusion zone 60 to flow into substrate 70 and bond with the substrate to form a regenerated aluminide protective coating. The regenerated protective aluminide coating has a coating microstructure and coating chemistry that matches the original diffusion coating of the new superalloy component prior to use in the turbine, meaning the microstructure and chemistry are substantially similar to the same.

[0042] Prior to removing the contaminants (502), the coated superalloy component 10 may optionally be degreased or hot water washed to remove any residual oil and grease from the surface of the coated superalloy component 10. Additionally, in some embodiments, the surface of the coated alloy component may be exposed to an aqueous cleaning process. After removing a portion of the contaminants and / or additive layer, an optional additional step is to remove any remaining grit or debris from the component surface by sandblasting or airflow dust removal. After removing a portion of the contaminants and / or additive layer and prior to applying the aluminide coating, another optional additional step is to repair the coated superalloy component. Method 500 is applicable to coated superalloy components 10 that require removal of an aluminide coating, including blades, impellers, nozzles, stators, shrouds, buckets, and combinations thereof.

[0043] Further aspects of the invention are provided by the subject matter of the following clauses:

[0044] A method of removing contaminants from a coated superalloy component having a diffusion coating including an additive layer on a surface of the component and a diffusion zone in the surface of the component, the method comprising: subjecting the surface of the coated superalloy component having contaminants thereon to laser beam pulses to remove the contaminants from the component such that the contaminants are removed without damaging or removing the diffusion zone of the diffusion coating.

[0045] A method according to any of the preceding clauses, wherein the diffusion coating is an aluminide diffusion coating.

[0046] A method according to any of the preceding clauses, wherein the contaminants include one or more of thermal corrosion products, oxides, dirt, dust or combinations thereof.

[0047] A method according to any of the preceding clauses, wherein subjecting the surface of the component to laser beam pulses produces exposed portions of the diffusion region, exposed portions of the additive layer, or both.

[0048] A method according to any of the preceding clauses, further comprising applying a diffusion coating material to an exposed portion of the diffusion zone or an exposed portion of the additive layer to form a regenerated protective diffusion coating on the component.

[0049] A method according to any of the preceding clauses, wherein the regenerated protective diffusion coating has a coating microstructure and coating chemistry that matches an initial diffusion coating of the component prior to use in a turbomachine.

[0050] A method according to any of the preceding clauses, further comprising inspecting the component for the presence of the contaminant, the method comprising alternatingly subjecting the surface to laser beam pulses to remove the contaminant and inspecting the component until all contaminants are removed from the component.

[0051] A method according to any of the preceding clauses, wherein the laser beam pulses have an energy equal to or less than 1 mJ / pulse.

[0052] A method according to any of the preceding clauses, wherein the laser beam pulses have a pulse length of 20 nanoseconds to 100 nanoseconds.

[0053] A method according to any of the preceding clauses, wherein the laser beam pulses provide a laser spot beam having a diameter of 75 μm to 95 μm when impinging on the surface of the component.

[0054] A method according to any of the preceding clauses, wherein the laser beam pulses provide a pulse intensity between 17,600 and 17,700 joules / cm 2 energy density in the range.

[0055] A method according to any of the preceding clauses, wherein the laser emitting the pulsed laser beam has a frequency of 10 kHz to 250 kHz.

[0056] A method according to any of the preceding clauses, wherein the laser emitting the pulsed laser beam has an output power of 50W to 1000W.

[0057] A method for regenerating a superalloy component that has been used in a turbine at high temperatures, the superalloy component having a diffusion coating, the diffusion coating including an additive layer on the surface of the component and a diffusion zone in the surface of the component, the method comprising: removing contaminants from the component by subjecting the component to laser beam pulses to remove contaminants from the component, so that the contaminants are removed without damaging or removing the diffusion zone of the diffusion coating, resulting in an exposed portion of the diffusion zone or an exposed portion of the additive layer; applying an aluminide coating to the exposed portion of the diffusion zone or the exposed portion of the additive layer; and performing a diffusion heat treatment at a preselected high temperature to form a regenerated protective aluminide coating on the superalloy component.

[0058] A method according to any of the preceding clauses, wherein the regenerated protective aluminide coating has a coating microstructure and coating chemistry that matches that of a diffusion coating prior to use in a turbine.

[0059] A method according to any of the preceding clauses, wherein the diffusion coating is an aluminide coating.

[0060] A method according to any of the preceding clauses, wherein the laser beam pulses have: (i) an energy equal to or less than 1 mJ / pulse, (ii) a pulse length of 20 ns to 100 ns, or (iii) a pulse providing 17,600 to 17,700 J / cm 2 energy density.

[0061] A method according to any of the preceding clauses, further comprising, before applying the aluminide coating, selectively removing at least a portion of the additive layer by additionally subjecting the component to the laser beam pulses.

[0062] A method according to any of the preceding clauses, further comprising: prior to applying the aluminide coating: inspecting the component to determine whether removal of the contaminants and removal of a portion of the additive layer is complete; and alternating subjecting the component to laser beam pulses and inspecting the component until removal is determined to be complete.

[0063] The method of any of the preceding clauses, wherein subjecting the component to the laser beam pulses to remove contaminants and selectively remove at least a portion of the additive layer comprises controlling one or more parameters of the laser beam pulses.

[0064] A method as claimed in any of the preceding clauses, comprising, optionally, removing at least a portion of the additive layer using laser beam pulses.

[0065] A method according to any of the preceding clauses, comprising, optionally, repairing the coated superalloy component.

[0066] This specification uses examples to describe the present disclosure, including the best mode, and also enables any person skilled in the art to practice the present disclosure, including making and using any device or system and performing any combined method. The patent scope of the present disclosure is defined by the claims, and may include other examples that occur to a person skilled in the art. If such other examples have structural elements that do not differ from the literal language of the claims, or if they include equivalent structural elements that do not differ substantially from the literal language of the claims, they are intended to be included within the scope of the claims.

Claims

1. A method of removing contaminants from a coated superalloy component, the coated superalloy component having a diffusion coating, the diffusion coating comprising an additive layer on a surface of the component and a diffusion zone in the surface of the component, the method comprising: A surface of a coated superalloy component having contaminants thereon is subjected to laser beam pulses to remove the contaminants from the component such that the contaminants are removed without damaging or removing the diffusion zone of the diffusion coating, The laser beam pulse has an energy of 1 mJ / pulse or less and a pulse length of 20 nanoseconds to 100 nanoseconds, and the laser beam pulse provides a pulse energy of 17,600 to 17,700 joules / cm 2 energy density in the range.

2. The method according to claim 1, wherein: The diffusion coating is an aluminide diffusion coating.

3. The method according to claim 1, wherein: The contaminants include one or more of thermal corrosion products, dirt, or a combination thereof.

4. The method according to claim 1, wherein: The contaminants include one or more of oxides, dust, or a combination thereof.

5. The method according to claim 1, wherein: The surface of the component is subjected to laser beam pulses, resulting in exposed portions of the diffusion region, exposed portions of the additive layer, or both.

6. The method according to claim 5, wherein: The method also includes applying a diffusion coating material to the exposed portion of the diffusion zone or the exposed portion of the additive layer to form a regenerated protective diffusion coating on the component.

7. The method according to claim 6, wherein: The regenerated protective diffusion coating has a coating microstructure and coating chemistry that matches the initial diffusion coating of the component prior to use in a turbine.

8. The method according to claim 1, wherein: The method further includes inspecting the component for the presence of the contaminant, the method comprising alternating subjecting the surface to laser beam pulses to remove the contaminant and inspecting the component until all contaminants are removed from the component.

9. The method according to claim 1, wherein: The laser beam pulse provides a laser spot beam having a diameter of 75 μm to 95 μm when impinging on the surface of the component.

10. The method according to claim 1, wherein: The laser emitting the pulse laser beam has a frequency of 10 kHz to 250 kHz.

11. The method according to claim 1, wherein: The laser emitting the pulse laser beam has an output power of 50W to 1000W.

12. A method of regenerating a superalloy component that has been used in a turbine at high temperatures, the superalloy component having a diffusion coating comprising an additive layer on a surface of the component and a diffusion zone in the surface of the component, the method comprising: removing contaminants from the component by subjecting the component to laser beam pulses to remove the contaminants from the component such that the contaminants are removed without damaging or removing the diffusion zone of the diffusion coating, resulting in an exposed portion of the diffusion zone or an exposed portion of the additive layer; applying an aluminide coating to the exposed portion of the diffusion zone or to the exposed portion of the additive layer; as well as Diffusion heat treatment at a preselected high temperature forms a regenerated protective aluminide coating on the superalloy component. The laser beam pulse has: (i) an energy equal to or less than 1 mJ / pulse, (ii) a pulse length of 20 nanoseconds to 100 nanoseconds, or (iii) a pulse providing 17,600 to 17,700 joules / cm 2 energy density.

13. The method according to claim 12, wherein: The regenerated protective aluminide coating has a coating microstructure and coating chemistry that matches the diffusion coating prior to use in the turbine.

14. The method according to claim 12, wherein: The diffusion coating is an aluminide coating.

15. The method according to claim 12, wherein: The method further comprises, prior to applying the aluminide coating, selectively removing at least a portion of the additive layer by additionally subjecting the component to the laser beam pulses.

16. The method according to claim 15, wherein: The method further comprises, before applying the aluminide coating: inspecting the assembly to determine whether removal of the contaminant and removal of a portion of the additive layer is complete; and Alternately subjecting the component to laser beam pulses and inspecting the component until removal is determined to be complete.

17. The method according to claim 15, wherein: Subjecting the component to the laser beam pulses to remove contaminants and selectively remove at least a portion of the additive layer includes controlling one or more parameters of the laser beam pulses.

Citation Information

Patent Citations

  • A method for removing a coating and a method for rejuvenating a coated superalloy component

    CN103382544A

  • Method for cleaning and stripping a turboshaft engine blade using a pulsed laser

    US20140082939A1