Pure flax grey cloth interwoven with dry-spun and wet-spun flax yarns and preparation method thereof
Through the interweaving and low-temperature sizing technology of dry spinning and wet spinning linen yarns, the tension relaxation caused by low efficiency and high-temperature sizing of linen spinning is solved, and the efficient and low-cost spinning process and excellent fabrics are achieved. performance.
Patent Information
- Application Number
- CN202210859729.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-07-21
AI Technical Summary
In the prior art, the wet spinning process of linen spinning is low efficiency and high cost, and high temperature sizing causes yarn tension to relax, affecting fabric performance.
The method of interweaving dry spun and wet spun linen yarn is used, dry spun linen yarn is used as warp yarn, wet spun linen yarn is used as weft yarn, and sizing is carried out through a low-temperature sizing process (slurry temperature is below 65℃), and oxidized phosphate potatoes are used. Starch acts as a slurry and controls the slurry temperature and speed to reduce tension and improves the strength and wear resistance of the yarn.
It realizes efficient simplification of the spinning process, reduces production costs and energy consumption, maintains the unique style and performance of linen fabrics, improves the strength and wear resistance of the yarn, and avoids tension relaxation problems caused by high-temperature slurry.
Smart Images

Figure BDA0003757796480000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textiles, and particularly relates to a pure flax grey cloth interwoven with dry-spun and wet-spun flax yarns and a preparation method thereof. Background Art
[0002] Flax is one of the earliest natural fibers used by humans. Its single fiber length is about 20mm and its fineness is 3000-5000 metric denier. It is coarser than cotton but finer than other bast fibers. It has high fiber strength, fast moisture absorption and dissipation, and good spinnability. The fabric woven from it has excellent moisture absorption and release properties, is breathable and smooth, crisp and comfortable, and has natural antibacterial effects. It is an excellent raw material for summer clothing, home textile products, etc.
[0003] Traditional flax spinning generally adopts wet spinning technology, referred to as "wet spinning". The main process includes softening, combing, drawing, roving, boiling and bleaching, wet spinning, drying, etc., gradually removing impurities such as colloid in the fiber. However, because the length of flax single fiber is short, a semi-degumming process is generally adopted, that is, a part of the colloid is retained during boiling and bleaching, so that each fiber adheres to each other into a bundle of fibers with a longer length for wet spinning. The flax yarn spun by wet spinning technology has a smooth surface, less hairiness, and a soft luster, but the flax yarn is coarse, the yarn is poor, the strength is uneven, and the woven fabric is stiff, with a unique texture of roughness and unevenness. On the other hand, the wet spinning process is long and inefficient, and the working environment of the wet spinning workshop is poor, and water and energy consumption is also high.
[0004] Compared with flax spinning, the equipment and technology of cotton ring spinning system are more advanced and mature, the production speed is much higher than flax wet spinning, and the yarn uniformity is significantly better than wet spinning. Therefore, using cotton spinning system to dry-spin flax yarn can not only simplify the spinning process, improve production and efficiency, but also improve the yarn performance. At the same time, the system can also effectively use the fallen flax in wet spinning for spinning, which can greatly reduce costs and energy consumption, and make full use of flax raw materials. However, compared with wet spinning, dry-spun flax yarn has shorter fiber length, looser structure, poor fiber cohesion, more surface hairiness and poor gloss. After being woven into fabric, it does not have the fabric style of flax wet spinning, which to a certain extent weakens the unique style of flax fabric that is generally accepted and loved by the public. The master's thesis "Research on wet-spun intertwined composite yarn and fabric properties of flax" uses the spinning method of intertwining flax yarn with wool or nylon to optimize the yarn performance, thereby reducing the itching of the fabric, but the air permeability of the intertwined composite yarn fabric (23.48mL / cm 2 ·s) is much lower than pure linen fabric (30.55mL / cm 2·s). The invention patent with application number CN200910072124.X - a method for sizing the warp yarn of pure flax grey cloth with high count and high density, uses starch slurry to size the warp yarn of pure flax grey cloth, solving the problems of low efficiency and excessive triple jump defects caused by strip weaving. However, the sizing temperature is 95-100℃, which consumes a lot of energy, and the sizing tank temperature is 70-80℃ during sizing, which easily causes the flax yarn to degummed and cause tension relaxation. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a pure linen grey cloth interlaced with dry-spun and wet-spun linen yarns and a preparation method thereof, and to solve the problem that the sizing temperature of the pure linen fabric is high, thereby causing tension relaxation.
[0006] The present invention provides a method for preparing a pure flax grey cloth interwoven with dry-spun and wet-spun flax yarns, comprising:
[0007] The dry-spun flax yarn is used as the warp yarn and the wet-spun flax yarn is used as the weft yarn. After warping and sizing processes, the pure flax grey cloth is woven, wherein the temperature of the sizing process is below 65°C.
[0008] Preferably, the wet-spun linen yarn used for the weft yarn has a yarn count of 24-48 and a twist coefficient of 240-320, which is 10-20% lower than the twist coefficient of conventional wet-spun linen yarn, so as to make the cloth softer, more beautiful and soft in luster.
[0009] Preferably, the dry-spun linen yarn used for the warp yarn has a yarn count of 24-40 and a twist coefficient of 500-600, which is 10-20% higher than the twist coefficient of conventional dry-spun linen yarn, so as to improve the strength and stiffness of the yarn and reduce the hairiness, making the performance of the dry-spun yarn closer to that of the wet-spun linen yarn.
[0010] Preferably, the sizing process is warp sizing, and the sizing formula is: 60-110 g / L of oxidized phosphate potato starch, 1.5-2.5 g / L of glycerol, 1.5-2 g / L of emulsifying wax, 0.5-2 g / L of fast penetrant T, and 1-2.5 g / L of antistatic agent.
[0011] Preferably, the preparation method of the potato starch containing oxidized phosphate comprises: reacting potato starch milk, hydrogen peroxide and sodium tripolyphosphate at 40-50° C. for 45-60 min, controlling the pH value to be 4-6, wherein the concentration of the potato starch milk is 40-50%, the amount of hydrogen peroxide is 0.8-2% of the dry weight of the potato starch, and the amount of sodium tripolyphosphate is 10-30% of the dry weight of the potato starch.
[0012] Preferably, the degree of substitution of the oxidized phosphate ester potato starch is 0.2-0.25, and the gelatinization temperature is 50-60° C.; when the solid content of the oxidized phosphate ester potato starch is 6%, the viscosity of the starch slurry is 15-20 mPa.s.
[0013] Preferably, the sizing process controls the slurry temperature to 50-60°C (to prevent temperature dissipation during sizing, the slurry tank temperature is determined to be 55-65°C, and the slurry temperature is made to be 50-60°C), the sizing speed is 25-40m / min, so that the sizing rate is 5-8%.
[0014] Preferably, in the sizing process, after the sizing yarn is skeined, the machine speed is adjusted to 20-40 m / min, the drying drum temperature is 110-130°C, and the moisture regain of the sizing yarn after drying is controlled to be 12%-16%, which is slightly larger than the moisture regain of the original linen yarn to enhance the fatigue strength and abrasion resistance of the warp yarn for subsequent weaving.
[0015] Preferably, the pure linen grey cloth structure comprises a plain weave or a twill weave.
[0016] The present invention also provides pure linen grey cloth prepared by the above preparation method.
[0017] The present invention also provides an application of the pure flax grey cloth prepared by the above-mentioned preparation method in clothing or home textile products.
[0018] The principle of the present invention is as follows:
[0019] The wet-spun linen yarn has a smooth surface, less hairiness, high strength, high rigidity, and a soft luster. The woven fabric is stiff and has a unique texture that is rough and uneven. In the fabric, the warp yarn is usually used as the skeleton of the fabric, giving the fabric strength, rigidity and other properties; the weft yarn is usually on the surface of the fabric, affecting the feel and luster of the fabric. Therefore, the interwoven fabric using dry-spun linen yarn as the warp yarn and wet-spun linen yarn as the weft yarn can show the same style as the fabric in which both the warp and weft yarns are pure linen wet-spun yarns in appearance. The present invention uses the linen dry-spun yarn produced on the cotton spinning equipment as the warp yarn. Since the linen (short fiber) produced in the wet spinning of the long linen is used for spinning, the linen raw material is fully utilized, and the advanced cotton spinning equipment platform can be used to realize the efficient short-process spinning of the linen yarn, and produce the linen short fiber dry-spun yarn with more uniform strips. At the same time, during spinning, the twist is increased by 10-20% compared with the conventional linen short-spun dry-spun yarn; and the weft yarn uses the wet-spun linen yarn, and its twist coefficient can be 10-20% lower than that of the conventional wet-spun linen yarn. The twist of flax staple dry-spun yarn is large in order to further improve the strength and stiffness of the yarn and reduce the hairiness, making its style and performance closer to flax wet-spun yarn, and suitable for the requirements of high warp strength, low hairiness and wear resistance; the twist of wet-spun yarn is small because the small twist can make the yarn softer, better gloss, and higher output during spinning. Since wet-spun yarn is used as the weft yarn exposed on the surface of the fabric, its strength requirement is not high, so its yarn twist can be completely reduced.
[0020] Since the flax fiber is only semi-degummed during spinning, the yarn still contains a lot of colloids, which are easily dissolved in the high-temperature slurry, making the fiber loose, reducing the sizing tension, causing the yarn to sag, and the yarn is easily entangled and broken when passing through the guide rollers, which deteriorates the sizing effect and affects the smooth sizing (the sizing breakage rate increases and the good axis rate decreases). To prevent the fiber from loosening, low-temperature sizing (below 65°C) is required. When the fiber and the slurry have polar groups with the same structure, the affinity between them is very large, and the slurry has good adhesion to the fiber. After the slurry is adsorbed on the surface of the yarn and dried, it forms a smooth and tough film, which makes the surface hairiness fit, reduces the friction coefficient, and improves the wear resistance. Starch is a natural polymer with glucose as the structural unit, and flax belongs to cellulose fiber. Both contain a large number of hydroxyl groups, so potato starch is selected as the main adhesive of the slurry. Under the action of the oxidant, the hydroxymethyl part on the glucose unit is oxidized to carboxyl, and the phosphate esterification makes part of the hydroxyl group of the starch combine with the acyl group of phosphoric acid. Oxidation and phosphation reduce the number of hydroxymethyl groups in starch molecules, hindering molecular association, that is, weakening the ability of hydrogen bonds between molecules; partially breaking the glycosidic bonds between the base rings of starch molecules, reducing the degree of polymerization, thereby reducing the gelatinization temperature of starch, making it possible to carry out low-temperature sizing. At the same time, acidic conditions will partially hydrolyze starch, greatly reducing the hardness, brittleness and roughness of the size film, making the size film soft and elastic, improving the fluidity of the size, and having good permeability to high-twist flax yarns, and flattening the hairiness.
[0021] Beneficial Effects
[0022] The present invention uses dry-spun linen yarn as warp yarn and wet-spun linen yarn as weft yarn. The twist coefficient of dry-spun linen yarn is 10-20% higher than that of conventional dry-spun linen yarn, so that it has the characteristics of high strength and high rigidity similar to wet-spun linen yarn, and can reduce the hairiness of the yarn; the twist coefficient of wet-spun linen yarn is 10-20% lower than that of conventional wet-spun linen yarn, which can not only give the cloth surface good softness and glossiness, but also increase the spinning output. The present invention combines the advantages of wet spinning and dry spinning technologies, and on the basis of retaining the unique style and natural simple texture of linen, as well as the air permeability, moisture permeability, good hand feel, good comfort, mildew and antibacterial properties, effectively shortens the process flow of (warp yarn) spinning, reduces production costs and energy consumption, takes into account the appearance, performance and cost of the fabric, and makes full use of flax noil to meet the market demand for pure flax fabrics of various specifications, which is conducive to the low-carbon and sustainable development of flax textiles.
[0023] In the sizing process of the present invention, oxidized phosphate ester potato starch is used as the main adhesive for warp sizing, and the sizing temperature is low, which avoids the problem that the high-temperature sizing causes the linen yarn to relax due to degumming, resulting in an increase in the breakage rate of the sizing yarn and a decrease in the good axis rate. The modified oxidized phosphate ester potato starch slurry has good fluidity and has good wettability for high-twist dry-spun linen yarn.
[0024] The surface density of the fabric of the present invention is 150-200g / m 2 The warp breaking strength is 398-433N, the weft breaking strength is 370-419N, the wear resistance is 10000-12000 times, the air permeability value is 845-1090mm / s, and the wrinkle recovery level is level 3. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0026] The breaking strength test method is in accordance with GB / T 3923.1-1997 Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break Strip method.
[0027] The abrasion resistance test method is in accordance with GB / T 21196.2-2007 Textiles - Determination of abrasion resistance of fabrics by the Martindale method - Part 2: Determination of specimen damage.
[0028] The air permeability test method is in accordance with GB / T 5453-1997 Determination of air permeability of textile fabrics.
[0029] The wrinkle recovery grade test method is carried out in accordance with GB / T 29257-2012 Appearance method for evaluating the wrinkle recovery of textile fabrics.
[0030] The good yarn spindle rate is the ratio of the number of spindles without yarn defects to the total number of spindles investigated: good yarn spindle rate = total number of good yarn spindles × 100% / total number of spindles inspected.
[0031] The yarn breakage rate is the number of yarn breaks per unit of sizing equipment per unit time.
[0032] Example 1
[0033] A method for preparing pure flax grey fabric interwoven with dry-spun and wet-spun flax yarns, wherein the plain weave grey fabric is used for preparing clothing, and the specific process flow is as follows:
[0034] Wet-spun linen yarn with a yarn count of 24 and a twist coefficient of 240 is used as the weft yarn, and dry-spun linen yarn with a yarn count of 20 and a twist coefficient of 500 is used as the warp yarn. After warping, the yarn is sized using low-temperature sizing technology. The sizing formula is: 60 kg of oxidized phosphate ester potato starch, 1.5 kg of glycerol, 2 kg of emulsifying wax, 1 kg of fast penetrant T, and 1.5 kg of antistatic agent in 1000 liters of slurry. The preparation process of oxidized phosphate ester potato starch is: potato starch milk concentration 40%, hydrogen peroxide dosage is 0.8% of starch dry weight, sodium tripolyphosphate dosage is 10% of starch dry weight, 50°C reaction for 60 minutes, and the pH value is controlled to be 6. The obtained oxidized phosphate ester potato starch has a substitution degree of 0.2, a gelatinization temperature of 60°C, and a viscosity of the starch slurry of 20 mPa.S when the solid content is 6%. To prevent temperature dissipation during sizing, the sizing tank temperature is set at 65°C, the sizing liquid temperature is set at 60°C, the sizing speed is set at 25m / min, and the sizing rate is controlled at 8%. After the sizing is skeined, the speed is adjusted to 20m / min, the drying drum temperature is 110°C, and the moisture regain of the sizing after drying is controlled to be 12%, which is slightly larger than the moisture regain of the original linen yarn to enhance the fatigue strength and wear resistance of the warp yarn for subsequent weaving. The organizational structure is plain weave, and the surface density of the pure linen woven grey cloth is 200g / m 2 The warp breaking strength is 433N, the weft breaking strength is 419N, the wear resistance is 12000 times, the air permeability value is 845mm / s, and the wrinkle recovery level is level 3.
[0035] Example 2
[0036] A method for preparing pure linen grey fabric interwoven with dry-spun and wet-spun linen yarns, weaving twill and plain weave grey fabric for preparing clothing, the specific process flow is as follows:
[0037] Wet-spun linen yarn with a yarn count of 36 and a twist coefficient of 280 is used as the weft yarn, and dry-spun linen yarn with a yarn count of 30 and a twist coefficient of 550 is used as the warp yarn. After warping, the yarn is sized using low-temperature sizing technology. The sizing formula is: 60kg of oxidized phosphate ester potato starch, 1.5kg of glycerol, 2kg of emulsifying wax, 1kg of fast penetrant T, and 1.5kg of antistatic agent in 1000 liters of slurry. The preparation process of oxidized phosphate ester potato starch is: potato starch milk concentration 45%, hydrogen peroxide dosage is 1.5% of starch dry weight, sodium tripolyphosphate dosage is 20% of starch dry weight, 45℃ reaction for 55min, and pH value is controlled to be 5. The obtained oxidized phosphate ester potato starch has a substitution degree of 0.23, a gelatinization temperature of 55℃, and a viscosity of the starch slurry of 17mPa.S when the solid content is 6%. To prevent temperature dissipation during sizing, the sizing tank temperature is set at 60°C, the sizing liquid temperature is set at 55°C, the sizing speed is set at 32m / min, and the sizing rate is controlled at 6%. After the sizing is skeined, the speed is adjusted to 30m / min, the drying drum temperature is 120°C, and the moisture regain of the sizing after drying is controlled to be 14%, which is slightly larger than the moisture regain of the original linen yarn to enhance the fatigue strength and wear resistance of the warp yarn for subsequent weaving. The organizational structure is twill organization, and the surface density of the pure linen woven grey cloth is 170g / m 2 The warp breaking strength is 410N, the weft breaking strength is 390N, the wear resistance is 11000 times / mg, the air permeability value is 930mm / s, and the wrinkle recovery level is level 3.
[0038] Example 3
[0039] A method for preparing pure linen grey fabric interwoven with dry-spun and wet-spun linen yarns, wherein the woven twill grey fabric is used for preparing bed sheets, and the specific process flow is as follows:
[0040] Wet-spun linen yarn with a yarn count of 48 and a twist coefficient of 320 is used as the weft yarn, and dry-spun linen yarn with a yarn count of 40 and a twist coefficient of 600 is used as the warp yarn. After warping, the yarn is sized using low-temperature sizing technology. The sizing formula is: 60kg of oxidized phosphate ester potato starch, 1.5kg of glycerol, 2kg of emulsifying wax, 1kg of fast penetrant T, and 1.5kg of antistatic agent in 1000 liters of slurry. The preparation process of oxidized phosphate ester potato starch is: potato starch milk concentration 50%, hydrogen peroxide dosage is 2% of starch dry weight, sodium tripolyphosphate dosage is 30% of starch dry weight, 40℃ reaction for 45min, and pH value is controlled to be 4. The obtained oxidized phosphate ester potato starch has a substitution degree of 0.25, a gelatinization temperature of 50℃, and a viscosity of the starch slurry of 15mPa.S when the solid content is 6%. To prevent temperature dissipation during sizing, the sizing tank temperature is set at 55°C, the sizing liquid temperature is set at 50°C, the sizing speed is set at 40m / min, and the sizing rate is controlled at 5%. After the sizing is skeined, the speed is adjusted to 40m / min, the drying drum temperature is 130°C, and the moisture regain of the sizing after drying is controlled to be 16%, which is slightly larger than the moisture regain of the original linen yarn to enhance the fatigue strength and wear resistance of the warp yarn for subsequent weaving. The organizational structure is twill organization, and the surface density of the pure linen woven grey cloth is 150g / m 2 The warp breaking strength is 398N, the weft breaking strength is 370N, the wear resistance is 10,000 times, the air permeability value is 1090mm / s, and the wrinkle recovery level is level 3.
[0041] Comparative Example 1
[0042] The comparison of low-temperature and high-temperature sizing effects (except for the temperature and sizing type, the sizing formula and process are the same as those in Example 3) is shown in Table 1 for the results of the same specification yarn (dry-spun linen yarn, yarn count is 40 public count, twist coefficient is 600).
[0043] Table 1 Comparison of low temperature and high temperature sizing effects
[0044] Slurry type Sizing temperature (℃) <![CDATA[Warp breakage rate (ends·(loom·h) -1 )]]> Good axis rate (%) Potato starch 100 3.73 47 Oxidized phosphate potato starch 60 (Example 3) 0.70 73 Oxidized phosphate potato starch 100 1.65 65
[0045] Comparative Example 2
[0046] The warp and weft wet-spun linen cloth is prepared by using wet-spun linen yarn with a yarn count of 48 and a twist coefficient of 320 as the weft yarn and wet-spun linen yarn with a yarn count of 40 and a twist coefficient of 600 as the warp yarn, using the same process as Example 3. The results are shown in Table 2.
[0047] Table 2 Performance comparison of the present invention and the warp and weft wet-spun linen fabric
[0048]
[0049]
[0050] As can be seen from Table 2, the linen cloth of the present invention has a slightly lower breaking strength than the pure wet-spun linen cloth in warp and weft directions, but its wrinkle recovery and abrasion resistance are close to those of pure wet-spun linen fabric, and its air permeability is high. It maintains the style of conventional wet-spun linen fabric, and can completely use short-fiber dry-spun linen yarn to replace traditional wet-spun linen yarn as warp yarn, thereby achieving the purpose of saving (fully utilizing) flax raw materials, shortening the spinning process, improving spinning efficiency, and saving energy and reducing emissions.
Claims
1. A method for preparing pure linen grey cloth interwoven with dry-spun and wet-spun linen yarns, include: The method comprises the following steps: using dry-spun linen yarn spun on a cotton spinning system as warp yarn and wet-spun linen yarn as weft yarn, and weaving pure linen grey cloth after warping and sizing, wherein the temperature of the sizing process is below 65°C; wherein the yarn count of the wet-spun linen yarn used for the weft yarn is 24-48 metric count and the twist coefficient is 240-320; the yarn count of the dry-spun linen yarn used for the warp yarn is 20-40 metric count and the twist coefficient is 500-600; the sizing process is sizing the warp yarn, and the sizing material formula is: 60-110 g / L of oxidized phosphate ester potato starch, 1.5-2.5 g / L of glycerol, 1.5-2 g / L of emulsified wax, 0.5-2 g / L of rapid penetrant T, and 1-2.5 g / L of antistatic agent; The preparation method of the potato starch containing oxidized phosphate ester comprises: reacting potato starch milk, hydrogen peroxide and sodium tripolyphosphate at 40-50° C. for 45-60 minutes, and controlling the pH value to be 4-6; wherein in the preparation method of the potato starch containing oxidized phosphate ester, the concentration of the potato starch milk is 40-50%, the amount of hydrogen peroxide used is 0.8-2% of the dry weight of the potato starch, and the amount of sodium tripolyphosphate used is 10-30% of the dry weight of the potato starch.
2. The preparation method according to claim 1, It is characterized in that The substitution degree of the oxidized phosphate ester potato starch is 0.2-0.25, and the gelatinization temperature is 50-60° C.; when the solid content of the oxidized phosphate ester potato starch is 6%, the viscosity of the starch slurry is 15-20 mPa.s.
3. The preparation method according to claim 1, It is characterized in that In the sizing process, the sizing liquid temperature is controlled at 50-60° C. and the sizing speed is controlled at 25-40 m / min, so that the sizing rate is 5-8%.
4. The preparation method according to claim 1, It is characterized in that In the sizing process, after the sizing is skeined, the machine speed is adjusted to 20-40 m / min and the drying drum temperature is 110-130° C., so that the moisture regain of the sizing after drying is controlled to be 12%-16%.
5. The preparation method according to claim 1, It is characterized in that The pure flax grey cloth structure comprises a plain weave or a twill weave.
6. A pure linen grey cloth prepared by the preparation method as claimed in claim 1.
7. A pure linen grey cloth prepared by the preparation method according to claim 1, which is used in clothing or home textile products.
Citation Information
Patent Citations
High-count and high-density pure linen grey cloth warp sizing method
CN101892566A
Wet-spinning cordettes and preparation method thereof
CN101624743A
Method for producing linen wet spinning high count yarns and plied yarns
CN101979732A
Sizing agent for slashing hemp yarn and preparation process thereof
CN102174740A
Production process for dry-spun flax yarns
CN104404670A