Negative electrode binder and its application
By using a negative electrode binder with a self-healing crosslinking network structure in lithium batteries, the structural damage caused by volume expansion of the lithium battery negative electrode is solved, and the cycle life and electrochemical performance are improved.
Patent Information
- Application Number
- CN202210559856.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-05-20
AI Technical Summary
The existing lithium battery negative electrode materials have problems such as structural damage and short cycle life due to volume expansion during charging and discharging. The bonding and buffering performance of existing adhesives are poor, making it difficult to effectively suppress this phenomenon.
A negative electrode binder is used, which consists of a binder matrix and an organic additive. The binder matrix contains active group B, which can form a covalent bond with the active group A in the organic additive, and form an automatic Repaired three-dimensional crosslinking network structure to improve bond strength and stress buffering performance.
It effectively suppresses the volume expansion of the negative electrode material, improves the cycle service life and electrochemical performance, avoids powdering and peeling, and enhances the stability of the negative electrode structure and the cycle performance of the battery.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a negative electrode binder and application thereof. Background Art
[0002] As people's awareness of environmental protection and energy crisis increases, secondary batteries, such as lithium batteries, are becoming more and more popular as a green and environmentally friendly energy storage technology. Lithium batteries are widely used due to their high energy density, long cycle and high stability. With the widespread application of electronic products and the booming development of electric vehicles, the market for lithium batteries is becoming increasingly broad, but at the same time, higher requirements are placed on the safety of lithium batteries.
[0003] At present, the negative electrode materials of lithium batteries are mainly divided into carbon materials and non-carbon materials. Graphite is the most widely used carbon material for lithium-ion battery negative electrode materials. Its actual specific capacity is very close to the theoretical specific capacity limit of 372mAh / g, which is difficult to improve further and is increasingly unable to meet the requirements of high energy density of future power batteries. Among non-carbon materials, the theoretical specific capacity of silicon-based negative electrode materials can reach up to 4200mAh / g, which is about 10 times that of graphite negative electrode. At the same time, it has a lower lithium deintercalation potential, which can avoid lithium precipitation on the surface during charging, and its safety performance is better than that of graphite negative electrode materials. Therefore, silicon-based negative electrode materials are considered to be the first choice for replacing current graphite negative electrode materials. However, in actual use, silicon-based negative electrode materials have a huge volume expansion effect when deintercalating lithium, such as the volume change of silicon can reach more than 300%. The internal stress generated by this drastic volume change will cause cracks, powdering, and peeling of silicon-based negative electrode particles, damage to the electrode structure, and continuous formation of new SEI films at cracks, which seriously affect the cycle life and capacity of lithium-ion batteries.
[0004] Adding a suitable binder is one of the effective ways to inhibit the volume expansion of silicon-based negative electrode materials. However, the existing binders have poor bonding and buffering properties, and have little effect on inhibiting the volume expansion of silicon-based negative electrodes and improving their electrochemical properties, especially cycle performance. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art and to provide a negative electrode binder to solve the technical problems of the existing binder having unsatisfactory adhesion and buffering properties.
[0006] Another object of the present invention is to provide a negative electrode and a secondary battery to solve the technical problem that the existing negative electrode has low structural strength and low peel strength, which leads to unsatisfactory battery cycle performance and other performance.
[0007] In order to achieve the above-mentioned invention object, the first aspect of the present application provides a negative electrode binder. The negative electrode binder of the present application includes a binder matrix, the binder matrix contains a group B, and also includes an organic additive, the organic additive is dispersed in the binder matrix, and the molecular formula of the organic additive is RA x , where RA x Wherein R is an organic group containing -SS-, A is a group that can form a covalent bond with group B, and x is a positive integer greater than or equal to 2.
[0008] Furthermore, the organic additive RA x The invention comprises at least one of 2-hydroxyethyl disulfide, 4,4'-diaminodiphenyl disulfide, 3,3'-dithiodipropionic acid, dithiodiglycolic acid, 4,4'-dithiodibutyric acid, 6,6'-dithiodicotinoic acid, 4,4'-didihydroxydiphenyl sulfide and bis(6-hydroxy-2-naphthalene) disulfide.
[0009] Further, the group B includes -COOH, and the group represented by A includes at least one of -OH and -NH2.
[0010] Or further, the group B includes at least one of -OH and -NH2, and the group represented by A includes -COOH.
[0011] Furthermore, the binder matrix includes at least one of polyacrylic acid, polyvinyl alcohol, polyvinyl alcohol-polyacrylic acid graft copolymer, polyethylene glycol-polyacrylic acid block copolymer, carboxymethyl cellulose, guar gum, chitosan, and polyacrylic acid copolymer.
[0012] Furthermore, the mass ratio of the binder matrix to the organic additive is 100:1 to 10:1.
[0013] Furthermore, the mass ratio of the binder matrix to the organic additive is 70:1 to 30:1.
[0014] In a second aspect of the present application, a negative electrode is provided. The negative electrode of the present application comprises a current collector and a negative electrode active layer bonded to the surface of the current collector, the negative electrode active layer contains a binder and a negative electrode active material, and the binder is the negative electrode binder of the present application.
[0015] Furthermore, the negative electrode active material includes a silicon-based negative electrode material.
[0016] Furthermore, the mass of the negative electrode binder accounts for 1% to 20% of the total mass of the negative electrode active layer.
[0017] In a third aspect of the present application, a secondary battery is provided. The secondary battery of the present application comprises a positive electrode, a negative electrode and a separator stacked between the positive electrode and the negative electrode, wherein the negative electrode is the negative electrode of the present application.
[0018] Compared with the prior art, this application has the following technical effects:
[0019] The binder matrix contained in the negative electrode binder of the present application gives the negative electrode binder of the present application good bonding performance and flexibility. The organic additive contained therein introduces the active group and reversible disulfide bond shown in A, which can form a covalent bond with the binder matrix during the preparation of the negative electrode to form a self-repairable three-dimensional cross-linked network structure. Therefore, the negative electrode binder of the present application has high bonding strength, stress buffering performance and self-repairing ability through the synergistic effect between the contained binder matrix and the organic additive, which can effectively inhibit the volume expansion of the negative electrode active material, especially the silicon-based negative electrode material, and alleviate the stress caused by the volume expansion of the negative electrode, thereby inhibiting the occurrence of material pulverization and structural damage of the negative electrode in the application, and improving the cycle life of the negative electrode and the negative electrode material. Moreover, the negative electrode binder of the present application does not consume active lithium and does not affect the first effect of the battery.
[0020] The negative electrode of the present application contains the negative electrode binder of the present application, so the negative electrode binder can form a three-dimensional network structure in the negative electrode active layer, effectively enhancing the structural stability of the negative electrode active layer, and having a high bonding strength with the current collector, so that the negative electrode of the present application has high structural strength and electrochemical properties such as cycle performance during the charge and discharge cycle, and high first efficiency. It effectively avoids undesirable phenomena such as pulverization and peeling of the negative electrode active layer.
[0021] The negative electrode of the secondary battery of the present application is the negative electrode of the present application described above. Therefore, the secondary battery of the present application has good cycle performance, long life, stable electrochemical performance, and high initial efficiency. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical scheme and technical effect of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is clearly and completely described. The embodiments described below are part of the embodiments of the present invention, rather than all of the embodiments. In conjunction with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or the conditions recommended by the manufacturer; if the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0023] In the description of the present invention, the term "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0024] In the description of the present invention, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0025] It should be understood that the weight of the relevant components mentioned in the embodiments of the present invention can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components in the embodiments of the present invention is proportionally enlarged or reduced, it is within the scope disclosed by the present invention. Specifically, the weight described in the embodiments of the present invention can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0026] In addition, unless the context clearly uses otherwise, the expression of the singular form of a word should be understood to include the plural form of the word. The term "include" or "have" is intended to specify the existence of a feature, quantity, step, operation, element, part or combination thereof, but is not used to exclude the existence or possible addition of one or more other features, quantities, steps, operations, elements, parts or combinations thereof.
[0027] In a first aspect, the present invention provides a negative electrode binder. The negative electrode binder of the present invention comprises a binder matrix and an organic additive, and the two are evenly dispersed to form a mixture.
[0028] Among them, the binder matrix contained in the negative electrode binder of the embodiment of the present application is used as a binder base component, giving the negative electrode binder of the embodiment of the present application good bonding performance and flexibility. Moreover, the binder matrix contains an active group B, which can react with the active group contained in the organic additive to form a chemical bond. In the embodiment, the active group B contained in the binder matrix can be at least one of -COOH, -OH, and -NH2. These active groups B can effectively react with the active groups contained in the organic additive to form a chemical bond, such as a covalent bond, and can enhance the compatibility with the negative electrode active material, thereby improving the bonding strength to the negative electrode active material. In the embodiment, the binder matrix includes at least one of polyacrylic acid, polyvinyl alcohol-polyacrylic acid graft copolymer, polyethylene glycol-polyacrylic acid block copolymer, carboxymethyl cellulose, guar gum, chitosan, and polyacrylic acid copolymer. These binder matrices have strong bonding and excellent flexibility, and have excellent compatibility with negative electrode active materials, especially silicon-based active materials, which improves the bonding strength to negative electrode active materials. Moreover, it is rich in the above-mentioned group B, which can form a stable chemical bond with the organic additive, thereby forming a self-repairing three-dimensional cross-linked network structure in the negative electrode active layer. For example, polyacrylic acid is used as the binder matrix, which has good bonding properties and flexibility, and its abundant carboxyl groups can form a hydrogen bond network between molecular chains; moreover, polyacrylic acid can connect organic additives containing reversible disulfide bonds in the form of covalent bonds to form a self-repairing three-dimensional cross-linked network structure.
[0029] The molecular formula of the organic additive contained in the negative electrode binder of the present embodiment is RA x ; Wherein, R is an organic group containing -SS-, A is a group that can form a chemical bond with the group B contained in the binder matrix; x is a positive integer greater than or equal to 2, specifically 2≤x≤12, and further 2≤x≤5, 5≤x≤12, etc. In this way, the organic additive introduces the active group and reversible disulfide bond (-SS-) shown in A, which can form a chemical bond with the binder matrix during the preparation of the negative electrode to form a self-repairable three-dimensional cross-linked network structure, specifically, the chemical bond formed between the active group A and the group B contained in the binder matrix can form a covalent bond, thereby forming a three-dimensional network structure in the negative electrode active material; moreover, the reversible disulfide bond can play a synergistic role, giving the negative electrode binder of the embodiment of the present application high bonding strength, buffering performance and self-repairing ability, which can effectively inhibit the volume expansion of the negative electrode active material, especially the silicon-based negative electrode material, and alleviate the stress caused by the volume expansion of the negative electrode, thereby inhibiting the occurrence of material pulverization and structural damage of the negative electrode in the application, and improving the cycle life of the negative electrode and the negative electrode material. Moreover, the negative electrode binder in the embodiment of the present application does not consume active lithium, thus ensuring the initial efficiency of the battery.
[0030] In the embodiment, the active group A contained in the organic additive can be at least one of -COOH, -OH, and -NH2. These active groups A can effectively react with the active groups B contained in the binder matrix to generate chemical bonds, such as forming covalent bonds, and can enhance the compatibility with the negative electrode active material, thereby improving the bonding strength to the negative electrode active material. Specifically, the polar active groups contained can generate hydrogen bonds with the surface of the negative electrode active material, especially the silicon-based active material, so that it can firmly bond and coat the negative electrode active material, especially the silicon-based active material, improve the dispersibility of the negative electrode active material, especially the silicon-based active material, and the stability of dispersion in the active layer, limit the movement and separation between the negative electrode active material and other components such as the conductive agent during the cycle, and inhibit the huge volume expansion of the negative electrode active material, especially the silicon-based active material during the charge and discharge process. As in the embodiment, the group B contained in the binder matrix includes -COOH, and the group A contained in the organic additive includes at least one of -OH and -NH2; or, the group B includes at least one of -OH and -NH2, and the group shown in A includes -COOH. At this time, a covalent bond is formed between group A and group B, which can form a rich network structure in the negative electrode active layer, enhance the compatibility between negative electrode binders, and improve the mechanical strength of the negative electrode active layer.
[0031] Based on the types of groups shown by R and A contained in the organic additive and their functions, in the embodiment, the organic additive includes at least one of 2-hydroxyethyl disulfide, 4,4'-diaminodiphenyl disulfide, 3,3'-dithiodipropionic acid, dithiodiglycolic acid, 4,4'-dithiodibutyric acid, 6,6'-dithiodinicotinic acid, 4,4'-dihydroxydiphenyl sulfide, and bis(6-hydroxy-2-naphthalene) disulfide. These organic additives are rich in reversible disulfide bonds (-SS-) and active groups A, which can form chemical bonds, specifically covalent bonds, with the groups B contained in the binder matrix to form a three-dimensional network structure in the negative electrode active material.
[0032] In the embodiment, the mass ratio of the above-mentioned binder matrix and the organic additive contained in the negative electrode binder of the embodiment of the present application can be 100:1 to 10:1. The mass ratio between the binder matrix and the organic additive has an impact on the bonding performance of the negative electrode binder of the present application. For example, when the mass ratio of the binder matrix to the organic additive is greater than 100:1, the cross-linking network density is too low, and the bonding strength, stress buffering capacity and self-repairing ability are all poor; when it is less than 10:1, the cross-linking network is easy to be too dense, the negative electrode active layer is not flexible enough and hardens, and the volume shrinks severely, resulting in the peeling of the negative electrode active layer and the current collector. Furthermore, the mass ratio of the binder matrix to the organic additive is 70:1 to 30:1. It can be understood that by optimizing the ratio of the two, the synergistic effect between the two can be improved, the stability of the three-dimensional network structure formed by the two can be enhanced, the bonding strength between the negative electrode binder and the negative electrode active material, the current collector, and the materials contained in the active layer can be enhanced, and the movement and separation between the negative electrode active material and other components such as the conductive agent during the cycle can be further restricted, and the huge volume expansion of the negative electrode active material such as the silicon-based active material during the charge and discharge process can be suppressed, the mechanical strength of the negative electrode active material can be enhanced, and the uniformity of the dispersion of the negative electrode active material in the negative electrode active layer and the stability during the cycle can be improved. At the same time, the amount of the negative electrode binder can be reduced, thereby effectively improving the structural stability of the negative electrode during the cycle and the stability of the electrochemical performance.
[0033] In addition, the negative electrode binder of the above application example can be prepared according to a method comprising the following steps:
[0034] The binder matrix is mixed with an organic additive to obtain a negative electrode binder.
[0035] The binder matrix is the binder matrix contained in the negative electrode binder of the above-mentioned application example, such as the binder matrix containing group B. The organic additive is also the organic additive contained in the negative electrode binder of the above-mentioned application example, such as the organic additive containing -SS- and having the molecular formula RA x In order to save the space of this application specification, the binder matrix and the organic additive are not described in detail here.
[0036] In this way, the negative electrode binder of the embodiment of the present application is directly mixed with the binder matrix and the organic additive to form a mixture, so that the prepared negative electrode binder forms a chemical bond between the organic additive and the binder matrix during the negative electrode preparation process to form a self-repairable three-dimensional cross-linked network structure, and has high bonding strength, buffering performance and self-repairing ability, and does not consume active lithium. In addition, the process conditions of the preparation method of the negative electrode binder of the embodiment of the present application are easy to control, and the prepared negative electrode binder has stable performance and high efficiency.
[0037] In the embodiment, during or before the mixing process, the binder matrix and the organic additive are added in a mass ratio of 100:1 to 10:1, and further in a ratio of 70:1 to 30:1, thereby improving the synergistic effect between the binder matrix and the organic additive and improving the bonding strength of the prepared negative electrode binder.
[0038] In a second aspect, the present invention also provides a negative electrode. The negative electrode of the present invention comprises a current collector and a negative electrode active layer bonded to the surface of the current collector.
[0039] The current collector may be a commonly used negative electrode current collector.
[0040] The negative electrode active layer may be a negative electrode active layer such as that contained in a conventional electrode, or an improved negative electrode active layer, which includes components such as negative electrode active materials, binders and conductive agents, and of course may also include other additives that are beneficial to the electrochemical performance of the negative electrode. In the present embodiment, the binder contained in the negative electrode active layer is the negative electrode binder of the above text application embodiment. In this way, in the negative electrode active layer, the negative electrode binder can form a three-dimensional network structure in the negative electrode active layer, so that the movement and separation between the negative electrode active material and other components such as the conductive agent are effectively restricted during the cycle process, and the huge volume expansion of the negative electrode active material such as the silicon-based active material during the charge and discharge process is suppressed, and at the same time, the components in the negative electrode active layer such as the negative electrode active material, the conductive agent and other components can be evenly dispersed, and the negative electrode active layer structure is stable, and the bonding strength between the negative electrode and the current collector is high, so that the negative electrode has high structural strength during the charge and discharge cycle, and the electrochemical properties such as the cycle performance are also high, and the first efficiency is high, which effectively avoids the occurrence of undesirable phenomena such as pulverization and peeling of the negative electrode active layer. In addition, since the negative electrode binder has a high bonding strength as described above, its content in the negative electrode is low, so that the negative electrode has high conductivity. As in the embodiment, the mass of the negative electrode binder can account for 1% to 20% of the total mass of the negative electrode active layer, and further can be 5% to 15%, 10% to 15%, 5% to 10%, etc.
[0041] Based on the excellent performance of the negative electrode binder in the above-mentioned embodiment of the present application as described above, the negative electrode active material contained in the negative electrode active layer may include a silicon-based negative electrode material. In this way, the negative electrode binder in the negative electrode active layer can be evenly coated and bonded to the surface of the silicon-based negative electrode material, thereby limiting the movement and separation between the silicon-based negative electrode material and other components such as the conductive agent during the cycle, and inhibiting the huge volume expansion of the silicon-based active material during the charge and discharge process, thereby significantly improving the structure of the silicon-based negative electrode active layer and the high bonding strength with the current collector, so that the structure and electrochemical properties such as cycle performance of the negative electrode during the charge and discharge cycle are significantly improved.
[0042] On the third aspect, the embodiments of the present application also provide a secondary battery. The secondary battery includes a positive electrode, a negative electrode and a separator stacked between the positive electrode and the negative electrode, and of course includes other necessary components of the secondary battery such as an electrolyte or a solid electrolyte. Among them, the negative electrode is the negative electrode of the above-mentioned embodiment of the present application. In this way, the secondary battery of the embodiment of the present application has good cycle performance, long life, stable electrochemical performance, and high first efficiency. In the embodiment, the negative electrode active material contained in the negative electrode active layer is a silicon-based negative electrode material. Therefore, the secondary battery has a high gram capacity, and the secondary battery has good cycle performance, long life, and stable electrochemical performance. In the embodiment, the secondary battery can be a lithium-ion battery.
[0043] The negative electrode binder and its preparation method and lithium metal battery according to the embodiments of the present invention are illustrated below through a plurality of specific embodiments.
[0044] 1. Negative electrode binder and preparation method thereof
[0045] Example A1
[0046] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 100:1. The binder matrix is polyacrylic acid [C3H4O2] n (PAA), the organic additive is 2-hydroxyethyl disulfide.
[0047] Example A2
[0048] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 50:1. The binder matrix is polyacrylic acid [C3H4O2] n (PAA), the organic additive is 2-hydroxyethyl disulfide.
[0049] Example A3
[0050] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 30:1. The binder matrix is polyacrylic acid [C3H4O2] n (PAA), the organic additive is 2-hydroxyethyl disulfide.
[0051] Example A4
[0052] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 10:1. The binder matrix is polyacrylic acid [C3H4O2] n(PAA), the organic additive is 2-hydroxyethyl disulfide.
[0053] Example A5
[0054] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 50:1. The binder matrix is polyacrylic acid [C3H4O2] n (PAA), the organic additive is 4,4'-diaminodiphenyl disulfide.
[0055] Example A6
[0056] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 50:1. The binder matrix is polyvinyl alcohol, and the organic additive is 3,3'-dithiodipropionic acid.
[0057] Example A7
[0058] This embodiment provides a negative electrode binder. The negative electrode binder includes a binder matrix and an organic additive dispersed in the binder matrix at a mass ratio of 50:1. The binder matrix is guar gum, and the organic additive is 3,3'-dithiodipropionic acid.
[0059] Comparative Example A1
[0060] This comparative example provides a binder which, compared with Example A2, does not contain organic additives.
[0061] Comparative Example A2
[0062] This comparative example provides a binder which, compared with Example A6, does not contain organic additives.
[0063] Comparative Example A3
[0064] This comparative example provides a binder which, compared with Example A7, does not contain organic additives.
[0065] 2. Lithium-ion battery embodiment
[0066] Example B1 to Example B7 and Comparative Example B1 to Comparative Example B3
[0067] Embodiments B1 to B7 and Comparative Examples B1 to B3 provide a lithium ion battery, respectively. The lithium ion batteries in Embodiments B1 to B7 and Comparative Examples B1 to B3 respectively include the following structures:
[0068] Negative electrode: The negative electrode binders provided in Examples A1 to A7 and Comparative Examples A1 to A3 were respectively used to prepare negative electrode slurries according to a ratio of silicon-based negative electrode (SiO): conductive agent (SP): negative electrode binder: deionized water of 80:10:10:100, and the negative electrode slurries were coated on copper foil to form negative electrode sheets. The negative electrode sheets were baked in a vacuum oven at 150° C. for 4 h to prepare negative electrode sheets of lithium ion batteries in Examples B1 to B7 and Comparative Examples B1 to B3;
[0069] Positive electrode: prepare positive electrode slurry according to the mass ratio of LiFePO4: conductive agent SP: binder PVDF: NMP of 95:2:3:100, apply it on aluminum foil and dry it to prepare positive electrode sheet, and bake the positive electrode sheet in a vacuum oven at 100°C to remove trace water. ;
[0070] Diaphragm: Use polyethylene (PE) diaphragm. ;
[0071] Electrolyte: The electrolyte is a 1 mol / L LiPF6 solution, and the solvent is composed of EC (ethylene carbonate) and DEC (diethyl carbonate) in a volume ratio of 1:1;
[0072] Assembly: The above-mentioned positive electrode sheet, negative electrode sheet, electrolyte and separator are assembled into a lithium-ion soft-pack battery according to the lithium-ion battery assembly requirements.
[0073] 3. Related characteristics test
[0074] The negative electrode sheets used in the above-mentioned Examples B1 to B7 and Comparative Examples B1 to B3 were respectively subjected to the following performance tests:
[0075] Peel strength test: Divide the negative electrode into 20mm*100mm strips, stick the pressure-sensitive 3M-VHB double-sided tape on the surface of the negative electrode sheet, and stick the other side on the stainless steel plate, and roll back and forth with a pressure wheel for 3 times; pre-peel off the free end of the current collector from the negative electrode material layer, and fold the free end of the current collector 180°, clamp the free end of the current collector and the stainless steel plate on the upper and lower fixtures of the tensile testing machine respectively, and perform a peel test at a speed of 300mm / min and an angle of 180°, and read the average value of the stable peeling stage as the peel strength value.
[0076] The lithium ion batteries assembled from the above-mentioned Examples B1 to B7 and Comparative Examples B1 to B3 were subjected to the following performance tests respectively:
[0077] 0.1C cycle performance test: The battery is placed at 25°C and charged and discharged at a current of 0.1C in the charge and discharge voltage range of 3.0-4.4V. The initial capacity is recorded as Q0, and the capacity after 50 cycles is recorded as Q1. The capacity retention rate of 0.1C cycle 50 cycles is calculated by the following formula:
[0078] 0.1C cycle 50 cycles capacity retention rate (%) = Q1 / Q0 × 100%. 0.5C cycle performance test: the charge and discharge current is 0.5C, and other operations are the same as the 0.1C cycle performance test.
[0079] The test results are shown in Table 1 below:
[0080] Table 1
[0081]
[0082]
[0083] It can be seen from Table 1 that the peel strengths of Examples B1 to B7 are above 0.33 N / cm, and the peel strengths of Comparative Examples B1 to B3 without -SS- are all below 0.25 N / cm, indicating that the negative electrode binder containing a cross-linked network structure provided by the present invention has a higher peel strength; comparing the capacity retention rates of Examples B1 to B7 after 50 cycles, the capacity retention rate of 0.1C cycles of 50 cycles using the negative electrode binder provided by the present invention (>92%) is significantly better than that of the comparative example (<86%), and when the rate is increased to 0.5C, the difference in capacity retention rate is further widened. This is because the negative electrode binder provided by the present invention can form a cross-linked network structure containing a reversible -SS- bond, has high bonding strength, buffering performance and self-repairing ability, can effectively inhibit the volume expansion of silicon-based negative electrode materials, and alleviate the stress caused by the volume expansion of the negative electrode, thereby inhibiting the occurrence of material pulverization and structural damage of the negative electrode in application, and improving the cycle life of the negative electrode and the negative electrode material.
[0084] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A negative electrode binder, comprising a binder matrix, characterized in that: The binder matrix contains a group B and also includes an organic additive, wherein the organic additive is dispersed in the binder matrix, and the molecular formula of the organic additive is RA x , wherein the R is an organic group containing -SS-, the A is a group that can form a covalent bond with the group B, and x is a positive integer greater than or equal to 2; The mass ratio of the binder matrix to the organic additive is 100:1 to 10:1; The RA x The invention comprises at least one of 2-hydroxyethyl disulfide, 4,4'-diaminodiphenyl disulfide, dithiodiglycolic acid, 4,4'-dithiodibutyric acid, 6,6'-dithiodicotinoic acid, 4,4'-didihydroxydiphenyl sulfide and bis(6-hydroxy-2-naphthalene) disulfide.
2. The negative electrode binder according to claim 1, characterized in that: The group B includes -COOH, and the group represented by A includes at least one of -OH and -NH2; or The group B includes at least one of -OH and -NH2, and the group represented by A includes -COOH.
3. The negative electrode binder according to any one of claims 1 to 2, characterized in that: The binder matrix includes at least one of polyacrylic acid, polyvinyl alcohol, polyvinyl alcohol-polyacrylic acid graft copolymer, polyethylene glycol-polyacrylic acid block copolymer, carboxymethyl cellulose, guar gum, chitosan, and polyacrylic acid copolymer.
4. The negative electrode binder according to any one of claims 1 to 2, characterized in that: The mass ratio of the binder matrix to the organic additive is 70:1 to 30:
1.
5. A negative electrode, comprising a current collector and a negative electrode active layer bonded to the surface of the current collector, characterized in that: The negative electrode active layer contains a binder and a negative electrode active material, and the binder is the negative electrode binder according to any one of claims 1 to 4.
6. The negative electrode according to claim 5, characterized in that: The negative electrode active material includes a silicon-based negative electrode material.
7. The negative electrode according to claim 6, characterized in that: The mass of the negative electrode binder accounts for 1% to 20% of the total mass of the negative electrode active layer.
8. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and a separator stacked between the positive electrode and the negative electrode, wherein the negative electrode is the negative electrode according to any one of claims 5 to 7.