Charge-adjusting powder having excellent ability to maintain charged charge and method for producing the same
By forming titanium niobium oxide particles on the core surface of the powder and controlling the alkali metal content, the powder structure is optimized, and the problem of charged charge loss under high humidity is solved, and stable control and charge maintenance of charged properties within a constant range is achieved. Increased rate.
Patent Information
- Application Number
- CN202180014990.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-21
- Filing Date
- 2021-02-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-02-09
AI Technical Summary
The existing powder for charged regulation is difficult to stabilize the amount of charged charge in a high humidity environment, and the charged charge is prone to flow to the outside, resulting in poor electrostatic regulation effect.
By forming titanium-niobium oxide particles on the core surface of the powder, and controlling the alkali metal content below 20.0 mmol/kg, the number of surface pits and the surface area ratio measured by the BET method was observed by scanning electron microscope to optimize the particle interface resistance. To improve charge maintenance capabilities.
The excellent ability to maintain charged charge in a high humidity environment is achieved, ensuring that the chargeability is within a constant range, and the charge maintenance rate of the charged adjustment powder is significantly improved.
Smart Images

Figure CN115103889B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a powder for adjusting charge for adjusting charge generated on the surface of a coating, a functional powder, a film, a fiber, a resin, a plastic, a paper, etc., and a method for producing the same. Background Art
[0002] Powders made of conductive metal oxides and paints, fibers, plastics, and paper containing the same are used to prevent static electricity and remove static electricity by utilizing the conductivity of the metal oxides.
[0003] For example, Japanese Patent Publication No. 2002-339235 (Patent Document 1) discloses a method of manufacturing a fabric with excellent antistatic properties by subjecting the fabric to low-temperature plasma treatment, wherein the fabric is obtained by arranging and weaving conductive synthetic fibers dispersed with titanium oxide particles coated with carbon black or tin oxide at a constant interval. In addition, Japanese Patent Publication No. 2010-59588 (Patent Document 2) proposes a polyester composite fiber with excellent color rendering properties, wherein the polyester composite fiber is formed by a non-conductive layer and a conductive layer, wherein the conductive layer is a thermoplastic polymer containing titanium oxide particles having a conductive coating such as tin oxide. The polyester composite fiber disclosed in Patent Document 2 has an antistatic property because the fiber interior is a conductive layer, thereby suppressing static electricity charging.
[0004] These conductive metal oxides and coatings, fibers, plastics, and papers containing them are intended or effective to prevent the generation of static electricity on their surfaces or to remove the generated static electricity. However, in recent years, the opportunities for utilizing static electricity in industries such as electrostatic precipitator, electrostatic copying, and electrostatic coating have increased, and it is required that the powder for charge regulation can not only simply remove the charged charge, but also control the amount of the charged charge.
[0005] The applicant has disclosed a powder for charge adjustment, which uses titanium dioxide as a core particle and has a coating of niobium-doped titanium dioxide on the surface of the core particle (Japanese Patent Publication No. 2018-141058) (Patent Document 3). By mixing or applying the powder for charge adjustment, in addition to preventing static electricity from charging the surface of the object, the charge amount can also be adjusted to a negative value.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 2002-339235
[0009] Patent Document 2: Japanese Patent Application Publication No. 2010-059588
[0010] Patent Document 3: Japanese Patent Application Publication No. 2018-141058 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] The charge adjustment powder of Patent Document 3 is intended to prevent static electricity, and the charged charge tends to decay immediately. In order to stably control the amount of the charged charge, the charge adjustment powder of Patent Document 3 is difficult to use. In particular, the charged charge tends to flow to the outside easily under high humidity.
[0013] The object of the present invention is to provide a powder for charge adjustment and a method for manufacturing the powder, which can be added, mixed, or coated on a charge adjustment object such as a coating, functional powder, film, fiber, resin, plastic, paper, etc., so as to control the charge of each surface within a constant range and has excellent ability to maintain the charge.
[0014] Solutions for solving problems
[0015] The inventors of the present invention have conducted intensive studies on charge adjustment powders and have found that the ability to maintain charge is improved when the alkali metal content in a powder formed of particles having titanium niobium oxide on at least a portion of the core material surface is 20.0 mmol / kg or less relative to the total.
[0016] The specific embodiments of the present invention are not limited to these, and are as follows.
[0017] [1] A charge adjustment powder comprising particles having titanium niobium oxide on at least a portion of a core material surface, wherein the charge adjustment powder has an alkali metal content of 20.0 mmol / kg or less relative to the entire powder.
[0018] [2] The charge adjustment powder according to [1], wherein the sum of the alkali metal content and the sulfur content is 35.0 mmol / kg or less relative to the whole.
[0019] [3] The charge adjustment powder according to any one of [1] or [2], wherein the niobium content is 15.0 mmol / kg or more and 225.0 mmol / kg or less relative to the total amount.
[0020] [4] The charge adjustment powder according to any one of [1] to [3], wherein the core material is titanium dioxide.
[0021] [5] The charge adjustment powder according to any one of [1] to [4], wherein pits are observed on at least a portion of the surface of particles constituting the powder when observed at a magnification of 50,000 times using a scanning electron microscope.
[0022] [6] The charge adjustment powder according to any one of [1] to [5], wherein the number of pits observed on the surface of particles constituting the powder when observed with a scanning electron microscope at a magnification of 50,000 times is 0.1 μm 2 More than 10 on the particle surface.
[0023] [7] A charge regulating powder according to any one of [1] to [6], wherein when the surface area per 1 g measured by the BET method is set to S1 and the surface area per 1 g calculated from the volume-based median particle size obtained based on observation with a scanning electron microscope is set to S2, S1 / S2 is greater than 1.05.
[0024] [8] A method for producing a charge-adjusting powder according to any one of [1] to [7], characterized by comprising the following steps A to D:
[0025] A: A process of dispersing the powder to be the core material in water to obtain a suspension of the core material;
[0026] B: adding an acidic mixed solution of titanium salt and niobium salt and an alkaline solution to the suspension obtained in step A, neutralizing the acidic mixed solution of titanium salt and niobium salt with the alkaline solution, and precipitating titanium and niobium hydroxides on at least a portion of the surface of the core material;
[0027] C: a step of removing water-soluble salts from the suspension obtained in step B and performing solid-liquid separation;
[0028] D: A step of calcining the solid component obtained in step C.
[0029] [9] The method for producing a charge-adjusting powder according to [8], wherein in the step B, neutralization is performed so that the pH of the suspension is 1.0 to 6.0.
[0030]
[10] The method for producing a charge-adjusting powder according to [8] or [9], wherein in the step B, an acidic mixed solution of titanium salt and niobium salt and an alkaline solution are added simultaneously.
[0031]
[11] A method for manufacturing a charge-adjustable powder according to any one of [8] to
[10] , wherein the aforementioned step D includes the following steps: calcining the solid component at a temperature of not less than 250°C and not more than 900°C in an air atmosphere, an inert atmosphere, a reducing atmosphere, or an atmosphere with an oxygen concentration lower than that of the air.
[0032] Effects of the Invention
[0033] According to the present invention, by using particles having a titanium niobium oxide on a portion of the core material surface and having an alkali metal content of 20.0 mmol / kg or less relative to the whole, a charge adjustment powder having excellent ability to maintain a charged charge is provided. In particular, the ability to maintain a charged charge is excellent when exposed to high humidity. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a scanning electron microscope photograph of the charge adjustment powder obtained in Example 5.
[0035] Figure 2 This is a scanning electron microscope photograph of the charge adjustment powder obtained in Comparative Example 1.
[0036] Figure 3 is the equivalent circuit model used to calculate the particle interface resistance. DETAILED DESCRIPTION
[0037] The charge adjustment powder of the present invention is formed of particles having titanium niobium oxide on at least a portion of a core material surface, and the charge adjustment powder has an alkali metal content of 20.0 mmol / kg or less relative to the entire powder.
[0038] The aforementioned powder for charge adjustment preferably has a core material of titanium dioxide and a composite oxide of titanium and niobium on the surface. The amount of niobium in the powder for charge adjustment is preferably 15.0 mmol / kg or more and 225.0 mmol / kg or less relative to the whole. If the niobium content is 15.0 mmol / kg or more, the charge generation effect is exerted, and the stability of oxygen deficiency that contributes to charge transport can be obtained. If the niobium content is 225.0 mmol / kg or less, since a single phase is formed in the particles, it is not easy to generate charge distribution, and the charge performance is easy to stabilize. The niobium content is more preferably 100.0 mmol / kg or more and 200.0 mmol / kg or less, and further preferably 125.0 mmol / kg or more and 200.0 mmol / kg or less. In addition, if the niobium content is 150.0 mmol / kg or more and 200.0 mmol / kg or less, it is further preferred.
[0039] The alkali metal content of the aforementioned charge regulating powder is less than 20.0 mmol / kg relative to the whole. If the alkali metal content is large, the alkali metal salt will precipitate on the particle surface and the particle interface resistance will decrease. When the particle interface resistance is small, the electric charge on the particle becomes easy to flow to the outside, and it becomes difficult to maintain the electric charge. The alkali metal content is more preferably less than 10.0 mmol / kg, and further preferably less than 8.0 mmol / kg. In this specification, "alkali metal" refers to sodium and potassium, and when it is referred to as "alkali metal content", it refers to the sum of the contents of these two metals.
[0040] The alkali metal in the charge adjustment powder is mainly derived from the alkaline solution used to neutralize the acidic mixed solution of the titanium salt and the niobium salt when the titanium niobium oxide is formed on at least a part of the particle surface constituting the powder.
[0041] In the aforementioned charge adjustment powder, the sum of the alkali metal content and the sulfur content is preferably 35.0 mmol / kg or less relative to the whole. If the sum of the alkali metal content and the sulfur content is 38.5 mmol / kg or less, the charge retention rate measured by the method described below is easily improved. It is more preferably 15.0 mmol / kg or less, and further preferably 13.0 mmol / kg or less.
[0042] The reason why the sum of the content of alkali metal and the content of sulfur affects the charge maintenance rate is unclear, but it is considered as follows. In the present invention, alkali metal and sulfur are sometimes added to the particles from the core material or from the solution used to form titanium niobium oxide on the core material, and both alkali metal and sulfur exist in the particles in a polar state. When the content of polar substances is large, it is believed that when the particles are charged, a circuit is formed in the particles, and the charge becomes easy to flow to the outside of the particles, making it difficult to maintain the charged charge.
[0043] In the charge adjustment powder of the present invention, it is preferred that fine pits exist on at least a portion of the surface of the particles constituting the powder. By having pits on the surface, the contact area between the primary particles is reduced, and it becomes less likely to cause charge transfer between the particles. The pits on the surface of the particles here refer to tiny holes in the form of black spots observed on the surface of the particles in a scanning electron microscope photograph with a magnification of 50,000 times. The shapes of the pits include circular, elliptical, rectangular, polygonal and amorphous, and the equivalent circle diameter is as small as 5nm and as large as about 45nm. In addition, there are also elongated groove-shaped pits. The groove-shaped pits also have a shape that bends in the middle, and the largest is about 25nm wide and 90nm long. The pits may also reach the core particles, with a maximum depth of about 15nm. Figure 1 , a scanning electron microscope photograph of the charge adjustment powder of the present invention (Example 5 described later) is shown in FIG. Figure 2 The scanning electron microscope photograph of the charge adjustment powder for comparison (Comparative Example 1 described later) is shown in FIG. The particle surfaces of the comparative powders are all smooth, and the number of pits is very small ( Figure 2 ), and it can be seen that a large number of black spot-like pits can be observed on the particle surface of the powder of the present invention ( Figure 1 ).
[0044] The reason why pits are formed on the particle surface is unclear, but it is considered as follows: a large amount of titanium niobium hydroxide exists on the surface of the core particle before calcination, and the calcination causes water and other components to volatilize, resulting in a reduction in volume and the formation of pits.
[0045] On the other hand, it is believed that when the temperature rises, the substance diffusion of the hydroxide and the composite oxide of titanium and niobium becomes active, and the pits disappear. In addition, it is believed that when an alkali metal salt such as sodium is present, the substance diffusion becomes more active, and therefore the pits disappear more easily.
[0046] In the powder for charge adjustment of the present invention, each particle size is 1 μm 2 The number of pits per surface area is preferably 10 or more. More preferably, the number of pits per 1 μm of the particle is 2 The number of pits on the surface area is 50 or more, more preferably 70 or more. 2 The number of pits in the surface area was measured by the method described below.
[0047] In the charge adjustment powder of the present invention, the specific surface area S1 (m 2 / g) and the specific surface area S2 (m 2 / g), preferably the value S1 / S2 obtained by dividing S1 by S2 is greater than 1.05. S1 and S2 are calculated by the method described below. Since S2 is the specific surface area calculated from the particle size, it does not reflect the pits on the surface. Therefore, the more pits on the surface of the particles, the larger S1 / S2. If S1 / S2 is greater than 1.05, there are many pits on the surface of the particles, so the contact area between the primary particles is reduced, and it becomes difficult to cause charge transfer between the particles. Preferably, S1 / S2 is greater than 1.10, and more preferably greater than 1.15.
[0048] In the charge adjustment powder of the present invention, the value of the particle interface resistance measured by the method described below is preferably 1.80×10 6 Ω·cm or more, more preferably 2.00×10 6 Ω·cm or more, more preferably 4.00×10 6 The larger the value of the particle interface resistance, the less likely it is that the charged charge will flow to the outside, and the more likely it is that the charged charge will be maintained.
[0049] The charge adjustment powder of the present invention preferably has a negative charge amount. The initial value of the charge amount is more preferably -20.0 μC / g or less, and further preferably -30.0 μC / g or less.
[0050] In the charge adjustment powder of the present invention, the charge maintenance rate measured by the method described below is preferably 84.0% or more, more preferably 86.0% or more, and further preferably 90.0% or more. In addition, the charge maintenance rate measured after humidification by the method described below is preferably 84.0% or more, more preferably 85.5% or more, and further preferably 88.0% or more.
[0051] The particle size of the primary particles constituting the charge regulating powder of the present invention is not particularly limited. Taking into account the ease of pulverization after calcination and the dispersibility in the charge regulating object, the volume-based median particle size measured by the method described below is preferably greater than 0.050 μm and less than 0.500 μm.
[0052] By adding, mixing, or applying the charge regulating powder of the present invention to charge regulating objects such as coatings, functional powders, films, fibers, resins, plastics, and paper, it is possible to provide a constant negative charge to each object while improving the ability to maintain the charge.
[0053] The charge adjustment powder of the present invention can be produced by a production method including the following steps A to D.
[0054] A: A process of dispersing the powder to be the core material in water to obtain a suspension of the core material.
[0055] B: adding an acidic mixed solution of titanium salt and niobium salt and an alkaline solution to the suspension obtained in step A, neutralizing the acidic mixed solution of titanium salt and niobium salt with the alkaline solution, and precipitating titanium and niobium hydroxides on at least a portion of the surface of the core material;
[0056] C: a step of removing water-soluble salts from the suspension obtained in step B and performing solid-liquid separation,
[0057] D: A step of calcining the solid component obtained in step C.
[0058] Hereinafter, the method for producing the charge adjustment powder of the present invention will be described.
[0059] [Process A: Core material]
[0060] The core material used in step A is preferably anatase titanium dioxide. In addition to anatase titanium dioxide, rutile titanium dioxide, mixed crystal titanium dioxide of anatase and rutile, and titanium dioxide generally having the chemical formula TiO 2-n / 2 (OH) n (n is greater than 0 and less than 4). Titanium dioxide in an anatase single phase or titanium dioxide having a rutile ratio of 0.05 or less as measured by X-ray diffraction is particularly preferred. When titanium dioxide is used as the core material used in step A, it is preferred to use titanium dioxide that has not been surface treated in order to promote the subsequent coating with titanium niobium oxide.
[0061] The particle size of the core material is not particularly limited, but is preferably about 0.050 to 0.500 μm from the viewpoint of suppressing aggregation of particles.
[0062] In step A, when the powder to be the core material is dispersed in water, it is preferred to raise the temperature while stirring. The temperature after the heating is preferably within the range of 55 to 85°C, more preferably 65 to 80°C.
[0063] [Step B: Acidic mixture of titanium salt and niobium salt]
[0064] The acidic mixed solution of titanium salt and niobium salt used in step B can be prepared by mixing an aqueous solution of titanium salt that will become a titanium source with an aqueous solution of niobium salt that will become a niobium source. As a titanium source, titanium sulfate, titanium chloride, etc. can be suitably used. As a niobium source, niobium pentachloride, niobium (V) hydroxide, niobium pentoxide, niobium (V) hydroxyhydroxide, etc. can be suitably used. Hydrochloric acid and sulfuric acid are preferably used for the dissolution of the niobium source, but aqueous solutions of niobium and other acids can also be used. For example, a titanium-niobium acidic mixed solution can be prepared by dissolving niobium chloride in hydrochloric acid to form a solution of 30 g / kg of niobium elemental Nb, and then mixing it with an aqueous solution of titanium sulfate. In addition, niobium hydroxide and niobium pentoxide can be dissolved in concentrated sulfuric acid and mixed with an aqueous solution of titanium sulfate to prepare a titanium-niobium acidic mixed solution.
[0065] [Process B: Neutralization]
[0066] In step B, an acidic mixture of titanium salt and niobium salt and an alkaline solution are added to the suspension obtained in step A, and the acidic mixture of titanium salt and niobium salt is neutralized with the alkaline solution, so that the hydroxides of titanium and niobium are precipitated on at least a portion of the surface of the core material. The suspension obtained in step B is subjected to solid-liquid separation, and when the dried sample is observed with a transmission electron microscope, it is preferred that more than 90% of the surface of the core material is covered with the hydroxides of titanium and niobium. The pH of the suspension when the acidic mixture and the alkaline solution are added is preferably within the range of 1.0 to 6.0. More preferably, it is 2.0 to 4.0. In addition, it is preferred that the pH is maintained at a constant value within the above range. In order to maintain the pH at a constant value, it is preferred to add the acidic mixture of titanium salt and niobium salt and the alkaline solution at the same time.
[0067] The alkaline solution added for neutralization is not particularly limited, and one or more selected from sodium hydroxide, potassium hydroxide, sodium carbonate, or ammonia can be preferably used. Sodium hydroxide is cost-effective.
[0068] The temperature during neutralization is preferably within a range of 55 to 85° C., more preferably within a range of 65 to 80° C., and is maintained at a constant value.
[0069] After the addition of the acidic mixed solution and the alkaline solution is completed, the suspension can be maintained at a predetermined pH and a predetermined temperature for a constant time to be aged. The temperature and pH at this time are not particularly limited. The maintenance time is not particularly limited, but is preferably about 10 minutes to 2 hours.
[0070] [Step C: Removal of water-soluble salts and solid-liquid separation]
[0071] In step C, it is preferred to repeatedly wash with an aqueous solvent having a low impurity content to remove water-soluble salts in such a way that the amount of water-soluble salts remaining in the suspension obtained in step B is as small as possible. For washing during the removal of water-soluble salts, a filter press or the like can be used arbitrarily.
[0072] Water-soluble salts include salts derived from acidic mixed solutions and alkaline solutions. As an indicator of the degree of removal of water-soluble salts in process C, the content of alkali metals and the content of sulfur in the solid components in the suspension can be used. Alkali metals are mainly derived from alkaline solutions. Therefore, when sodium hydroxide or sodium carbonate is used as an alkaline solution, the content of sodium can be used as an indicator of the degree of removal of water-soluble salts. Sulfur is mainly derived from sulfuric acid. The content of alkali metals (such as sodium) and sulfur can be evaluated by sampling a part of the solid components after washing and fully drying them, and then the method described below is described. It should be noted that since sulfur volatilizes at high temperatures, its content decreases after roasting, so a certain amount of sulfur may also remain in the stage of process C.
[0073] The alkali metal content of the solid content after washing in step C is preferably 18.5 mmol / kg or less, more preferably 10.0 mmol / kg or less, and further preferably 5.0 mmol / kg or less. In addition, the sulfur content of the solid content after washing in step C is preferably 230.0 mmol / kg or less, more preferably 200.0 mmol / kg or less, and further preferably 150.0 mmol / kg or less.
[0074] After the water-soluble salts are removed, solid-liquid separation is performed to obtain a solid component. The obtained solid component can be dried arbitrarily. The temperature and time during drying are not particularly limited, for example, 100 to 150° C. for 1 to 24 hours.
[0075] [Step D: Calcination]
[0076] The temperature during calcination is preferably above 250°C and below 900°C. The calcination atmosphere is not particularly limited, and calcination can be carried out in an atmosphere having an oxygen concentration increased compared to the atmosphere, an atmospheric atmosphere, an atmosphere having an oxygen concentration reduced compared to the atmosphere, a non-oxidizing atmosphere of nitrogen, or a reducing atmosphere of hydrogen. By calcining in an atmosphere having oxygen, the oxidation of the particle surface is calcined in a non-oxidizing atmosphere or a reducing atmosphere, thereby reducing the particle surface. The atmosphere can be changed to carry out 2-stage calcination or 3-stage calcination or more, and the atmosphere and temperature of the 2nd stage or 3rd stage and the subsequent calcination can be appropriately changed according to the degree of oxidation of the particle surface. By adjusting the surface oxidation or reduction, the resistance, charging performance and hue of the calcined powder can be adjusted. The calcination time, the holding time, and the atmospheric gas flow rate can be appropriately adjusted according to the characteristics of the desired powder and the size of the furnace used, and the input amount of the solid component. For example, but not limited to this, it is preferred to perform the first stage calcination at a temperature of 250°C to 780°C in a non-oxidizing atmosphere or a reducing atmosphere, and then perform the second stage calcination at a temperature of 250°C to 500°C in an air atmosphere.
[0077] [crush]
[0078] The obtained calcined body can be appropriately pulverized to form a powder for charge adjustment. The pulverization method can use a known method such as a roller mill, a jet mill, a container-driven mill, etc. without limitation, and can be pulverized with a general-purpose pulverizer. The pulverization method is determined in consideration of the particle size, the proportion of coarse particles in the pulverized product, the cost, etc.
[0079] Next, a method for measuring the physical properties of the charge adjustment powder will be described.
[0080] [Method for measuring the rutile rate of titanium dioxide]
[0081] The diffraction intensity of the (101) plane of anatase titanium dioxide and the (110) plane of rutile titanium dioxide was measured using an X-ray diffraction device RINT-TTR III manufactured by Rigaku Co., Ltd., with a target of copper (Cu), a tube voltage of 50 kV, a tube current of 300 mA, a divergence slit of 1 / 2°, a divergence longitudinal slit of 10 mm, a scattering slit of 1 / 2°, a receiving slit of 0.15 mm, and a scanning speed of 0.5° / min, with 2θ scanning from 20 deg to 35 deg. Based on these diffraction intensities, the diffraction intensity (R) of the (110) plane of rutile titanium dioxide was divided by the sum of the diffraction intensity (A) of the (101) plane of anatase titanium dioxide and the diffraction intensity (R) of the (110) plane of rutile titanium dioxide to obtain the rutile rate.
[0082] Rutile rate = R / (A+R)
[0083] [Determination method of niobium, sulfur, and alkali metal content]
[0084] Niobium, potassium and sulfur were measured using a fluorescent X-ray analyzer, and the content was determined from the characteristic X-ray intensity. Sodium was dissolved in a sample and the content was determined using the ICP method.
[0085] [Measurement method of specific surface area S1 by BET method]
[0086] The specific surface area S1 based on the BET method was measured by a one-point method using GEMINI 2375 manufactured by MICROMETORICS INSTRUMENT CO.
[0087] [Measurement of Volume-Based Median Particle Size of Primary Particles and Calculation Method of Specific Surface Area S2]
[0088] The observation of the sample based on the scanning electron microscope (hereinafter abbreviated as "SEM") was performed using JESM-7200 manufactured by JEOL Ltd. More than 200 primary particles were measured from the image. The projected area circle equivalent diameter was measured as the primary particle size. In the present invention, for the case where two or more particles are combined by roasting, the particle size of each particle is measured only when the boundary can be determined from the SEM photograph. The particle size equivalent to 50% in the cubic cumulative curve is taken as the volume-based median particle size. The volume-based median particle size is set to r v When μm, the specific surface area S2 is calculated by the following formula.
[0089] S2=4×π×[(r v / 2) / 10 6 ] 2 / {4 / 3×π×[(r v / 2) / 10 6 ] 3 × Particle density (g / m 2 )}
[0090] It should be noted that in the following examples and comparative examples, the particles are composed of about 97.7% anatase titanium dioxide (particle density 3.90×10 6 g / m 3 ) and about 2.3% niobium pentoxide (particle density 4.47×10 6 g / m 3 ) is composed of, therefore, as the particle density of the above formula, 3.93×10 6 g / m 3 .
[0091] [Method for measuring the number of pits per unit area on particle surface]
[0092] Use SEM to observe the particles at a magnification of 50,000 times. For more than 200 particles whose half-surface can be completely confirmed, count the number of pits existing on the half-surface. In the SEM photo, the pits are observed as black spots on the surface of the particles. The number of pits is set to 2 times, which is the number of pits existing on the surface of each particle. For the aforementioned primary particle size, a cumulative curve of the square of the particle size is prepared, and the particle size equivalent to 50% is taken as the area-based median particle size (μm). The surface area of each particle is calculated from the area-based median particle size. For one particle, the value obtained by dividing the number of pits by the area of the particle (2 significant figures) is taken as the number of pits per unit area of the particle surface.
[0093] [Measurement method of particle interface resistance]
[0094] 1 g of the sample was compressed with a powder resistance measurement jig manufactured by TOYO Corporation and measured using VersaSTAT4 manufactured by Research at a voltage of 300 mV and a frequency of 10 -3 Hz and above and 10 6 The Nyquist plot was obtained by measuring as follows: assuming that there are three resistance components, namely, bulk resistance, particle interface resistance, and electrode contact resistance, the particle interface resistance was obtained by fitting with an equivalent circuit. Figure 3 . The equivalent circuit model for calculating the particle interface resistance is shown in FIG.
[0095] [Measurement method of powder charge maintenance rate]
[0096] 0.100g of the sample was mixed with 9.900g of the iron powder carrier, placed in a polyethylene bottle with a diameter of 40mm and a height of 85mm, and shaken in a Paint Shaker 5110 made by Red Devil for 1 minute. After friction charging, the powder charge was quickly measured using a powder charge measuring device TB-200 made by Toshiba Chemical as the initial value of the charge. After the measurement, the mixture was allowed to stand for 4 minutes in a state mixed with the iron powder carrier, and then measured again. The value obtained by dividing the measured value after 4 minutes by the initial value was used as the charge maintenance rate.
[0097] [Measurement method of powder charge maintenance rate of humidified sample]
[0098] After the sample was left to stand in a humidified environment at a temperature of 40° C. and a relative humidity of 98% for 48 hours, the powder charge retention rate was measured in the same manner as above.
[0099] Example
[0100] The present invention will be described in more detail with reference to the following examples and comparative examples. The following examples are given for illustrative purposes only and the protection scope of the invention is not limited thereto.
[0101] [Example 1]
[0102] Niobium (V) hydroxide was dissolved in concentrated sulfuric acid and mixed with an aqueous solution of titanium sulfate to prepare an acidic mixed solution of titanium salt and niobium salt (hereinafter referred to as "titanium-niobium mixed solution"). A surface-untreated titanium dioxide powder having an average primary particle size of 0.18 μm and a rutile rate of 0.01 was dispersed in water to form a suspension, and the temperature was raised while stirring. After reaching 70°C, a titanium-niobium mixed solution containing 337 g / kg of Ti and 20.6 g / kg of Nb relative to the weight of titanium dioxide to be the core material and an aqueous solution of sodium hydroxide were added simultaneously while maintaining the pH at 2.5. After the addition was completed, an aqueous solution of sodium hydroxide was added to adjust the pH of the reaction solution to 5.5. After maintaining at 70°C for 0.5 hour, the reaction solution was cooled, washed until the sodium content in the solid component was less than 0.2 mmol / kg and the sulfur content was 11.9 mmol / kg, and solid-liquid separation was performed. The washed solid component was dried in a dryer at 110°C for 12 hours. The dried solid component was calcined at 700° C. for 2 hours in nitrogen, and the calcined product was further calcined at 430° C. for 2 hours in air atmosphere and pulverized to prepare Sample 1.
[0103] The results of the measurement of sample 1 by fluorescent X-ray and ICP method showed that the niobium content was 170.1 mmol / kg, the alkali metal content was 1.5 mmol / kg, and the sum of the alkali metal content and the sulfur content was 5.2 mmol / kg. The specific surface area S1 obtained by the BET method was 9.00 m 2 The volume-based median diameter of the primary particles analyzed by SEM images was 0.226 μm, and the surface area S2 per 1 g calculated from the volume-based median diameter was 6.77 m 2 / g, S1 / S2 is 1.33. The area-based median particle size is 0.203 μm, and the number of pits per unit area is 100 / μm 2 The particle interface resistance is 6.90×10 6 Ω·cm, the initial value of the charge amount was -42.2 μC / g, the charge maintenance rate was 91.1%, and the charge maintenance rate of the humidified sample was 89.1%.
[0104] [Example 2]
[0105] After the reaction solution was cooled, washing was completed when the sodium content in the solid content reached 2.3 mmol / kg and the sulfur content reached 14.7 mmol / kg, and the second stage calcination temperature was set to 400°C. Sample 2 was prepared in the same manner as in Example 1. Sample 2 had a niobium content of 176.1 mmol / kg, an alkali metal content of 5.8 mmol / kg, a total of an alkali metal content and a sulfur content of 9.6 mmol / kg, an S1 / S2 ratio of 1.36, and a number of pits per unit area on the particle surface of 100 / μm. 2 The particle interface resistance is 5.50×10 6 Ω·cm, the initial value of the charge amount was -36.3 μC / g, the charge maintenance rate was 99.4%, and the charge maintenance rate of the humidified sample was 98.5%.
[0106] [Example 3]
[0107] After the reaction solution was cooled, washing was terminated when the sodium content in the solid content reached 3.9 mmol / kg and the sulfur content reached 7.9 mmol / kg. Sample 3 was prepared in the same manner as in Example 1 except that the niobium content of Sample 3 was 173.8 mmol / kg, the alkali metal content was 7.2 mmol / kg, the sum of the alkali metal content and the sulfur content was 12.2 mmol / kg, S1 / S2 was 1.23, and the number of pits per unit area on the particle surface was 74 / μm. 2 The particle interface resistance is 5.80×10 6 Ω·cm, the initial value of the charge amount was -35.0 μC / g, the charge maintenance rate was 94.1%, and the charge maintenance rate of the humidified sample was 98.0%.
[0108] [Example 4]
[0109] After the addition of the titanium-niobium mixed solution and the sodium hydroxide aqueous solution, the pH of the reaction solution was not adjusted to 5.5, and the pH was kept at 70°C for 0.5 hours while maintaining the pH at 2.5. After the reaction solution was cooled, it was washed until the sodium content in the solid component was less than 0.2 mmol / kg and the sulfur content was 83.2 mmol / kg. The calcination temperature in the first stage was 750°C and the calcination temperature in the second stage was 450°C. Sample 4 was prepared in the same manner as in Example 1 except that the niobium content of Sample 4 was 167.0 mmol / kg, the alkali metal content was 1.7 mmol / kg, the sum of the alkali metal content and the sulfur content was 14.2 mmol / kg, S1 / S2 was 1.27, and the number of pits per unit area on the particle surface was 100 / μm. 2 The particle interface resistance is 2.30×10 6Ω·cm, the initial value of the charge amount was -37.8 μC / g, the charge maintenance rate was 87.7%, and the charge maintenance rate of the humidified sample was 85.9%.
[0110] [Example 5]
[0111] After the addition of the titanium-niobium mixed solution and the sodium hydroxide aqueous solution, the pH of the reaction solution was not adjusted to 5.5. The pH was kept at 70°C for 0.5 hour while maintaining the pH at 2.5. After the reaction solution was cooled, it was washed until the sodium content in the solid component was less than 0.2 mmol / kg and the sulfur content was 175.1 mmol / kg. The calcination temperature of the first stage was 780°C and the calcination temperature of the second stage was 470°C. Except for this, sample 5 was prepared in the same manner as in Example 1. Figure 1 The SEM photograph of sample 5 is shown. The niobium content of sample 5 is 170.4 mmol / kg, the alkali metal content is 1.5 mmol / kg, the sum of the alkali metal content and the sulfur content is 30.2 mmol / kg, S1 / S2 is 1.57, and the number of pits per unit area on the particle surface is 110 / μm. 2 The particle interface resistance is 1.30×10 7 Ω·cm, the initial value of the charge amount was -47.6μC / g, the charge maintenance rate was 84.7%, and the charge maintenance rate of the humidified sample was 85.2%.
[0112] [Example 6]
[0113] After the reaction solution was cooled, it was washed until the sodium content in the solid content was less than 0.2 mmol / kg, the sulfur content was 8.6 mmol / kg, and the first stage calcination temperature was 730°C. The same method as in Example 1 was used to prepare Sample 6. Sample 6 had a niobium content of 174.6 mmol / kg, an alkali metal content of 2.1 mmol / kg, a total of an alkali metal content and a sulfur content of 5.9 mmol / kg, an S1 / S2 ratio of 1.33, and a number of pits per unit area on the particle surface of 110 / μm. 2 The particle interface resistance is 8.20×10 6 Ω·cm, the initial value of the charge amount was -44.7 μC / g, the charge maintenance rate was 92.2%, and the charge maintenance rate of the humidified sample was 86.5%.
[0114] [Comparative Example 1]
[0115] After the reaction solution was cooled, washing was stopped when the sodium content in the solid content reached 26.4 mmol / kg and the sulfur content reached 10.4 mmol / kg, and the calcination temperature in the first stage was 800°C and the calcination temperature in the second stage was 450°C. Sample 6 was prepared in the same manner as in Example 1. Sample 6 had a niobium content of 164.2 mmol / kg, an alkali metal content of 31.0 mmol / kg, a total of an alkali metal content and a sulfur content of 39.8 mmol / kg, an S1 / S2 ratio of 0.98, and a number of pits per unit area on the particle surface of 1.4 / μm. 2 The particle interface resistance is 1.50×10 6 Ω·cm, the initial value of the charge amount was -23.9 μC / g, the charge maintenance rate was 83.0%, and the charge maintenance rate of the humidified sample was 82.9%.
[0116] [Comparative Example 2]
[0117] The liquid temperature of the reaction liquid was set to 60°C when the titanium-niobium mixed liquid and the sodium hydroxide aqueous solution were added and when the temperature was maintained after the addition was completed. After the reaction liquid was cooled, the washing was completed when the sodium content in the solid component reached 39.4 mmol / kg and the sulfur content reached 6.7 mmol / kg. The roasting temperature in the first stage was set to 800°C and the roasting temperature in the second stage was set to 450°C. Sample 7 was prepared in the same manner as in Example 1 except that the niobium content of Sample 7 was 169.9 mmol / kg, the alkali metal content was 44.7 mmol / kg, the sum of the alkali metal content and the sulfur content was 50.9 mmol / kg, S1 / S2 was 0.96, and the number of pits per unit area on the particle surface was 8.1 / μm. 2 The particle interface resistance is 1.60×10 6 Ω·cm, the initial value of the charge amount was -47.9 μC / g, the charge maintenance rate was 83.6%, and the charge maintenance rate of the humidified sample was 80.4%.
[0118] Table 1 shows the neutralization pH and reaction temperature of step B when preparing each sample, the alkaline solution used, the sodium content and sulfur content at the end of cleaning in step C, the calcination atmosphere and calcination temperature of step D, and the characteristic values of each sample obtained (niobium content, sodium content, potassium content, alkali metal content, the sum of alkali metal content and sulfur content, S1 / S2, the number of pits per unit area on the particle surface, particle interface resistance, charge maintenance rate and charge maintenance rate of humidified samples).
[0119] [Table 1]
[0120]
[0121] The charge adjustment powder of the present invention has an initial value of charge of less than -30.0μC / g. Compared with the charge adjustment powder having an alkali metal content greater than 20.0mmol / kg and a sum of the alkali metal content and the sulfur content greater than 35.0mmol / kg, the particle interface resistance and the charge maintenance rate are large. It can be seen that the charge adjustment powder of the present invention has an excellent ability to control the charge within a constant range and maintain the charged charge. Furthermore, the charge maintenance rate is large even after exposure to high humidity, so it can be seen that the charge adjustment powder of the present invention has an excellent ability to maintain the charged charge in an environment with high humidity.
Claims
1. A powder for charge adjustment, which is formed by particles having titanium niobium oxide on at least a part of the surface of a core material, The core material is titanium dioxide, The content of alkali metal in the charge adjustment powder is 8.0 mmol / kg or less relative to the whole powder. The sum of the alkali metal content and the sulfur content is 30.2 mmol / kg or less relative to the whole. When observed using a scanning electron microscope at a magnification of 50,000 times, pits were confirmed on at least a portion of the surface of the particles constituting the powder. When observing the surface of the particles constituting the powder using a scanning electron microscope at a magnification of 50,000 times, the number of pits observed was 1 μm. 2 More than 70 on the particle surface, When the surface area per 1 g measured by the BET method is defined as S1 and the surface area per 1 g calculated from the volume-based median diameter obtained by observation with a scanning electron microscope is defined as S2, S1 / S2 is 1.15 or more.
2. The powder for charge adjustment according to claim 1, wherein The content of niobium is 15.0 mmol / kg or more and 225.0 mmol / kg or less based on the total amount.
3. A method for producing a powder for charge adjustment according to claim 1 or 2, characterized in that: It has the following processes A~D: A: A process of dispersing the powder to be the core material in water to obtain a suspension of the core material; B: adding an acidic mixed solution of titanium salt and niobium salt and an alkaline solution to the suspension obtained in step A, neutralizing the acidic mixed solution of titanium salt and niobium salt with the alkaline solution, and precipitating titanium and niobium hydroxides on at least a portion of the surface of the core material; C: a step of removing water-soluble salts from the suspension obtained in step B and performing solid-liquid separation; D: a step of calcining the solid component obtained in step C, The alkali metal content of the solid content after washing in step C is 10.0 mmol / kg or less.
4. The method for producing a powder for charge adjustment according to claim 3, wherein: In the step B, neutralization is performed so that the pH of the suspension is 1.0 or more and 6.0 or less.
5. The method for producing a powder for charge adjustment according to claim 3, wherein: In the step B, an acidic mixed solution of titanium salt and niobium salt and an alkaline solution are added simultaneously.
6. The method for producing a charge-adjusting powder according to claim 3, wherein: The step D includes the step of calcining the solid component at 250° C. or higher and 900° C. or lower in an air atmosphere, an inert atmosphere, a reducing atmosphere, or an atmosphere having an oxygen concentration lower than that of the air.