Glass composition for sealing organic light emitting display device
By using a mixture of crystalline glass and amorphous glass in a sealed organic light emitting display device and adjusting its composition to match the thermal expansion coefficient of the substrate, the adhesion and crack problems caused by ceramic fillers are solved, and higher seal strength and protection effect are achieved .
Patent Information
- Application Number
- CN202110570755.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-19
- Filing Date
- 2021-05-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-05-25
AI Technical Summary
Prior art When used to seal organic light emitting display devices, differences in thermal expansion coefficients caused by ceramic fillers lead to reduced adhesion and risk of cracks, and reduced fluidity is difficult to seal.
A mixture of crystalline glass and amorphous glass is used to adjust its composition to match the thermal expansion coefficient of the substrate, and to reduce the thermal expansion coefficient through densification of the crystalline glass, improve the bonding strength and prevent cracks.
It achieves matching with the thermal expansion coefficient of the substrate, improves the adhesion and strength of the seal, prevents cracks, and effectively protects the organic light-emitting device.
Smart Images

Figure CN115108725B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a glass composition for sealing an organic light-emitting display device, and more particularly, to a glass composition for sealing an organic light-emitting display device comprising crystallized glass and amorphous glass. Background Art
[0002] An organic light emitting display device is a self-luminous display device that emits light by electrically exciting organic compounds. It usually has a display substrate and a packaging substrate bonded together with an organic light emitting device therebetween.
[0003] The organic light-emitting devices of the organic light-emitting display device are fragile and sensitive to moisture and air. When exposed to moisture and air, their characteristics are degraded and their lifespan is shortened. Therefore, it is very important to protect the organic light-emitting devices by sealing. For this purpose, a method of sealing between substrates by melting and bonding glass frit for sealing with laser is used.
[0004] On the other hand, the thermal expansion coefficient of the substrate is usually about 38×10 -7 / ℃, which is lower than the thermal expansion coefficient of glass frit, but this difference in thermal expansion coefficient will cause excessive stress on the bonding surface after sealing, resulting in reduced adhesion and becoming a factor that reduces the reliability of sealing. Therefore, ceramic fillers for adjusting the thermal expansion coefficient are usually added to the glass frit used for sealing.
[0005] Ceramic fillers not only overcome the difference in thermal expansion coefficient between the glass frit and the substrate by reducing the thermal expansion coefficient of the glass frit, but also play a role in preventing cracks. However, there are problems such as that when ceramic fillers are added, it is difficult to seal due to reduced fluidity, and when sintered, the ceramic fillers may protrude or pinholes may be generated, thereby reducing adhesion.
[0006] Therefore, there is still a need for a material for sealing an organic light emitting display device that has a thermal expansion coefficient similar to that of a substrate while ensuring excellent adhesion and strength and preventing cracks. Summary of the invention
[0007] Technical issues
[0008] The present invention is used to solve the above-mentioned problems of the prior art. The purpose of the present invention is to provide a glass composition for sealing, which is used to join substrates of an organic light-emitting display device and block the organic light-emitting device from the outside.
[0009] Furthermore, an object of the present invention is to provide a glass composition for sealing an organic light-emitting display device, which reduces the thermal expansion coefficient of the glass composition while improving the adhesive strength and preventing cracks.
[0010] Means of solving the problem
[0011] A glass composition for sealing an organic light-emitting display device according to an embodiment of the present invention comprises crystallized glass and amorphous glass, wherein the crystallized glass and the amorphous glass are mixed in a mass ratio of 10:90 to 50:50.
[0012] According to an embodiment of the present invention, the crystallized glass may include 10 to 25 mol% of V2O5, 5 to 20 mol% of TeO2, 5 to 15 mol% of B2O3, 30 to 50 mol% of ZnO, 10 to 20 mol% of CuO and 1 to 5 mol% of ZrO2.
[0013] According to an embodiment of the present invention, the crystallized glass may further include 0-6 mol % of Bi2O3 and 0-5 mol % of SiO2.
[0014] According to an embodiment of the present invention, the amorphous glass may include 15 to 45 mol % of V2O5, 10 to 25 mol % of TeO2, 15 to 45 mol % of ZnO, 2 to 10 mol % of CuO, and 1 to 8 mol % of ZrO2.
[0015] According to one embodiment of the present invention, the amorphous glass may further include 0-6 mol% of Bi2O3, 0-3 mol% of SiO2, 0-15 mol% of B2O3, 0-3 mol% of Al2O3 and 0-7 mol% of Nb2O5.
[0016] According to one embodiment of the present invention, the thermal expansion coefficient of the crystallized glass can be 45×10 -7 / ℃ to 60×10 -7 / ℃.
[0017] Effects of the Invention
[0018] According to an embodiment of the present invention, by including crystallized glass in a glass composition for sealing an organic light emitting display device, the thermal expansion coefficient of the glass composition can be reduced and the bonding strength can be improved.
[0019] Also, by mixing the crystallized glass and the amorphous glass, bonding between the substrates can be facilitated, so that the organic light emitting device can be blocked from the outside to protect it. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 A diagram briefly illustrating a cross section of an organic light emitting display device using a glass composition for sealing an organic light emitting display device according to an embodiment of the present invention as a sealing member.
[0021] Description of Reference Numerals
[0022] 10: Organic light-emitting display device
[0023] 11: Display substrate 12: Packaging substrate
[0024] 13: Organic light-emitting device 14: Sealing component DETAILED DESCRIPTION
[0025] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention.
[0026] In order to clearly describe the present invention, the description of parts not related to the present invention has been omitted. It should be understood that the specific shapes, structures and characteristics recorded in the specification can be changed from one embodiment to another without departing from the concept and scope of the present invention.
[0027] Therefore, the following detailed description is not to be taken in a limiting sense, and the scope of the present invention should be construed as including the scope of the claims and all equivalents thereto.
[0028] Figure 1 A diagram briefly illustrating a cross section of an organic light emitting display device using a glass composition for sealing an organic light emitting display device according to an embodiment of the present invention as a sealing member.
[0029] Reference Figure 1 , the organic light-emitting display device 10 includes: a display substrate 11 and a packaging substrate 12, facing each other; an organic light-emitting device 13, arranged between the substrates; and a sealing member 14, used to bond the display substrate 11 and the packaging substrate 12. As described above, since the organic light-emitting device 13 of the organic light-emitting display device 10 is relatively vulnerable to moisture and air, it is very important to protect the organic light-emitting device 13 by sealing between the substrates. Hereinafter, the glass composition constituting the sealing member 14 for sealing the organic light-emitting display device will be described in detail, and the above-mentioned sealing member 14 protects the organic light-emitting device 13 located between the display substrate 11 and the packaging substrate 12 by bonding between them.
[0030] The glass composition for sealing an organic light-emitting display device according to an embodiment of the present invention comprises crystallized glass and amorphous glass, which can protect the organic light-emitting device located between the substrates from the influence of moisture, oxygen, ultraviolet rays, etc. flowing in from the outside by bonding and sealing the substrates of the organic light-emitting display device.
[0031] As described above, the sealing component is usually used by adding a ceramic filler for adjusting the thermal expansion coefficient to the glass material used for sealing. However, since the crystallinity of the ceramic filler is close to 100%, there is a problem of hindering bonding by chemical reaction when joining the substrates. Therefore, in the present invention, crystallized glass is used instead of the ceramic filler to adjust the thermal expansion coefficient of the sealing component. The crystallinity of the crystallized glass is about 20 to 70%, so it can be mixed in the form of nano-sized crystals distributed in the amorphous glass, and when joining the substrates, bonding by chemical reaction can be effectively performed. In addition, cracks can be prevented by increasing the strength.
[0032] The crystallized glass contained in the glass composition for sealing according to one embodiment of the present invention has high heat resistance and excellent mechanical strength, which plays a role in reducing the thermal expansion coefficient of the entire glass composition and improving the bonding strength after sealing. Specifically, when the crystallized glass is crystallized, it is densified, that is, its density increases, and the thermal expansion coefficient decreases accordingly. Therefore, it is possible to make the substrate (thermal expansion coefficient: 40×10 -7 / °C) The thermal expansion coefficient of the glass composition to be bonded is close to that of the substrate, and when sealing, the stress between the substrate and the glass composition is reduced, thereby improving the bonding strength.
[0033] According to the present embodiment, the crystallized glass may include 10-25 mol% of V2O5, 5-20 mol% of TeO2, 5-15 mol% of B2O3, 30-50 mol% of ZnO, 10-20 mol% of CuO, 1-5 mol% of ZrO2, 0-6 mol% of Bi2O3 and 0-5 mol% of SiO2. Hereinafter, the function and preferred content of each component of the crystallized glass composition will be described in detail.
[0034] V2O5 acts as a glass former, has a low melting point characteristic, and increases the laser absorption capability. In this embodiment, the content of V2O5 is 10 to 25 mol%. If the content of V2O5 is less than 10 mol%, the low melting point effect may not be properly exerted due to the increase in the glass transition point. On the contrary, if the content of V2O5 is greater than 25 mol%, the excessive laser reactivity causes the vanadium oxide to volatilize and remain as bubbles, which causes the problem of reduced adhesion and drop strength due to such bubbles.
[0035] TeO2 improves the water resistance and chemical resistance of glass by improving the bonding strength of glass, and reduces the glass transition temperature. In this embodiment, the content of TeO2 is 5-20 mol%. If the content of TeO2 is less than 5 mol%, the effect of its addition is insufficient. On the contrary, if the content of TeO2 is greater than 20 mol%, the thermal expansion coefficient may increase significantly.
[0036] B2O3 is a glass-forming substance, which contributes to the excellent mechanical strength and durability of glass and has a low thermal expansion coefficient. In this embodiment, considering the influence of B2O3 on the glass properties, its content is set to 5 to 15 mol%.
[0037] ZnO plays a role in improving the water resistance of the glass composition, reducing the thermal expansion coefficient, and stabilizing the glass composition. In this embodiment, the content of ZnO is 30-50 mol%. If the ZnO content is less than 30 mol%, it may be difficult to manufacture the glass due to the low meltability of the glass. On the contrary, if the content is greater than 50 mol%, the transparency may be reduced due to the formation of crystals inside the glass.
[0038] CuO helps to reduce the thermal expansion coefficient and improve the infrared absorption rate of laser sealing. In this embodiment, the content of CuO is 10-20 mol%. If the content of CuO is less than 10 mol%, the effect of its addition is insufficient. If the added content is greater than 20 mol%, it may lead to a decrease in glass forming ability and an increase in thermal expansion coefficient.
[0039] ZrO2 is a component for improving chemical resistance. In this embodiment, the content of ZrO2 is 1 to 5 mol%. If the content of ZrO2 is less than 1 mol%, the effect of improving the water resistance of the glass is small. If it is greater than 5 mol%, the melting property is reduced and it is difficult to form glass.
[0040] Bi2O3 increases the refractive index and reduces the viscosity. In this embodiment, the content of Bi2O3 is 0-6 mol%. If the added content of Bi2O3 is greater than 6 mol%, the thermal expansion coefficient may increase.
[0041] SiO2 is used as a glass forming substance to help improve the stability of glass and reduce the thermal expansion coefficient. If the content of SiO2 is greater than 5 mol%, the softening point may increase, so in this embodiment, the content of SiO2 is set to 0-5 mol%.
[0042] According to one embodiment of the present invention, the thermal expansion coefficient of the crystallized glass containing the above-mentioned multiple components can be 45×10 -7 / ℃ to 60×10 -7 As described above, by making the crystallized glass have a thermal expansion coefficient close to that of the substrate, the problem of reduced adhesion and sealing reliability due to the difference in thermal expansion coefficient can be overcome.
[0043] On the other hand, in the case of using only crystallized glass, there is no softening flow, and thus the adhesion may be reduced. Therefore, in the present invention, a glass composition for sealing is composed by mixing crystallized glass with amorphous glass.
[0044] According to an embodiment of the present invention, a glass composition for sealing can be formed by mixing crystallized glass and amorphous glass in a mass ratio of 10:90 to 50:50. If the amount of crystallized glass added is greater than 50%, the fluidity of the glass mixture is sharply reduced, which may cause the airtightness of the packaging part to deteriorate. If the amount of crystallized glass added is less than 10%, it is difficult to achieve the effect of reducing the thermal expansion coefficient and improving the bonding strength.
[0045] In this embodiment, the amorphous glass may contain 15 to 45 mol% V2O5, 10 to 25 mol% TeO2, 15 to 45 mol% ZnO, 2 to 10 mol% CuO, 1 to 8 mol% ZrO2, 0 to 6 mol% Bi2O3, 0 to 3 mol% SiO2, 0 to 12 mol% B2O3, 0 to 3 mol% Al2O3 and 0 to 7 mol% Nb2O5.
[0046] The glass composition having the above composition can be prepared in the form of a paste to seal an organic light-emitting display device. Specifically, a carrier can be prepared by mixing an organic solvent such as an alcohol solvent, a ketone solvent, and an ether solvent with an organic binder such as an acrylic polymer or a cellulose polymer, and amorphous glass powder and crystallized glass powder are mixed therein at an appropriate ratio to prepare a paste. In this case, an inorganic pigment can be further contained within a range that does not reduce the physical properties of the glass and the physical properties of the coating.
[0047] Hereinafter, the characteristics of the glass composition for sealing according to one embodiment of the present invention described above will be described in detail through specific experimental examples.
[0048] Experimental example
[0049] Table 1 shows the contents of the crystallized glass compositions of the examples of the present invention. The mol% of each component is a value calculated based on the total content of the crystallized glass composition.
[0050] Table 1
[0051] Classification <![CDATA[V2O5]]> <![CDATA[Bi2O3]]> <![CDATA[TeO2]]> <![CDATA[B2O3]]> ZnO CuO <![CDATA[ZrO2]]> <![CDATA[SiO2]]> count T8h T8h Composition 1 20.0 6.0 8.0 11.0 38.5 13.5 3.0 - 100 320 417 Composition 2 18.0 3.5 8.5 14.0 40.0 14.0 2.0 - 100 318 435 Composition 3 23.0 2.0 12.0 12.5 37.5 11.0 1.0 1.0 100 317 418 Composition 4 24.0 2.0 12.5 10.0 39.5 10.0 2.0 - 100 315 419 Composition 5 21.0 3.0 18.0 11.5 31.5 13.0 2.0 - 100 319 423 Composition 6 17.5 5.0 14.0 13.0 36.0 13.0 1.5 - 100 323 444 Composition 7 16.0 - 9.5 12.0 44.0 14.0 1.5 3.0 100 340 485
[0052] Table 2 shows the contents of the amorphous glass compositions of the examples of the present invention. The mol% of each component is a value calculated based on the total content of the amorphous glass composition.
[0053] Table 2
[0054]
[0055]
[0056] Table 3 shows the characteristics according to the mixing ratio of crystallized glass and amorphous glass. Specifically, the coefficient of thermal expansion (CTE), adhesion, and drop test results according to the mixing ratio of crystallized glass and amorphous glass (based on mass ratio) are shown. Among them, the drop test is used to measure the strength, and the breakage rate and degree of detachment are measured by performing a drop test at a specified height. The adhesion measurement results are judged as 4.5kgf / cm or more for excellent, 3.5-4.5kgf / cm for general, and 3.5kgf / cm or less for insufficient. The drop test results are judged as 15% or less for excellent, 15-20% for general, and 20% or more for insufficient.
[0057] Table 3
[0058]
[0059]
[0060] Referring to Table 3, it can be confirmed that the thermal expansion coefficient decreases as the proportion of crystallized glass increases. However, when the proportion of crystallized glass is greater than 50% (Comparative Examples 1 to 3), it can be confirmed that the adhesion and drop strength decrease.
[0061] Specifically, in Examples 1 to 10, the adhesion was 4.0 kgf / cm or more, which was found to be basically excellent, whereas in Comparative Examples 1 to 3, the adhesion was 3.5 kgf / cm or less, which was found to be insufficient. Also, in Examples 1 to 10, as a result of the drop test, the breakage rate and the degree of detachment were less than 20% (most of which were less than 15%), showing very excellent strength, whereas in Comparative Examples 1 to 3, the breakage rate and the degree of detachment were more than 20%, which showed a significant decrease in strength.
[0062] On the other hand, when the proportion of crystallized glass is less than 5% (Comparative Examples 4 and 5), the adhesion is 4.5 kgf / cm or more, which is good, but as a result of the drop test, the crack and breakage rate is more than 20%, which is a significant increase. This is the result of the increase in the thermal expansion coefficient and the increase in the thermal expansion coefficient difference between the substrate and the substrate.
[0063] Considering these experimental results, it is preferable to add crystallized glass at a ratio of 10% or more and 50% or less to reduce the crack and breakage rate while having excellent adhesion.
[0064] The preferred embodiments of the present invention are described above with reference to the accompanying drawings, but those skilled in the art will appreciate that the present invention can be implemented in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above embodiments are exemplary and non-restrictive in all aspects.
Claims
1. A glass composition for sealing an organic light-emitting display device, characterized in that: Including crystal glass and amorphous glass, The crystallized glass and the amorphous glass are mixed in a mass ratio of 10:90 to 50:50, The crystallized glass comprises 10 to 25 mol% of V2O5, 5 to 20 mol% of TeO2, 5 to 15 mol% of B2O3, 30 to 50 mol% of ZnO, 10 to 20 mol% of CuO and 1 to 5 mol% of ZrO2. The amorphous glass contains 15 to 45 mol% of V2O5, 10 to 25 mol% of TeO2, 15 to 45 mol% of ZnO, 2 to 10 mol% of CuO and 1 to 8 mol% of ZrO2.
2. The glass composition for sealing an organic light-emitting display device according to claim 1, characterized in that: The above-mentioned crystallized glass further contains 0 to 6 mol% of Bi2O3 and 0 to 5 mol% of SiO2.
3. The glass composition for sealing an organic light-emitting display device according to claim 1, characterized in that: The above-mentioned amorphous glass also contains 0-6 mol% of Bi2O3, 0-3 mol% of SiO2, 0-15 mol% of B2O3, 0-3 mol% of Al2O3 and 0-7 mol% of Nb2O5.
4. The glass composition for sealing an organic light-emitting display device according to claim 1, characterized in that: The thermal expansion coefficient of the above crystallized glass is 45×10 -7 / ℃ to 60×10 -7 / ℃.