A method for simultaneously measuring the operating temperature and piezoelectric coefficient of ferroelectrics using fluorescence

Through the combination of rare earth Er3+ doped ferroelectric materials and fiber spectrometer, the working temperature and high temperature piezoelectric coefficient of the ferroelectric are measured in real time, solving the problem of measurement difficulties in complex environments, and achieving fast, convenient and low-cost Measure the effect.

CN115112262BActive Publication Date: 2024-11-22JINGDEZHEN CERAMIC UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210838903.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-16
Publication Date
2024-11-22
Estimated Expiration
2042-07-16

AI Technical Summary

Technical Problem

The prior art is difficult to measure the working temperature and high temperature piezoelectric coefficient of a ferroelectric body in real time in complex environments, and the traditional contact measurement method has problems such as complex equipment and difficulty in operation.

Method used

Using rare earth Er3+ doped ferroelectric materials, prepared by solid phase reaction and atmosphere annealing, plated with transparent electrodes for polarization, draw standard curves using fluorescence peak intensity ratio and fluorescence intensity peak, and determine green fluorescence intensity with fiber spectrometer The ratio and intensity peak value are used to determine the working temperature and piezoelectric coefficient of the ferroelectric body in real time.

Benefits of technology

It realizes the rapid, simple and cost-effective measurement of the working temperature and high-temperature piezoelectric coefficient of the ferroelectric body in complex environments, avoids the equipment complexity and operation difficulties of traditional measurement methods, and improves the accuracy and convenience of measurement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115112262B_ABST
    Figure CN115112262B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for simultaneously measuring the operating temperature and piezoelectric coefficient of a ferroelectric by using fluorescence, comprising the following steps: 1. adding rare earth Er when preparing the ferroelectric by solid phase method; 3+ , and perform component compensation and atmosphere annealing; second, plate transparent electrodes on both sides of the ferroelectric obtained in step one, and obtain a ferroelectric standard sample after polarization; third, measure the fluorescence peak intensity ratio, intensity peak and piezoelectric coefficient of the standard sample in step two; fourth, draw a standard curve 1 of peak intensity ratio and working temperature and a standard curve 2 of intensity peak and piezoelectric coefficient according to the measured value of step three; fifth, use a fiber optic spectrometer to measure the fluorescence intensity ratio and intensity peak of the ferroelectric to be tested, and find out the working temperature and piezoelectric coefficient of the ferroelectric to be tested according to standard curves 1 and 2. The present invention uses fluorescence to measure the working temperature of the ferroelectric in real time, and quickly detects the piezoelectric coefficient of the ferroelectric at different ambient temperatures. It is simple and convenient to operate, does not require a clamp and a high-temperature resistant wire, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of piezoelectric functional ceramic materials, and specifically relates to a method for simultaneously measuring the operating temperature and piezoelectric coefficient of a ferroelectric body by utilizing fluorescence. Background Art

[0002] Bismuth layered ferroelectric ceramics are a type of piezoelectric functional ceramic material suitable for high temperature environments. They are widely used in many special fields such as aerospace, nuclear energy, metallurgy, petrochemicals, geological exploration, etc. Ferroelectrics that have been polarized at high voltage have certain piezoelectricity. An important feature of bismuth layered ferroelectric ceramics is that their piezoelectric coefficient will depolarize with the increase of temperature, which will cause the piezoelectric coefficient to decay and cause the material to fail.

[0003] In recent years, the application and research of ferroelectric materials doped with rare earth elements to prepare photoluminescent materials has increased. The relevant literature reports can be found in the journal "Journal of the European Ceramic Society", 2017, Issue 2, Article Number: 10842; you can also refer to "Journal of Photochemistry and Photobiology A: Chemistry", 2019, Issue 380, Article Number: 111864. In addition, the Chinese invention patent "An upconversion luminescent transparent ferroelectric ceramic material and its preparation method and application" (Authorization Announcement No.: CN 111484326 B) reports related applications. The upconversion luminescent material with bismuth layered structure has improved chemical properties and physical stability, and has the unique electrical properties of ferroelectric materials. At the same time, the preparation process is relatively simple. It is a new multifunctional material with both electrical and optical properties.

[0004] Since the piezoelectric coefficient of ferroelectric materials will decay at high temperatures, it will lead to material failure. How to measure the working temperature and high-temperature piezoelectric coefficient of ferroelectrics in real time is an important guarantee to ensure their normal operation. Therefore, it is very important to measure the working temperature and high-temperature piezoelectric coefficient of such ferroelectrics. At present, the traditional contact measurement is generally used for the detection of the piezoelectric coefficient of ferroelectrics. However, this contact measurement method cannot meet the real-time detection in complex environments, and requires a fixture and high-temperature resistant wires, which has a series of problems such as complex equipment and difficult operation. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for simultaneously measuring the operating temperature and piezoelectric coefficient of a ferroelectric body by using fluorescence, which has stable performance, convenient operation and low cost.

[0006] In order to solve the above technical problems, the technical solution of the present invention is: a method for simultaneously measuring the operating temperature and piezoelectric coefficient of a ferroelectric using fluorescence, characterized in that it comprises the following steps:

[0007] Step 1: Weigh the original ferroelectric ingredients and add rare earth Er into them 3+ , and simultaneously carry out component compensation, carry out solid phase reaction at 1000-1200° C. for 10-20 hours to prepare a rare earth ion-doped ferroelectric material, and perform an atmosphere annealing process on the prepared ferroelectric material;

[0008] Step 2: Plating transparent electrodes on both sides of the ferroelectric material prepared in step 1, and subjecting it to a polarization process to obtain a ferroelectric standard sample;

[0009] Step 3: measuring the green fluorescence peak intensity ratio, green fluorescence intensity peak value and piezoelectric coefficient of the ferroelectric standard sample in step 2;

[0010] Step 4: based on the measured values ​​in step 3, draw a standard curve 1 of green fluorescence peak intensity ratio and working temperature and a standard curve 2 of green fluorescence intensity peak and piezoelectric coefficient;

[0011] Step 5: Add the same rare earth Er as the ferroelectric standard sample in step 1 to the ferroelectric to be tested during preparation. 3+ , and perform component compensation and atmosphere annealing, then use a fiber optic spectrometer to measure the green fluorescence intensity ratio and green fluorescence intensity peak of the ferroelectric to be tested, and find out the operating temperature and piezoelectric coefficient of the ferroelectric on the standard curves 1 and 2 in step 4 based on the fluorescence intensity ratio and fluorescence intensity peak.

[0012] The ferroelectric material is ABi2Nb2O9, and the A position is Na + , Li + 、Bi 3+ At least one of .

[0013] In the step 1, rare earth Er 3+ The ions occupy the A site and the molar ratio is not greater than 0.20.

[0014] The component compensation is to add excess Bi2O3 as Bi compensation, and the molar ratio of the compensated Bi2O3 to the Bi2O3 in the original ingredients is less than 0.05.

[0015] The annealing process is to anneal at a temperature of 800-900° C. in an oxygen atmosphere for 5-10 hours, and then naturally cool to room temperature.

[0016] The fluorescence is excited by 980nm laser to emit rare earth Er 3+ The up-conversion green fluorescence; the green fluorescence intensity ratio is 2 H 11 / 2 and4 S 3 / 2 The green fluorescence intensity ratio of the two energy levels, the peak green fluorescence intensity is 4 S 3 / 2 The peak green fluorescence intensity at the energy level.

[0017] The polarization process is to perform polarization treatment under the conditions of temperature of 100-180° C. and electric field of 10-15 kV / mm.

[0018] The numerical measurement method in step 3 is to use a quasi-static d 33 The measuring instrument and the optical fiber spectrometer are used to test the green fluorescence peak intensity ratio, green fluorescence intensity peak value and piezoelectric coefficient of the sample, with the temperature increasing by 3 to 5°C per minute and kept at the working temperature to be tested for 10 to 15 minutes.

[0019] The standard curve 1 in step 4 is obtained by plotting the green fluorescence peak intensity ratio measured in step 3 against the operating temperature one by one, with the operating temperature of the ferroelectric as the horizontal coordinate and the green fluorescence peak intensity ratio as the vertical coordinate.

[0020] The standard curve 2 in step 4 is obtained by mapping the green fluorescence intensity peak value measured in step 3 to the piezoelectric coefficient one by one, with the piezoelectric coefficient of the ferroelectric as the horizontal coordinate and the green fluorescence intensity peak value as the vertical coordinate.

[0021] Due to rare earth 3+ The green emission level 2 H 11 / 2 and 4 S 3 / 2 are thermally coupled energy levels, from these two energy levels to the ground state 4 I 15 / 2 The fluorescence emission intensity ratio of the transition is closely related to temperature. 2 H 11 / 2 → 4 I 15 / 2 and 4 S 3 / 2 → 4 I 15 / 2 The green light emission peak intensity ratio can be used to measure the operating temperature of the ferroelectric in real time.

[0022] According to JO theory, the oscillator strength parameter Ω of green light t(t=2, 4, 6) depends on parameters such as the crystal field and the distance between rare earth ions. As the temperature rises, the ferroelectric structure gradually changes from a low-symmetry ferroelectric phase to a high-symmetry paraelectric phase. The emergence of a high-symmetry phase will increase the symmetry of the crystal field, resulting in a decrease in the green light emission intensity. Since paraelectric phase ferroelectrics do not have piezoelectric properties, their piezoelectric coefficient will also decrease with increasing temperature. Therefore, after calibrating the green light intensity peak and the piezoelectric coefficient, the piezoelectric coefficient of the ferroelectric at different operating temperatures can be quickly and real-time determined by the green light intensity peak.

[0023] Compared with the prior art, the advantages of the present invention are: using fluorescence to measure the working temperature of the ferroelectric in real time, and being able to quickly detect the piezoelectric coefficient of the ferroelectric at the working temperature in a complex environment; the test operation is simple and convenient, and no fixtures and high-temperature resistant wires are required, and the overall test cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the X-ray diffraction pattern of each component ceramic in Example 1;

[0025] Figure 2 is the up-conversion fluorescence spectrum of each component ceramic in Example 1;

[0026] Figure 3 is Na in Example 1 0.5 Bi 2.5-x Er x The change of green fluorescence intensity ratio and working temperature of Nb2O9 (x=0.15) ceramics;

[0027] Figure 4 is Na in Example 1 0.5 Bi 2.5-x Er x Changes in the green fluorescence intensity peak and piezoelectric coefficient of Nb2O9 (x=0.15) ceramics;

[0028] Figure 5 is the X-ray diffraction pattern of each component ceramic in Example 2;

[0029] Figure 6 is the up-conversion fluorescence spectrum of each component ceramic in Example 2;

[0030] Figure 7 is Na in Example 2 0.45 Li 0.05 Bi 2.5-x Er x The change of green fluorescence intensity ratio and working temperature of Nb2O9 (x=0.10) ceramics;

[0031] Figure 8 is Na in Example 20.45 Li 0.05 Bi 2.5-x Er x Changes in green fluorescence intensity peak and piezoelectric coefficient of Nb2O9 (x=0.10) ceramics. DETAILED DESCRIPTION

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0033] Embodiment 1:

[0034] Example 1: Using high-purity Nb2O5, Bi2O3, Na2CO3, and Er2O3 as the original ingredients, a certain proportion of Bi2O3 is added as Bi compensation based on the content of Bi2O3 in the original ingredients, wherein the molar ratio of the compensated Bi2O3 to the Bi2O3 in the original ingredients is 0.02. Na2CO3 is prepared at 1150°C using solid phase preparation technology. 0.5 Bi 2.5-x Er x The obtained ceramic was placed in a quartz tube of a tubular resistance furnace for annealing at 800°C in an O2 atmosphere for 5 hours, and then cooled naturally to room temperature to obtain Na 0.5 Bi 2.5-x Er x Bismuth layered ferroelectric ceramics of Nb2O9 (0.05≤x≤0.20). Transparent electrodes are plated on both sides of the prepared bismuth layered ferroelectric ceramics, and polarization treatment is performed under the conditions of temperature 120°C and electric field 11kV / mm.

[0035] Figure 1 For typical Na 0.5 Bi 2.5-x Er x X-ray diffraction patterns of Nb2O9 (x=0.05, 0.10, 0.15, 0.20) ferroelectric ceramics. It can be seen from the figure that the prepared ceramics have a bismuth layered structure and an orthorhombic phase structure.

[0036] Figure 2 The visible fluorescence spectra of the above four component ceramics under 980nm laser excitation are shown in Figure 2. The two green emission peaks at 525nm and 550nm are due to 2 H 11 / 2 → 4 I 15 / 2 and 4 S 3 / 2 → 4 I 15 / 2 Caused by conversion.

[0037] The x=0.15 component ceramic with the best fluorescence intensity was selected and a quasi-static d 33 The sample was tested by a measuring instrument and a fiber optic spectrometer. The specific test method is as follows: the temperature was raised by 3°C per minute, and the temperature was kept at 300°C, 350°C, 400°C, and 450°C for 10 minutes in sequence, and the green fluorescence peak intensity ratio, green fluorescence intensity peak, and piezoelectric coefficient of the ceramic were measured. The green fluorescence intensity ratio and green fluorescence intensity peak were respectively matched with the working temperature and the piezoelectric coefficient. The results are listed in Table 1.

[0038] Table 1 shows the Na 0.5 Bi 2.5-x Er x Changes in green fluorescence intensity ratio, green fluorescence intensity peak and piezoelectric coefficient of Nb2O9 (x=0.15) ceramics

[0039] Operating temperature (°C) <![CDATA[Green light intensity ratio I 525 / I 550 > <![CDATA[Green light intensity I 550 > <![CDATA[Piezoelectric coefficient d 33 (pC / N)]]> 300 1.09 2430 20.8 350 1.20 2080 19.8 400 1.33 1560 18.5 450 1.45 910 17.0

[0040] With the ferroelectric operating temperature as the horizontal axis and the green fluorescence intensity ratio as the vertical axis, a standard curve of the operating temperature and the green fluorescence intensity ratio is drawn, as shown in Figure 3 As shown. According to the green fluorescence intensity ratio of the ceramic, the working temperature of the ferroelectric is found on the standard curve. At the same time, with the piezoelectric coefficient as the horizontal axis and the green fluorescence intensity peak as the vertical axis, a standard curve of the green fluorescence intensity peak and the piezoelectric coefficient is drawn, as shown in Figure 4 According to the peak value of the green fluorescence intensity of the ceramic, the piezoelectric coefficient d of the ferroelectric to be tested at high temperature can be found on the standard curve. 33 value.

[0041] Embodiment 2:

[0042] High-purity Nb2O5, Bi2O3, Na2CO3, Li2CO3, and Er2O3 were used as the original ingredients. A certain proportion of Bi2O3 was added as Bi compensation based on the content of Bi2O3 in the original ingredients. The molar ratio of the compensated Bi2O3 to the Bi2O3 in the original ingredients was 0.04. The solid phase preparation technology was used at 1080 o Na 0.45 Li 0.05 Bi 2.5-x Er x The obtained ceramic was placed in a quartz tube of a tubular resistance furnace for annealing at 900°C in an O2 atmosphere for 10 hours, and then cooled naturally to room temperature to obtain Na 0.45 Li 0.05 Bi 2.5-x Er xBismuth layered ferroelectric ceramics of Nb2O9 (0.05≤x≤0.20). Transparent electrodes are plated on both sides of the prepared bismuth layered ferroelectric ceramics, and polarization treatment is performed under the conditions of temperature 170°C and electric field 14kV / mm.

[0043] Figure 5 For typical Na 0.45 Li 0.05 Bi 2.5-x Er x X-ray diffraction pattern of Nb2O9 (0.05≤x≤0.20) ceramics. It can be seen from the figure that the prepared ceramics are pure bismuth layered structures and the ceramics are orthorhombic phase structures.

[0044] Figure 6 The visible fluorescence spectra of the above four component ceramics under 980nm laser excitation are shown in Figure 2. The two green emission peaks at 525nm and 550nm are due to 2 H 11 / 2 → 4 I 15 / 2 and 4 S 3 / 2 → 4 I 15 / 2 Caused by conversion.

[0045] The x=0.10 component ceramic with the best fluorescence intensity was selected and a quasi-static d 33 The sample was tested by a measuring instrument and a fiber optic spectrometer. The specific method is as follows: the temperature was raised by 5°C per minute, and kept at 300°C, 350°C, 400°C, and 450°C for 15 minutes in sequence, and the green fluorescence peak intensity ratio, green fluorescence intensity peak, and piezoelectric coefficient of the ceramic were measured. The green fluorescence intensity ratio and green fluorescence intensity peak were respectively corresponded to the working temperature and piezoelectric coefficient. The results are listed in Table 2.

[0046] Table 2 shows the Na 0.45 Li 0.05 Bi 2.5-x Er x Changes in green fluorescence intensity ratio, green fluorescence intensity peak and piezoelectric coefficient of Nb2O9 (x=0.10) ceramics

[0047] Operating temperature (°C) <![CDATA[Green light intensity ratio I 525 / I 550 > <![CDATA[Green light intensity I 550 > <![CDATA[Piezoelectric coefficient d 33 (pC / N)]]> 300 1.07 3010 27.4 350 1.16 2680 26.5 400 1.28 2150 25.3 450 1.40 1530 24.0

[0048] With the ferroelectric operating temperature as the horizontal axis and the green fluorescence intensity ratio as the vertical axis, a standard curve of temperature and green fluorescence intensity ratio is drawn, such as Figure 7As shown. According to the green fluorescence intensity ratio of the ceramic, the working temperature of the ferroelectric is found on the standard curve. At the same time, with the piezoelectric coefficient as the horizontal axis and the green fluorescence intensity peak as the vertical axis, a standard curve of the green fluorescence intensity peak and the piezoelectric coefficient is drawn, as shown in Figure 8 According to the peak value of the green fluorescence intensity of the ceramic, the piezoelectric coefficient d of the ferroelectric to be tested at high temperature can be found on the standard curve. 33 The introduction of Li ions can reduce the sintering temperature of ceramics, reduce the internal defects of ceramics, and effectively improve their piezoelectric coefficient and green fluorescence intensity.

Claims

1. A method for simultaneously measuring the operating temperature and piezoelectric coefficient of a ferroelectric using fluorescence, characterized in that The steps include: Step 1: Weigh the original ferroelectric ingredients and add rare earth Er into them 3+ , and simultaneously carry out component compensation, carry out solid phase reaction at 1000-1200°C for 10-20h to prepare a ferroelectric material doped with rare earth ions, and perform atmosphere annealing on the prepared ferroelectric material; Step 2: plate transparent electrodes on both sides of the ferroelectric material prepared in Step 1, and perform polarization process to obtain a ferroelectric standard sample; Step 3: measuring the green fluorescence peak intensity ratio, green fluorescence intensity peak value and piezoelectric coefficient of the ferroelectric standard sample in step 2; The numerical measurement method in step 3 is to use a quasi-static d 33 The measuring instrument and the optical fiber spectrometer are used to test the green fluorescence peak intensity ratio, green fluorescence intensity peak value and piezoelectric coefficient of the sample, and the temperature is increased by 3 to 5°C per minute and kept at the working temperature to be tested for 10 to 15 minutes; Step 4: based on the measured values ​​in step 3, draw a standard curve 1 of green fluorescence peak intensity ratio and working temperature and a standard curve 2 of green fluorescence intensity peak and piezoelectric coefficient; Step 5: Add the same rare earth Er as the ferroelectric standard sample in step 1 to the ferroelectric to be tested during preparation. 3+ , and perform component compensation and atmosphere annealing, then use a fiber optic spectrometer to measure the green fluorescence intensity ratio and green fluorescence intensity peak of the ferroelectric to be tested, and find out the operating temperature and piezoelectric coefficient of the ferroelectric on the standard curves 1 and 2 in step 4 according to the fluorescence intensity ratio and the fluorescence intensity peak; The component compensation is to add excess Bi2O3 as Bi compensation, and the molar ratio of the compensated Bi2O3 to the Bi2O3 in the original ingredients is less than 0.05; The fluorescence is excited by 980nm laser to emit rare earth Er 3+ The up-conversion green fluorescence; the green fluorescence intensity ratio is 2 H 11 / 2 and 4 S 3 / 2 The green fluorescence intensity ratio of the two energy levels, the peak green fluorescence intensity is 4 S 3 / 2 The peak green fluorescence intensity at the energy level.

2. The method according to claim 1, characterized in that: The ferroelectric material is ABi2Nb2O9, and the A position is Na + , Li + 、Bi 3+ At least one of .

3. The method according to claim 1, characterized in that: In the step 1, rare earth Er 3+ The ions occupy the A site and the molar ratio is not greater than 0.

20.

4. The method according to claim 1, characterized in that: The annealing process is to anneal at a temperature of 800-900° C. in an oxygen atmosphere for 5-10 hours, and then naturally cool to room temperature.

5. The method according to claim 1, characterized in that: The polarization process is to perform polarization treatment under the conditions of temperature of 100-180° C. and electric field of 10-15 kV / mm.

6. The method according to claim 1, characterized in that: The standard curve 1 in step 4 is obtained by plotting the green fluorescence peak intensity ratio measured in step 3 against the operating temperature one by one, with the operating temperature of the ferroelectric as the horizontal coordinate and the green fluorescence peak intensity ratio as the vertical coordinate.

7. The method according to claim 1, characterized in that: The standard curve 2 in step 4 is obtained by mapping the green fluorescence intensity peak value measured in step 3 to the piezoelectric coefficient one by one, with the piezoelectric coefficient of the ferroelectric as the horizontal coordinate and the green fluorescence intensity peak value as the vertical coordinate.