A magnetic field detector and a method for preparing the same
By covering the protein membrane protective layer on the graphene field effect transistor and coupling magnetic induction protein, the problems of high cost and insufficient sensitivity of magnetic field detection units in the prior art are solved, and a miniaturized, high-sensitivity magnetic field detector is realized, which can detect Weak magnetic field, suitable for autonomous navigation systems.
Patent Information
- Application Number
- CN202210552563.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-05-20
AI Technical Summary
The magnetic field detection unit in the existing geomagnetic navigation system is costly and inconvenient to miniaturize, and cannot effectively detect weak magnetic fields, which limits the application of autonomous navigation in complex environments.
Using graphene field effect transistors as the basic structure, the design of miniaturized and digital magnetic field detectors is realized by covering the protein membrane protective layer on the conductive channel and covalently coupling magnetic induction proteins.
It enhances the response ability of biomagnetic induction protein to magnetic field excitation signals, can detect the weakest magnetic field intensity of 10gs (1mT), realizes data acquisition with high sampling rate and multi-bit resolution, and has the advantages of miniaturization, digitization and integration.
Smart Images

Figure CN115113108B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of magnetic field detection, and more specifically to a magnetic field detector and a preparation method thereof. Background Art
[0002] The application demand of autonomous navigation and positioning technology in national defense and people's livelihood is increasing day by day. For example, in the denied environment such as natural disaster areas, the non-autonomous navigation Beidou, GPS and other signals are blocked and cannot complete the positioning, navigation and other functions. At this time, a vehicle equipped with an autonomous navigation unit is needed to complete the corresponding navigation and positioning functions.
[0003] The autonomous navigation methods currently under research and development include inertial navigation, polarized light navigation, geomagnetic navigation, etc. The changes in the geomagnetic field over a time scale of hundreds of millions of years are extremely weak, so it is a relatively good and stable map for humans to use for geomagnetic navigation. At present, the basic magnetic field detection units of the geomagnetic navigation system are mostly magnetoelectric sensors, fluxgates, proton meters, etc.
[0004] However, the above basic devices all have limitations such as high cost and difficulty in miniaturization.
[0005] Animal behavior studies have shown that animals can use the geomagnetic field for positioning and navigation. The key to animals sensing magnetic fields and using magnetic fields is the protein substance called magnetic induction protein on their retina. The biological magnetic induction proteins discovered in recent years have been proven to be widely present in various biological lineages, and they are mostly expressed in the visual system such as the biological retina. Biophysical experiments have shown that the protein polymers and complexes have obvious intrinsic magnetic moments and have ferromagnetic hysteresis loops. And through hyperfine coupling spectroscopy, it was found that the protein complex causes its spectrum to split under the geomagnetic intensity (0.35gs~0.65gs), which means that the protein substance can sense weak magnetic fields.
[0006] Inspired by this theory, there is an urgent need to develop a new path for geomagnetic detection, that is, to use biological magnetic field sensing proteins as the transducer core and combine them with biochemical sensors to develop a bionic magnetic field detection device.
[0007] At present, the academic community has reported on a microfluidic chip based on biological magnetic induction protein. The chip uses electrochemical impedance spectroscopy to detect the impedance changes caused by the spatial conformational changes of magnetic induction protein under magnetic field stimulation. However, since the protein is fixed by using redox graphene to couple the magnetic induction protein, the sensitivity and detection limit of the chip can only verify whether the biological magnetic induction protein can respond to magnetic field stimulation. Summary of the invention
[0008] The object of the present invention is to provide a magnetic field detector and a preparation method thereof, which has the advantages of digitization, miniaturization and integration.
[0009] On the one hand, the present invention provides a magnetic field detector, including a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate, a conductive channel is formed between the source and the drain, the conductive channel is graphene, the conductive channel is covered with a protein film protective layer, and a magnetic induction protein is connected to the protein film protective layer.
[0010] Furthermore, the protein membrane protective layer is formed by heating and denaturing a bovine serum albumin solution at 70-100°C.
[0011] Furthermore, the magnetic induction protein is MagR, Cry or a complex of MagR and Cry.
[0012] Furthermore, the gate includes a first gate and a second gate, the first gate is configured to modulate the charge of the conductive channel, and the second gate is configured to monitor the voltage of the first gate.
[0013] Another aspect of the present invention provides a method for preparing a magnetic field detector, comprising the following steps:
[0014] S1: preparing a substrate and sputtering a metal on the substrate to obtain a substrate, wherein the substrate comprises a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate;
[0015] S2: transferring graphene onto the substrate;
[0016] S3: covering the graphene with a protein film protective layer;
[0017] S4: patterning a conductive channel on the substrate, and etching away excess graphene and protein film protective layers to obtain a conductive channel;
[0018] S5: Connecting magnetic induction protein to the protein membrane protective layer.
[0019] Furthermore, step S1 further comprises:
[0020] S11: using a silicon wafer with an oxide layer as a substrate, sequentially placing it in standard cleaning liquid pools I to III for cleaning, and then thermally baking to remove water vapor;
[0021] S12: placing the substrate on a coating machine and spin coating the substrate with positive photoresist at a standard rotation speed;
[0022] S13: placing the coated substrate on a hot plate and baking it at 105° C. for 8 minutes;
[0023] S14: exposing the substrate so that the pattern of the exposed area of the positive photoresist is the same as the pattern of the gate, source and drain;
[0024] S15: developing in a corresponding alkaline developer to wash away the positive photoresist in the exposed area;
[0025] S16: using an indium tin alloy target, sputtering titanium and copper onto the substrate at 600-800° C. with a DC power of 200-400 W and an argon gas flow rate of 100-200 sccm;
[0026] S17: placing the metal substrate into a degumming solution, placing the degumming solution on a hot plate at 80°C, and degumming for 1 to 2 hours to obtain a substrate, wherein the substrate includes a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate.
[0027] Furthermore, in step S2, the graphene is transferred to the substrate by using a graphene wet transfer technique.
[0028] Furthermore, step S3 includes placing the substrate on a coating machine, rotating it at a speed of 500rpm to 1000rpm, and then slowly pouring a 0.1g / ml bovine serum protein solution on the substrate. After the bovine serum protein solution is evenly spread on the surface of the substrate, the substrate is removed and placed on a hot plate at 70 to 100°C to denature the protein solution into a film, thereby forming the protein film protective layer.
[0029] Furthermore, step S4 further comprises:
[0030] S41: placing the substrate on a coating machine and spin coating the substrate with positive photoresist at a standard rotation speed;
[0031] S42: baking the substrate on a hot plate at 80° C. to 105° C. for 5 to 8 minutes;
[0032] S43: performing patterning of the conductive channel under a photolithography machine, wherein the exposure area is an area outside the conductive channel area, and the conductive channel area is shielded from light;
[0033] S44: removing the positive photoresist in the exposed area in an alkaline developer to wash out the pattern of the conductive channel;
[0034] S45: performing plasma etching using oxygen as etching gas;
[0035] S46: Use a photoresist coating machine to coat the photoresist as an insulating protective layer.
[0036] Furthermore, step S5 includes: mixing EDC solution, NHS solution and MagR / Cry solution into a mixed solution in a volume ratio of 1:1:2, using a pipette to take 20 to 100 ul and drip it on the protein film protective layer in the conductive channel area of the substrate, and then placing the substrate in an incubation box and incubating it at 37°C in a moist dark environment for 1 to 2 hours, after the incubation is completed, rinsing the unbound MagR / Cry protein complex with a phosphate buffer solution, and finally blocking the excess reactive groups on the graphene surface with a 1% bovine serum albumin solution for 1 to 2 hours.
[0037] The magnetic field detector and its preparation method of the present invention use graphene field effect transistor as the basic structure, cover the conductive channel with a protein film protective layer, and then connect the magnetic induction protein with the protein protective film covered on the graphene by covalent coupling. Compared with redox graphene, its conductivity is higher; the charge transfer of the magnetic induction protein in response to the magnetic field is detected by the conductive channel, thereby improving the sensitivity of magnetic field detection. The present invention has the advantages of miniaturization, digitization and integration, which can enhance the response of the biological magnetic induction protein to the magnetic field excitation signal, and can realize the mapping between the magnetic induction protein and the magnetic field strength with a high sampling rate and multi-bit resolution data acquisition system, and the weakest magnetic field strength that can be detected is 10gs (1mT). BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a schematic structural diagram of a magnetic field detector according to an embodiment of the present invention;
[0039] Figure 2 for Figure 1 A cross-sectional view of
[0040] Figure 3 The figure shows the change value of the drain current of the magnetic field detector of the embodiment of the present invention and the magnetic field detector in the prior art under different static magnetic field intensities;
[0041] Figure 4 is a mapping relationship curve diagram between the drain current change rate and the static magnetic field strength of the magnetic field detector according to an embodiment of the present invention;
[0042] Figure 5 is a flow chart of a method for preparing a magnetic field detector according to another embodiment of the present invention;
[0043] Figure 6 FIG. 4 is a schematic diagram of a conductive channel processing flow according to another embodiment of the present invention. DETAILED DESCRIPTION
[0044] The preferred embodiments of the present invention are given below in conjunction with the accompanying drawings and described in detail.
[0045] like Figure 1As shown, an embodiment of the present invention provides a magnetic field detector, which uses a graphene field effect transistor as a basic structure, including a substrate 10 and a gate 20 and at least a pair of source 30 and drain 40 arranged on the substrate 10, a conductive channel 50 is formed between the source 30 and the drain 40, the conductive channel 50 is graphene, and the conductive channel 50 is covered with a protein film protective layer 60, and the protein film protective layer 60 is connected to a magnetic induction protein.
[0046] The protein membrane protective layer 60 is formed by heating a bovine serum albumin solution at a high temperature of 70-100° C. to denature it. During heating, the protein space of the bovine serum albumin solution collapses, thereby forming the protein membrane protective layer.
[0047] The magnetic sensing protein can be MagR, Cry or a complex of MagR / Cry, which can respond to magnetic field signals, and there is charge transfer during the response. The transferred charge, as a component of the source-drain current of the transistor, can be read out through the drain current, thereby realizing the detection of the magnetic field.
[0048] Specifically, carboxyl groups and the like on the surface of the protein film protective layer 60 are coupled with the magnetic induction protein to form a covalent bond, thereby connecting the two.
[0049] like Figure 2 As shown, the magnetic field detector includes 6 pairs of source electrodes 30 and drain electrodes 40, and the gate 20 includes a first gate 21 and a second gate 22. The first gate 21 redistributes the surface charge-ion interface of each conductive channel 50 through the potential thereon, thereby modulating the charge of the conductive channel; the second gate 22 is used to monitor the voltage of the first gate 21 to ensure that the voltage applied to the first gate 21 is the output voltage of the voltage source. In addition, the conductive channel 50 and the protein film protective layer 60 thereon are both in a wet or liquid environment, thereby, the capacitance effect of the solid-liquid interface can be modulated by the gate 20, thereby significantly modulating the carrier concentration of the graphene, so that the magnetic field detector of the present invention has the ability to amplify signals.
[0050] Since the basic structure of a transistor is a source-drain electrode, a gate and a conductive channel, the first gate 21 can form six independent transistors with six pairs of source electrodes 30 and drain electrodes 40 respectively. The first gate 21 can simultaneously perform voltage modulation on the channel current between all source and drain electrodes, and the modulation effect is the same. In this way, the six transistors can simultaneously act on the error analysis of the signal. That is to say, when the magnetic field detector is working, it is equivalent to six transistors working at the same time.
[0051] In this embodiment, the magnetic field detection device is 10-15 mm long and 8-12 mm wide. The substrate used is a silicon wafer with a 300 nm oxide layer SiO2. The source, drain and gate heights are 50-150 um. The length L of the conductive channel 50 is 100-2000 um and the width W is 50-250 um. As a two-dimensional material, graphene has a thickness of only one atomic layer. The length L1 of the second gate 22 is 1500-3000 um and the width W1 is 50-100 um. The distance D between the first gate 21 and the conductive channel 50 is 100-2000 um. The spacing d between each transistor is between 150-500 um.
[0052] The method of using the magnetic field detector of the present invention is as follows:
[0053] It is placed in a magnetic shielding shell made of iron-nickel alloy, and a small hole is opened on the shell to expose the conductive channel 50. When in use, only the conductive channel 50 is exposed to the magnetic field, and the rest is shielded by the static magnetic field provided by the magnetic shielding shell. The magnetic field detector is located perpendicular to the direction of the static magnetic field, and the static magnetic field is provided by a solenoid with current flowing through it. A modulation voltage is applied to the first grid 21, and the source 30 and drain 40 ports are connected to a data acquisition card. The data acquisition card applies a current between the source and drain, and the static magnetic field strength is changed by adjusting the current on the solenoid. Then, the data acquisition card collects the drain current modulated by the voltage of the first grid 21 under different static magnetic field strengths, such as Figure 3 As shown, the magnetic field detector with fixed magnetic induction protein (i.e., the detector of the present invention) will change the drain current under different static magnetic field strengths, while the magnetic field detector without fixed magnetic induction protein (i.e., the existing detector) will not change the current under different static magnetic field strengths. The collected drain current data is transmitted to a computer terminal for data processing between static magnetic field strength and drain current, and the mapping relationship between static magnetic field strength and drain current change rate is obtained, as shown in FIG. Figure 4 As shown, the drain current change rate is (Ids-Io) / Io, Ids is the drain current under a certain magnetic field, and Io is the drain current without a magnetic field. Then the magnetic field detector is placed in the environment to be detected, and the magnetic field strength can be calculated by comparing the drain current output by it with the mapping relationship obtained above, which is the magnetic field strength of the environment to be detected.
[0054] The magnetic field detector of the embodiment of the present invention uses a graphene field effect transistor as the basic structure, covers a protein film protective layer 60 on the conductive channel 50, and then connects the magnetic induction protein to the protein protective film 60 by covalent coupling. Compared with redox graphene, it has higher conductivity, and uses the conductive channel 50 to detect the charge transfer of the magnetic induction protein in response to the magnetic field, thereby improving the sensitivity of magnetic field detection. The present invention has the advantages of miniaturization, digitization and integration, which can enhance the response of the biological magnetic induction protein to the magnetic field excitation signal, and can realize the mapping between the magnetic induction protein and the magnetic field strength with a high sampling rate and multi-bit resolution data acquisition system, and the weakest magnetic field strength that can be detected is 10gs (1mT).
[0055] like Figure 5 As shown, another embodiment of the present invention provides a method for preparing a magnetic field detector, comprising the following steps:
[0056] S1: preparing a substrate 10 and sputtering a metal on the substrate to obtain a substrate, wherein the substrate comprises a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate;
[0057] S1 specifically includes:
[0058] S11: Substrate preparation: Use a silicon wafer with an oxide layer as the substrate, place it in standard cleaning solution pools I to III for cleaning, and then heat-bake to remove water vapor;
[0059] S12: Glue coating: The substrate silicon wafer is placed on a glue coating machine and spin-coated with positive photoresist at a standard speed;
[0060] S13: Pre-baking: placing the coated substrate on a hot plate and baking it at 105°C for 8 minutes;
[0061] S14: Exposure: exposing the substrate so that the pattern of the exposed area of the positive photoresist is the same as the pattern of the gate, source and drain;
[0062] S15: Development: developing in a corresponding alkaline developer to wash away the positive photoresist in the exposed area;
[0063] S16: Metal sputtering: sputtering Ti / Au (50 / 100 nm) using an indium-tin alloy target at 200-400 W DC power and 100-200 sccm argon gas at 600-800°C;
[0064] S17: Stripping: Place the metal substrate into RemoverPG degumming solution, place the degumming solution on a hot plate at 80°C, and degumming for 1 to 2 hours to obtain a substrate, which includes a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate.
[0065] S2: transfer graphene to substrate;
[0066] In this embodiment, the graphene wet transfer technology is used to transfer the graphene to the substrate, including:
[0067] Cut the copper-based graphene into the required size, place it in a 0.2g / ml~1g / ml ammonium persulfate solution to corrode the copper substrate for 2~3 hours; after the copper substrate is completely corroded, use a glass slide to transfer it to 2 boxes of deionized water in turn; then use a transistor to scoop the graphene to the middle of the metal source / drain; after naturally draining the water for 3~8 hours, place it in an 80℃~105℃ oven and bake it for 30~60 minutes to make the graphene and the indium tin oxide surface completely adhere to each other; at this time, there is still a layer of photoresist on the graphene surface to protect the graphene surface from contamination, and it is necessary to use acetone and other organic solutions to remove this protective glue, prepare three boxes of clean acetone, and soak the electrode with the transferred graphene in each box of acetone for 8~10 minutes in turn to remove the glue; then use anhydrous ethanol to clean off the acetone remaining on the electrode; finally, use deionized water to remove the residual ethanol.
[0068] S3: Covering the graphene with a protein film protective layer;
[0069] Specifically, prepare a 0.1g / ml bovine serum albumin solution, place the substrate on a gel-spinning machine, rotate it at a low speed (500rpm~1000rpm), then slowly pour the bovine serum albumin solution, wait for the protein solution to be evenly spread on the surface of the substrate, remove the substrate, and place it on a 70~100℃ hot plate to denature the protein into a film, thereby forming a protein film protective layer.
[0070] S4: patterning a conductive channel on the substrate, and etching away excess graphene and protein film protective layers to obtain a conductive channel 50;
[0071] Step S4 further comprises:
[0072] S41: Glue coating: Place the device on a glue spreader and spin coat positive photoresist at a standard speed;
[0073] S42: Pre-baking: baking on a hot plate at 80°C to 105°C for 5 to 8 minutes;
[0074] S43: Exposure: Patterning of the conductive channel is performed under a photolithography machine, and the exposure area is the area outside the conductive channel area, and the conductive channel area is shielded from light;
[0075] S44: Development: removing the positive photoresist in the exposed area in an alkaline developer to wash out the pattern of the conductive channel;
[0076] The alkaline developer dissolves the exposed positive photoresist. The basic components of photoresist are polymer photosensitive resin, sensitizer and organic solvent. During the exposure process, the long-chain molecules in the exposed area break down and become shorter under the action of light, while the resin molecular chains in the unexposed area are longer than those in the exposed area. The solubility of the two in alkaline (the developer of positive photoresist is generally alkaline) developer and the difference in dissolution rate result in the photoresist in the exposed area being completely dissolved in the developer within a certain period of time, while the photoresist in the unexposed area is retained due to its slow dissolution rate.
[0077] S45: plasma etching: plasma etching is performed using oxygen as etching gas;
[0078] In step S45, the graphene and protein film protective layers outside the conductive channel are etched away. In the exposure stage, the conductive channel area is shielded from light, while the portion outside the conductive channel is exposed, so that the photoresist outside the conductive channel is dissolved by the developer, leaving only the photoresist on the conductive channel. When the oxygen plasma bombards the substrate, the high-energy ions on the conductive channel will not hit the graphene and protein film protective layers protected by the photoresist due to the blocking of the photoresist, while the portion outside the conductive channel is not protected by the photoresist because the photoresist is developed, and thus is bombarded and removed by the high-energy ions.
[0079] S46: Use a coating machine to coat photoresist such as PI, SU-8, etc. as an insulating protective layer.
[0080] like Figure 5 As shown, the step S46 further includes: after coating the photoresist as the insulating protective layer, performing exposure and stripping to remove the insulating protective layer at the conductive channel region and the positive photoresist covering the protein film protective layer.
[0081] S5: Connecting magnetic induction protein to the protein membrane protective layer 60 .
[0082] S5 includes: preparing 0.1mol / L MES (2-(N-morpholino)ethanesulfonic acid) solution, 0.5mol / L EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride) solution, 0.1mol / L NHS (N-hydroxysuccinimide) solution, wherein the MES solution solvent is deionized water, so that the solution has a suitable pH value and the concentration of the reactants participating in the covalent coupling is equivalent, which is more conducive to the coupling efficiency; the solvent of the EDC and NHS solutions is the MES solution. In this embodiment, the magnetic induction protein is a mixture of MagR and Cry, specifically, a MagR / Cry protein solution (0.25mg / ml to 1mg / ml) in a solution state is prepared. EDC solution, NHS solution and MagR / Cry solution are mixed into a mixed solution in a volume ratio of 1:1:2, and 20-100 ul is taken by a pipette and dropped on the protein film protection in the conductive channel area of the substrate, and then the substrate is placed in an incubation box and incubated at 37°C in a moist dark environment for 1-2 hours, so that the -OH groups exposed in the protein film protection layer 60 are connected to the magnetic sensing protein through incubation. Figure 6 As shown; after the incubation is completed, the unbound MagR / Cry protein complex is washed away with a phosphate buffer, and finally, the excess reactive groups on the graphene surface are blocked with a 1% bovine serum albumin solution for 1 to 2 hours; thus, the magnetic field detector is prepared.
[0083] The method for preparing a magnetic field detector provided in an embodiment of the present invention covers graphene with a protein film protective layer, couples a magnetic induction protein to the protein film protective layer, and fixes the magnetic induction protein on the protein film protective layer, thereby enabling the magnetic field detector to have a magnetic field detection function.
[0084] The above is only a preferred embodiment of the present invention, and is not intended to limit the scope of the present invention. The above embodiment of the present invention can also be modified in various ways. That is, all simple, equivalent changes and modifications made according to the claims and the description of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.
Claims
1. A magnetic field detector, characterized in that: The invention comprises a substrate, a gate and at least one pair of source and drain electrodes arranged on the substrate, a conductive channel is formed between the source and the drain electrodes, the conductive channel is graphene, the conductive channel is covered with a protein film protective layer, a magnetic induction protein is connected to the protein film protective layer, the protein film protective layer is coupled with the magnetic induction protein to form a covalent bond, so that the protein film protective layer and the magnetic induction protein are connected to each other.
2. The magnetic field detector according to claim 1, characterized in that: The protein membrane protective layer is formed by heating and denaturing a bovine serum albumin solution at 70-100°C.
3. The magnetic field detector according to claim 1, characterized in that: The magnetic induction protein is MagR, Cry or a complex of MagR and Cry.
4. The magnetic field detector according to claim 1, characterized in that: The gate includes a first gate and a second gate, the first gate is configured to modulate the charge of the conductive channel, and the second gate is configured to monitor the voltage of the first gate.
5. A method for preparing a magnetic field detector, characterized in that: The following steps are involved: S1: preparing a substrate and sputtering a metal on the substrate to obtain a substrate, wherein the substrate comprises a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate; S2: transferring graphene onto the substrate; S3: covering the graphene with a protein film protective layer; S4: patterning a conductive channel on the substrate, and etching away excess graphene and protein film protective layers to obtain a conductive channel; S5: connecting a magnetic induction protein to the protein membrane protective layer; wherein the protein membrane protective layer is coupled to the magnetic induction protein to form a covalent bond, so that the protein membrane protective layer and the magnetic induction protein are connected to each other.
6. The method for preparing a magnetic field detector according to claim 5, characterized in that: Step S1 further comprises: S11: using a silicon wafer with an oxide layer as a substrate, sequentially placing it in standard cleaning solution pools I to III for cleaning, and then thermally baking to remove water vapor; S12: placing the substrate on a coating machine and spin coating the substrate with positive photoresist at a standard rotation speed; S13: placing the coated substrate on a hot plate and baking it at 105° C. for 8 minutes; S14: exposing the substrate so that the pattern of the exposed area of the positive photoresist is the same as the pattern of the gate, source and drain; S15: developing in a corresponding alkaline developer to wash away the positive photoresist in the exposed area; S16: using an indium tin alloy target, sputtering titanium and copper onto the substrate at 600-800° C. with a DC power of 200-400 W and an argon gas flow rate of 100-200 sccm; S17: placing the metal substrate into a degumming solution, placing the degumming solution on a hot plate at 80°C, and degumming for 1 to 2 hours to obtain a substrate, wherein the substrate includes a substrate and a gate and at least one pair of source and drain electrodes arranged on the substrate.
7. The method for preparing a magnetic field detector according to claim 5, characterized in that: In step S2, graphene is transferred to the substrate by using a graphene wet transfer technique.
8. The method for preparing a magnetic field detector according to claim 5, characterized in that: Step S3 includes placing the substrate on a coating machine, rotating it at a speed of 500 rpm to 1000 rpm, and then slowly pouring a 0.1 g / ml bovine serum protein solution on the substrate. After the bovine serum protein solution is evenly spread on the surface of the substrate, the substrate is removed and placed on a hot plate at 70 to 100° C. to denature the protein solution into a film, thereby forming the protein film protective layer.
9. The method for preparing a magnetic field detector according to claim 5, characterized in that: Step S4 further comprises: S41: placing the substrate on a coating machine and spin coating the substrate with positive photoresist at a standard rotation speed; S42: baking the substrate on a hot plate at 80° C. to 105° C. for 5 to 8 minutes; S43: performing patterning of the conductive channel under a photolithography machine, wherein the exposure area is an area outside the conductive channel area, and the conductive channel area is shielded from light; S44: removing the positive photoresist in the exposed area in an alkaline developer to wash out the pattern of the conductive channel; S45: performing plasma etching using oxygen as etching gas; S46: Use a photoresist coating machine to coat the photoresist as an insulating protective layer.
10. The method for preparing a magnetic field detector according to claim 5, characterized in that: Step S5 includes: mixing EDC solution, NHS solution and MagR / Cry solution into a mixed solution in a volume ratio of 1:1:2, using a pipette to take 20-100 ul and drip it on the protein film protective layer in the conductive channel area of the substrate, and then placing the substrate in an incubation box and incubating it at 37°C in a moist dark environment for 1-2 hours, and after the incubation is completed, rinsing the unbound MagR / Cry protein complex with a phosphate buffer solution, and finally blocking the excess reactive groups on the graphene surface with a 1% bovine serum albumin solution for 1-2 hours.