A method for improving the peel strength and flexibility of negative electrode sheets of PAA system
By optimizing the negative electrode slurry formula and process, the peeling strength and flexibility of the PAA system negative electrode sheet are improved, the problems of cracking and edge powder loss during coating are solved, and the processing efficiency and performance of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202210811359.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-11
AI Technical Summary
The PAA system negative electrode sheet has low peeling strength and is prone to cracking during the coating process. The electrode sheet has poor flexibility, resulting in serious powder loss from the edges during processing.
By optimizing the formula and process of the negative electrode slurry, water-based binder A, water-based binder B and dispersion aids are added to form a synergistic effect and improve bonding performance and flexibility. The slurry is adjusted by using a mixer for multiple stirring and scraping steps. Viscosity, solid content and vacuum degree are controlled, and nanometer ultra-fine carbon powder and graphite are used to form a conductive network.
It improves the peel strength and flexibility of the negative electrode sheet, solves the problems of cracking and edge powder loss during coating, improves the yield and production efficiency of rolling, laser cutting, winding and hot pressing, and reduces the amount of conductive agent , enhancing the cycle and high-temperature performance of lithium-ion batteries.
Smart Images

Figure BDA0003739288610000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery pole pieces, and in particular relates to a method for improving the peeling strength and flexibility of a negative pole piece of a PAA system. Background Art
[0002] Compared with lead-acid batteries, nickel-metal hydride batteries, and nickel-cadmium batteries, lithium-ion batteries have the advantages of higher energy density, low self-discharge, and long cycle life. They are currently widely used in the fields of consumer electronics and power batteries. At present, lithium-ion battery slurries generally use fluorinated polymers such as polyvinylidene fluoride as binders. However, since organic solvents are easy to cause environmental pollution and harm the health of operators, it is necessary to increase the cost investment to recover the organic solvents during the coating and drying process. At the same time, the cost of NMP is relatively high, which increases the production cost of the battery. Therefore, people have studied and developed water-based binder systems. The use of water-based systems can avoid environmental pollution and reduce production costs.
[0003] SBR water-based binder uses water as the dispersion medium for negative electrode powder materials. It is environmentally friendly, pollution-free, and harmless to production operators. However, due to the limitations of the chemical properties of SBR material components, the comprehensive battery performance of SBR as a binder for negative electrode powder materials of lithium-ion batteries can no longer meet the application requirements of increasingly improved battery quality.
[0004] The advantages of PAA water-based binder system compared with SBR water-based binder system are as follows:
[0005] 1. Storage stability: When the ambient temperature drops below freezing, PAA will freeze and solidify. Unlike SBR emulsion, PAA water-based binder will not demulsify and fail. When the ambient temperature rises above freezing, it can regain fluidity and its performance remains unchanged.
[0006] 2. Stable electrochemical performance: PAA can maintain stable electrochemical performance within the voltage range of 2V to 7V.
[0007] 3. Good rate performance. The 1C capacity of PAA system battery is more than 92% of the 0.1C capacity. However, for SBR system battery, the 1C capacity is only about 85% of the 0.1C capacity.
[0008] Based on the above advantages, most domestic battery manufacturing plants give priority to the PAA system. However, during the processing of the PAA system, there will be obvious cracking at the edges after coating and drying, the electrode peeling strength is low, and the edges will suffer from severe powder loss after winding. Summary of the invention
[0009] The purpose of the present invention is to overcome the shortcomings of the existing PAA system negative electrode sheet, such as low peeling strength, easy cracking during the coating process, and poor flexibility of the electrode sheet, and to provide a method for improving the peeling strength and flexibility of the PAA system negative electrode sheet.
[0010] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0011] A method for improving the peel strength and flexibility of a PAA system negative electrode sheet, wherein the PAA system negative electrode sheet comprises a negative electrode current collector and a negative electrode slurry, wherein the negative electrode slurry comprises a negative electrode active material, an aqueous binder A, an aqueous binder B, a conductive agent, a dispersing aid and a solvent;
[0012] The preparation process of the negative electrode slurry comprises the following steps:
[0013] S1. The negative electrode active material, aqueous binder A, and conductive agent are placed in a mixer;
[0014] S2. First forward stirring: set the mixer parameters, stirring speed 10 rpm, dispersion speed 300 rpm, time 10 min, control temperature 30 ° C, do not open the vacuum;
[0015] S3. First addition of solvent: Add the solvent to the mixer to control the solid content to 79% to 83%;
[0016] S4. Second forward stirring: set the mixer parameters, stirring speed 15rpm, dispersion speed 0rpm, time 10min, control temperature 30℃, do not open vacuum;
[0017] S5. First scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and clear the powder pipeline with a special stainless steel spoon;
[0018] S6. Adding a dispersing aid;
[0019] S7. Adding aqueous binder B;
[0020] S8. The third forward stirring: set the mixer parameters, stirring speed 22rpm, dispersion speed 0rpm, time 30min, control temperature 30℃, do not open the vacuum;
[0021] S9. Second scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel;
[0022] S10. Fourth forward stirring: set the mixer parameters, stirring speed 30 rpm, dispersion speed 0 rpm, time 30 min, control temperature 30 ° C, do not open the vacuum;
[0023] S11. Adding solvent for the second time: Add the solvent to the mixer and control the solid content to 45% to 48%;
[0024] S12. Fifth forward stirring: set the mixer parameters, stirring speed 15 rpm, dispersion speed 0 rpm, time 3 min, control temperature 30 ° C, do not open the vacuum;
[0025] S13. The sixth forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 30min, control temperature 30°C, do not open the vacuum;
[0026] S14. Scrape the bottom of the barrel: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and turn up the sediment at the bottom of the barrel;
[0027] S15. Seventh forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 45min, control temperature 30℃, control vacuum degree ≤-85Kpa;
[0028] S16. Adjust the slurry viscosity to complete the discharge.
[0029] Preferably, the negative electrode active material is graphite, and the weight ratio of the negative electrode active material, aqueous binder A, aqueous binder B, conductive agent and dispersing aid is 93-96: 1.5-3: 0.5-1: 1-1.5: 0.01-0.05.
[0030] Preferably, the aqueous binder A is sodium carboxymethyl cellulose, and the aqueous binder B is polyacrylic acid.
[0031] Preferably, the conductive agent is nano-ultrafine carbon powder, the average particle size of the nano-ultrafine carbon powder is 20nm, and the specific surface area is 35m 2 / g.
[0032] Preferably, the dispersing aid is 1,3-butanediol, and the solvent is deionized water.
[0033] Preferably, the amount of the dispersing aid is 0.5%wt to 1%wt of the negative electrode active material.
[0034] Compared with the prior art, the present invention improves the bonding performance and flexibility of the negative electrode sheet by optimizing the formula and process, solves the problem of cracking and falling off during coating, and the electrode sheet has good flexibility, thereby improving the yield rate and production efficiency of rolling, laser cutting, winding and hot pressing; the negative electrode active material graphite and the conductive agent nano-ultrafine carbon powder form a long- and short-range conductive network, improve the conductivity, and reduce the amount of the conductive agent; the aqueous binder A, the aqueous binder B and the dispersing aid produce a synergistic effect in deionized water, have slurry moisture retention during coating, and solve the problems of low peeling strength of the electrode sheet and serious edge powder falling after winding. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in conjunction with specific embodiments, but the present invention is not limited to these embodiments. It should be noted that, under the premise of not conflicting, the embodiments described below or the technical features can be arbitrarily combined to form new embodiments. In the present invention, unless otherwise specified, all parts and percentages are mass units, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, if not otherwise specified, are conventional methods in the art.
[0036] As used herein, the terms "comprising," "including," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0037] When amount, concentration, or other value or parameter is expressed as a range, preferred range, or a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing a range of "1 to 5", the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0038] Example 1
[0039] Preparation of negative electrode sheet: The negative electrode slurry is evenly coated on 8μm copper foil, then dried at 110℃, rolled, and cut into strips to make negative electrode sheets;
[0040] The negative electrode slurry comprises a negative electrode active material, an aqueous binder A, an aqueous binder B, a conductive agent, a dispersing agent and a solvent, wherein the weight ratio of the negative electrode active material, the aqueous binder A, the aqueous binder B, the conductive agent and the dispersing agent is 95:2.2:0.8:1.2:0.03;
[0041] The preparation process of the negative electrode slurry comprises the following steps:
[0042] S1. Place the negative electrode active material, aqueous binder A, and conductive agent into a 650L mixer;
[0043] S2. First forward stirring: set the mixer parameters, stirring speed 10 rpm, dispersion speed 300 rpm, time 10 min, control temperature 30 ° C, do not open the vacuum;
[0044] S3. First addition of solvent: Add the solvent to the mixer to control the solid content to 81%;
[0045] S4. Second forward stirring: set the mixer parameters, stirring speed 15rpm, dispersion speed 0rpm, time 10min, control temperature 30℃, do not open vacuum;
[0046] S5. First scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and clear the powder pipeline with a special stainless steel spoon;
[0047] S6. Adding a dispersing aid;
[0048] S7. Adding aqueous binder B;
[0049] S8. The third forward stirring: set the mixer parameters, stirring speed 22rpm, dispersion speed 0rpm, time 30min, control temperature 30℃, do not open the vacuum;
[0050] S9. Second scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel;
[0051] S10. Fourth forward stirring: set the mixer parameters, stirring speed 30 rpm, dispersion speed 0 rpm, time 30 min, control temperature 30 ° C, do not open the vacuum;
[0052] S11. Adding solvent for the second time: Add the solvent to the mixer and control the solid content to 47%;
[0053] S12. Fifth forward stirring: set the mixer parameters, stirring speed 15 rpm, dispersion speed 0 rpm, time 3 min, control temperature 30 ° C, do not open the vacuum;
[0054] S13. The sixth forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 30min, control temperature 30°C, do not open the vacuum;
[0055] S14. Scrape the bottom of the barrel: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and turn up the sediment at the bottom of the barrel;
[0056] S15. Seventh forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 45min, control temperature 30℃, control vacuum degree ≤-85Kpa;
[0057] S16. Adjust the slurry viscosity to complete the discharging;
[0058] The negative electrode active material is graphite, the aqueous binder A is sodium carboxymethyl cellulose, the aqueous binder B is polyacrylic acid, and the weight average molecular weight of the polyacrylic acid is 350,000 to 400,000; the conductive agent is nano-ultrafine carbon powder, and the average particle size of the nano-ultrafine carbon powder is 20 nm, and the specific surface area is 35 m 2 The dispersing agent is 1,3-butanediol, the amount of the dispersing agent is 0.7%wt of the negative electrode active material, and the solvent is deionized water.
[0059] Preparation of positive electrode sheet: 97% of lithium nickel cobalt manganese oxide, 1.5% of PVDF (polyvinylidene fluoride), and 1.5% of conductive carbon are mixed to make slurry, the solvent of the slurry is N-methylpyrrolidone (NMP), and the solid content of the slurry is 60%. The slurry is evenly coated on both sides of aluminum foil, and then the aluminum foil is hot rolled and compacted by a roller press to obtain a positive electrode sheet.
[0060] Preparation of lithium-ion battery: The positive electrode sheet of Example 1 and the negative electrode sheet of Example 1 are cut, stacked together with a ceramic isolation membrane, and the conductive electrode ears are welded. They are packaged in an aluminum-plastic film packaging bag, and 1 mol / L electrolyte is injected. The solute is LiPF6, and the solvent is a mixture of PC (propylene carbonate) / EC (ethylene carbonate) / DMC (dimethyl carbonate) / EP (ethyl propionate) in a volume ratio of 3:2:2:3. After packaging, the battery is dried, injected, sealed once, aged, formed, degassed, sealed twice (removing the air bag), folded, divided into volumes, aged, grouped, and capacity tested to obtain a 5Ah square soft-pack lithium battery.
[0061] Example 2
[0062] Preparation of negative electrode sheet: The negative electrode slurry is evenly coated on 8μm copper foil, then dried at 110℃, rolled, and cut into strips to make negative electrode sheets;
[0063] The negative electrode slurry comprises a negative electrode active material, an aqueous binder A, an aqueous binder B, a conductive agent, a dispersing agent and a solvent, wherein the weight ratio of the negative electrode active material, the aqueous binder A, the aqueous binder B, the conductive agent and the dispersing agent is 96:1.5:1:1:0.05;
[0064] The preparation process of the negative electrode slurry comprises the following steps:
[0065] S1. Place the negative electrode active material, aqueous binder A, and conductive agent into a 650L mixer;
[0066] S2. First forward stirring: set the mixer parameters, stirring speed 10 rpm, dispersion speed 300 rpm, time 10 min, control temperature 30 ° C, do not open the vacuum;
[0067] S3. First addition of solvent: Add the solvent to the mixer to control the solid content to 83%;
[0068] S4. Second forward stirring: set the mixer parameters, stirring speed 15rpm, dispersion speed 0rpm, time 10min, control temperature 30℃, do not open vacuum;
[0069] S5. First scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and clear the powder pipeline with a special stainless steel spoon;
[0070] S6. Adding a dispersing aid;
[0071] S7. Adding aqueous binder B;
[0072] S8. The third forward stirring: set the mixer parameters, stirring speed 22rpm, dispersion speed 0rpm, time 30min, control temperature 30℃, do not open the vacuum;
[0073] S9. Second scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel;
[0074] S10. Fourth forward stirring: set the mixer parameters, stirring speed 30 rpm, dispersion speed 0 rpm, time 30 min, control temperature 30 ° C, do not open the vacuum;
[0075] S11. Adding solvent for the second time: Add the solvent to the mixer and control the solid content to 45%;
[0076] S12. Fifth forward stirring: set the mixer parameters, stirring speed 15 rpm, dispersion speed 0 rpm, time 3 min, control temperature 30 ° C, do not open the vacuum;
[0077] S13. The sixth forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 30min, control temperature 30°C, do not open the vacuum;
[0078] S14. Scrape the bottom of the barrel: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and turn up the sediment at the bottom of the barrel;
[0079] S15. Seventh forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 45min, control temperature 30℃, control vacuum degree ≤-85Kpa;
[0080] S16. Adjust the slurry viscosity to complete the discharging;
[0081] The negative electrode active material is graphite, the aqueous binder A is sodium carboxymethyl cellulose, the aqueous binder B is polyacrylic acid, and the weight average molecular weight of the polyacrylic acid is 350,000 to 400,000; the conductive agent is nano-ultrafine carbon powder, and the average particle size of the nano-ultrafine carbon powder is 20 nm, and the specific surface area is 35 m 2 The dispersing agent is 1,3-butanediol, the amount of the dispersing agent is 1%wt of the negative electrode active material, and the solvent is deionized water.
[0082] Preparation of positive electrode sheet: the same as in Example 1.
[0083] Preparation of lithium-ion batteries: The positive electrode sheet of Example 1 and the negative electrode sheet of Example 2 are cut, stacked together with a ceramic isolation membrane, and the conductive electrode ears are welded. They are packaged in an aluminum-plastic film packaging bag, and 1 mol / L electrolyte is injected. The solute is LiPF6, and the solvent is a mixture of PC (propylene carbonate) / EC (ethylene carbonate) / DMC (dimethyl carbonate) / EP (ethyl propionate) in a volume ratio of 3:2:2:3. After packaging, the battery is dried, injected, sealed once, aged, formed, degassed, sealed twice (removing the air bag), folded, divided into volumes, aged, grouped, and capacity tested to obtain a 5Ah square soft-pack lithium battery.
[0084] Example 3
[0085] Preparation of negative electrode sheet: The negative electrode slurry is evenly coated on 8μm copper foil, then dried at 110℃, rolled, and cut into strips to make negative electrode sheets;
[0086] The negative electrode slurry comprises a negative electrode active material, an aqueous binder A, an aqueous binder B, a conductive agent, a dispersing agent and a solvent, wherein the weight ratio of the negative electrode active material, the aqueous binder A, the aqueous binder B, the conductive agent and the dispersing agent is 93:3:0.5:1.5:0.01;
[0087] The preparation process of the negative electrode slurry comprises the following steps:
[0088] S1. Place the negative electrode active material, aqueous binder A, and conductive agent into a 650L mixer;
[0089] S2. First forward stirring: set the mixer parameters, stirring speed 10 rpm, dispersion speed 300 rpm, time 10 min, control temperature 30 ° C, do not open the vacuum;
[0090] S3. First addition of solvent: Add the solvent to the mixer to control the solid content to 79%;
[0091] S4. Second forward stirring: set the mixer parameters, stirring speed 15rpm, dispersion speed 0rpm, time 10min, control temperature 30℃, do not open vacuum;
[0092] S5. First scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and clear the powder pipeline with a special stainless steel spoon;
[0093] S6. Adding a dispersing aid;
[0094] S7. Adding aqueous binder B;
[0095] S8. The third forward stirring: set the mixer parameters, stirring speed 22rpm, dispersion speed 0rpm, time 30min, control temperature 30℃, do not open the vacuum;
[0096] S9. Second scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel;
[0097] S10. Fourth forward stirring: set the mixer parameters, stirring speed 30 rpm, dispersion speed 0 rpm, time 30 min, control temperature 30 ° C, do not open the vacuum;
[0098] S11. Adding solvent for the second time: adding the solvent to the mixer to control the solid content to 48%;
[0099] S12. Fifth forward stirring: set the mixer parameters, stirring speed 15 rpm, dispersion speed 0 rpm, time 3 min, control temperature 30 ° C, do not open the vacuum;
[0100] S13. The sixth forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 30min, control temperature 30°C, do not open the vacuum;
[0101] S14. Scrape the bottom of the barrel: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and turn up the sediment at the bottom of the barrel;
[0102] S15. Seventh forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 45min, control temperature 30℃, control vacuum degree ≤-85Kpa;
[0103] S16. Adjust the slurry viscosity to complete the discharging;
[0104] The negative electrode active material is graphite, the aqueous binder A is sodium carboxymethyl cellulose, the aqueous binder B is polyacrylic acid, and the weight average molecular weight of the polyacrylic acid is 350,000 to 400,000; the conductive agent is nano-ultrafine carbon powder, and the average particle size of the nano-ultrafine carbon powder is 20 nm, and the specific surface area is 35 m 2 The dispersing agent is 1,3-butanediol, the amount of the dispersing agent is 0.5%wt of the negative electrode active material, and the solvent is deionized water.
[0105] Preparation of positive electrode sheet: the same as in Example 1.
[0106] Preparation of lithium-ion batteries: The positive electrode sheet of Example 1 and the negative electrode sheet of Example 3 are cut, stacked together with a ceramic isolation membrane, and the conductive electrode ears are welded. They are packaged in an aluminum-plastic film packaging bag, and 1 mol / L electrolyte is injected. The solute is LiPF6, and the solvent is a mixture of PC (propylene carbonate) / EC (ethylene carbonate) / DMC (dimethyl carbonate) / EP (ethyl propionate) in a volume ratio of 3:2:2:3. After packaging, the battery is dried, injected, sealed once, aged, formed, degassed, sealed twice (removing the air bag), folded, divided, aged, grouped, and capacity tested to obtain a 5Ah square soft-pack lithium battery.
[0107] Comparative Example 1
[0108] Preparation of negative electrode sheet: The difference from Example 1 is that the negative electrode slurry does not include a dispersing aid (1,3-butanediol), and the other method steps are consistent with Example 1.
[0109] Comparative Example 2
[0110] Preparation of negative electrode sheet: The difference from Example 1 is that the dispersing aid in the negative electrode slurry is ethanol, and the other method steps are consistent with Example 1.
[0111] Comparative Example 3
[0112] Preparation of negative electrode sheet: The difference from Example 1 is that the dispersing aid in the negative electrode slurry is isopropanol, and the other method steps are consistent with Example 1.
[0113] Comparative Example 4
[0114] Preparation of negative electrode sheet: The difference from Example 1 is that the dispersing aid in the negative electrode slurry is n-butanol, and the other method steps are consistent with Example 1.
[0115] Comparative Example 5
[0116] Preparation of negative electrode sheet: The difference from Example 1 is that the aqueous binder B is sodium carboxymethyl cellulose, and the other method steps are consistent with Example 1.
[0117] Comparative Example 6
[0118] Preparation of negative electrode sheet: The difference from Example 1 is that the aqueous binder A is polyacrylic acid, and the other method steps are consistent with Example 1.
[0119] Comparative Example 7
[0120] Preparation of negative electrode sheet: The difference from Example 1 is that the negative electrode active material graphite, aqueous binder A sodium carboxymethyl cellulose, aqueous binder B polyacrylic acid, conductive agent nano-ultrafine carbon powder and dispersing aid 1,3-butanediol are directly put into a 650L mixer in a weight ratio of 95:2.2:0.8:1.2:0.03;
[0121] Then, the first forward stirring was performed: the stirring machine parameters were set to 10 rpm stirring speed, 300 rpm dispersion speed, 10 min time, 30 °C temperature control, and no vacuum.
[0122] Then add deionized water as solvent;
[0123] Perform the second forward stirring: set the mixer parameters, stirring speed 15rpm, dispersion speed 0rpm, time 10min, control temperature 30℃, do not open the vacuum;
[0124] Scrape the material and shovel the bottom: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, dredge the powder pipeline with a special stainless steel spoon, and turn up the sediment at the bottom of the barrel;
[0125] The third forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 45min, control temperature 30℃, control vacuum degree ≤-85Kpa;
[0126] Finally, adjust the slurry viscosity to complete the discharge;
[0127] Test Example 1
[0128] (1) Peel strength test
[0129] The negative electrode sheets obtained in Examples 1-3 and Comparative Examples 1-7 were cut into rectangles of 20 mm in length and 10 cm in width as test pieces. The test pieces were adhered to clean stainless steel plates with 20 mm wide double-sided tape. A Shimadzu AG-X50N universal tensile tester was used to perform 180° peel stress at a speed of 50 mm / min from one end of the test piece. The test was measured 5 times, and the average value was taken as the peel strength. The results are shown in Table 1. The greater the peel strength, the better the bonding state between the electrode active material layer and the current collector.
[0130] In addition to testing the characteristics of the negative electrode sheets, the characteristics of the lithium-ion batteries prepared in Examples 1-3 and Comparative Examples 1-7 were also tested.
[0131] (2) Normal temperature cycle test: The test equipment is a Xinwei 5V20A lithium battery performance tester. At room temperature, charge to 3.65V at 1CCCCV, leave for 10 minutes, then discharge to 2.5V at 1C, leave for 10 minutes. Repeat 500 cycles and express the ratio of the discharge capacity of the 500th cycle to the first cycle as a percentage, as the capacity retention rate. The results are shown in Table 1.
[0132] (3) High temperature discharge test: At room temperature, the battery was charged to 3.65 V at a constant current and constant voltage of 1C, with a cut-off current of 0.05C. At 45°C, the battery was kept at rest for 8 h, discharged to 3.0 V at 1C, and then discharged to 2.5 V at 0.2C. The discharge capacity obtained is the high temperature discharge capacity of the battery. The results are shown in Table 1.
[0133] The performance of the lithium ion batteries of Examples 1 to 3 and Comparative Examples 1 to 7 was measured. The results are shown in Table 1.
[0134] Table 1 Performance measurement results of lithium ion batteries of Examples 1 to 3 and Comparative Examples 1 to 7
[0135]
[0136] In summary, the PAA system negative electrode sheet prepared by the specific components and method steps of the present invention has excellent bonding performance, flexibility and stability, solves the problem of cracking and falling off during coating, and the flexibility of the electrode sheet is good, thereby improving the yield and production efficiency of rolling, laser cutting, winding and hot pressing; the negative electrode active material graphite and the conductive agent nano-ultrafine carbon powder form a long- and short-range conductive network, improve the conductivity, and reduce the amount of the conductive agent; the aqueous binder A, the aqueous binder B and the dispersing aid produce a synergistic effect in the solvent deionized water, and have slurry moisture retention during coating, which solves the problem of low peeling strength of the electrode sheet and serious powder falling off at the edges after winding; further, the lithium ion battery prepared by using the negative electrode sheet has excellent cycle performance and high temperature performance.
[0137] The above embodiments are merely preferred implementations of the present invention. Any simple modification, amendment and substitution of the above embodiments based on the technical essence of the present invention shall fall within the scope of the technical solution of the present invention.
Claims
1. A method for improving the peel strength and flexibility of a PAA system negative electrode sheet, wherein the PAA system negative electrode sheet comprises a negative electrode current collector and a negative electrode slurry, characterized in that: The negative electrode slurry includes a negative electrode active material, an aqueous binder A, an aqueous binder B, a conductive agent, a dispersing aid and a solvent. The preparation process of the negative electrode slurry includes the following steps: S1. The negative electrode active material, aqueous binder A, and conductive agent are placed in a mixer; S2. First forward stirring: set the mixer parameters, stirring speed 10 rpm, dispersion speed 300 rpm, time 10 min, control temperature 30 ° C, do not open the vacuum; S3. First addition of solvent: Add the solvent into the mixer and control the solid content to 79%~83%; S4. Second forward stirring: set the mixer parameters, stirring speed 15rpm, dispersion speed 0rpm, time 10min, control temperature 30℃, do not open vacuum; S5. First scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and clear the powder pipeline with a special stainless steel spoon; S6. Adding a dispersing aid; S7. Adding aqueous binder B; S8. The third forward stirring: set the mixer parameters, stirring speed 22rpm, dispersion speed 0rpm, time 30min, control temperature 30℃, do not open the vacuum; S9. Second scraping: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel; S10. Fourth forward stirring: set the mixer parameters, stirring speed 30 rpm, dispersion speed 0 rpm, time 30 min, control temperature 30 ° C, do not open the vacuum; S11. Add solvent for the second time: add solvent into the mixer and control the solid content to 45%~48%; S12. Fifth forward stirring: set the mixer parameters, stirring speed 15 rpm, dispersion speed 0 rpm, time 3 min, control temperature 30 ° C, do not open the vacuum; S13. Sixth forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 30min, control temperature 30°C, do not open the vacuum; S14. Scrape the bottom of the barrel: scrape the sediment and dry material on the mixing paddle and barrel wall into the barrel, and turn up the sediment at the bottom of the barrel; S15. Seventh forward stirring: set the mixer parameters, stirring speed 25rpm, dispersion speed 1200rpm, time 45min, control temperature 30℃, control vacuum degree ≤-85Kpa; S16. Adjust the slurry viscosity to complete the discharging; The aqueous binder A is sodium carboxymethyl cellulose, and the aqueous binder B is polyacrylic acid.
2. A method for improving the peel strength and flexibility of a negative electrode sheet of a PAA system according to claim 1, characterized in that: The negative electrode active material is graphite, and the weight ratio of the negative electrode active material, aqueous binder A, aqueous binder B, conductive agent and dispersing aid is 93-96:1.5-3:0.5-1:1-1.5:0.01-0.
05.
3. The method for improving the peel strength and flexibility of the negative electrode sheet of the PAA system according to claim 1, characterized in that: The conductive agent is nano-ultrafine carbon powder, the average particle size of the nano-ultrafine carbon powder is 20nm, the specific surface area is 35m 2 / g.
4. The method for improving the peel strength and flexibility of the negative electrode sheet of the PAA system according to claim 1, characterized in that: The dispersing aid is 1,3-butanediol, and the solvent is deionized water.
5. A method for improving the peel strength and flexibility of a negative electrode sheet of a PAA system according to claim 4, characterized in that: The amount of the dispersing aid used is 0.5%wt~1%wt of the negative electrode active material.