Polyurethane foam for comfort applications
The problem of foam in moisture absorption, airflow and compression permanent deformation is solved by using a combination of isocyanate mixture, polymer polyol, silicone surfactant and phase change material in polyurethane foam, achieving bedding Efficient moisture-absorbing and cool touch in applications such as seats.
Patent Information
- Application Number
- CN202180011759.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-31
- Filing Date
- 2021-01-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-01-27
AI Technical Summary
The existing polyurethane foam cannot effectively conduct heat during use, resulting in local temperature rise. The high-porosity foam lacks load-bearing characteristics, while the hydrophilic foam has permanent deformation problems and cannot meet the hygroscopic, airflow and cool touch at the same time. demand.
Using a combination of isocyanate mixtures, polymer polyols, silicone surfactants and phase change materials, flexible polyurethane foams are prepared through specific reaction mixtures and processes to improve their moisture-wicking, low compression permanent deformation and airflow characteristics, and at 25 Provides a cool touch from °C to 37°C.
The good moisture-wicking, low compression permanent deformation and proper airflow characteristics of polyurethane foam in applications such as bedding and seats provide a cool touch while supporting human weight.
Smart Images

Figure GDA0004859536160000071 
Figure GDA0004859536160000081 
Figure GDA0004859536160000181
Abstract
Description
[0001] The present invention relates to flexible polyurethane foams suitable for use in comfort applications such as pillows, mattresses, mattress topper and seat cushions.
[0002] Polyurethane foams are used in very large quantities to make cushioning materials, particularly for bedding and seating. The problem with these foams is that they do not conduct heat very efficiently. As a result, the heat given off by the user is trapped by the foam in areas that are in close proximity to the user's body. This results in a local temperature rise that the user typically perceives as discomfort.
[0003] Various ways have been proposed to address this problem. Increasing the porosity of the foam so that air can move in and out of the foam more easily helps a lot. Making the foam more hydrophilic allows moisture such as sweat to be wicked away from the user's body more effectively, helping to improve comfort. So-called "gel technology" is used to impart a cool-to-the-touch sensation, which is important at the point of sale.
[0004] None of these approaches is completely satisfactory. Foams that are highly porous and have high airflow are "breathable," but may lack the necessary load-bearing properties. Hydrophilic foams tend to have poor compression set. This can cause the foam to permanently deform, sag, or form depressions during normal use. Formulation modifications that reduce compression set tend to reduce airflow. Hydrophilic foams also lack the "cool touch" characteristics that are desired at the point of sale.
[0005] Phase change materials or "gels" are often used to impart a "cool touch" characteristic. These materials have a melting or phase change temperature of about room temperature or slightly above. As the material undergoes its phase change, the material effectively absorbs body heat when touched. This creates a cool sensation when first touched.
[0006] Gels are used as surface facings or injected into foam. Gels are not breathable and therefore do not transfer heat effectively. Once the gel is heated to body temperature, the gel tends to trap heat rather than dissipate it. Gels also tend to be sticky and therefore are often encapsulated in a polymer film. This further reduces the breathability of the gel, exacerbating the problem.
[0007] There is a need for polyurethane foams that exhibit good moisture wicking and low compression set for use in bedding and other comfort applications. Ideally, the foams also exhibit high airflow and a cool feel to the touch.
[0008] In one aspect, the present invention is a flexible polyurethane foam comprising the reaction product of a reaction mixture comprising
[0009] a) an isocyanate mixture comprising
[0010] a-1) a first isocyanate functional prepolymer which is the reaction product of at least one hydroxyl terminated polymer of ethylene oxide and optionally a hydroxyl functional branching agent and / or a hydroxyl functional chain extender with an excess of diphenylmethane diisocyanate, wherein at least 50% by weight of the diphenylmethane diisocyanate is 4,4′-diphenylmethane diisocyanate;
[0011] a-2) optionally diphenylmethane diisocyanate, wherein components a-1) and a-2) together have an isocyanate content of 5 to 15 wt. % and contain 30 to 75 wt. % of ethylene oxide units, based on the combined weight of components a-1) and a-2), and components a-1) and a-2) together constitute 40 to 60 % of the total weight of the isocyanate mixture;
[0012] a-3) a second isocyanate functional prepolymer which is the reaction product of at least one hydroxyl terminated polymer of ethylene oxide and a hydroxyl functional branching agent having at least three hydroxyl groups per molecule and a hydroxyl equivalent weight of up to 250 grams / equivalent, and an excess of toluene diisocyanate; and
[0013] a-4) optionally toluene diisocyanate, wherein a-3) and a-4) together have an isocyanate content of 5% to 15% by weight and contain 30% to 75% by weight, based on the combined weight of components a-3) and a-4), of ethylene oxide units and 2% to 5% by weight, based on the combined weight of components a-3) and a-4), of residues from the hydroxy-functional branching agent; components a-3) and a-4) together constitute 40% to 60% of the total weight of the isocyanate mixture; and components a-1), a-2), a-3) and a-4) together make up the entire weight of the isocyanate mixture;
[0014] b) water;
[0015] c) at least one polymer polyol comprising polymer particles dispersed in at least one base polyol, the base polyol being a polyether having at least 50 wt% oxypropylene units and a hydroxyl equivalent weight of 500 g / equivalent to 3000 g / equivalent;
[0016] d) optionally poly(ethylene oxide) which is a homopolymer of ethylene oxide or a random and / or block copolymer of at least 80% by weight of ethylene oxide and up to 20% by weight of another alkylene oxide, the poly(ethylene oxide) having a number average molecular weight of from 400 g / mol to 1200 g / mol;
[0017] At least one of e) and f), wherein e) is at least one silicone surfactant; and f) is at least one ethylene oxide / higher alkylene oxide block copolymer containing 40 to 90 wt% of ethylene oxide units and having a number average molecular weight of 1500 to 12,000 g / mol; and optionally
[0018] g) at least one phase change material having a melting or glass transition temperature of 25° C. to 37° C. and containing no isocyanate groups or isocyanate-reactive groups;
[0019] in
[0020] i) the isocyanate mixture comprises 40% to 65% by combined weight of components ag;
[0021] ii) water comprises from 15% to 41% by weight of the combined weight of components ag;
[0022] iii) the at least one polymer polyol comprises from 8% to 20% of the combined weight of components ag, and the polymer particles comprise from 0.5% to 10% of the combined weight of components ag;
[0023] iv) when present, the poly(ethylene oxide) comprises up to 5% by combined weight of components ag;
[0024] v) the at least one silicone surfactant comprises from 0% to 3% by combined weight of components ag;
[0025] vi) the at least one ethylene oxide / higher alkylene oxide block copolymer comprises from 0% to 3% of the combined weight of components ag;
[0026] vii) the at least one phase change material comprises up to 15% by combined weight of components ag; and
[0027] viii) Component ag comprises at least 95% by weight of the reaction mixture.
[0028] The flexible polyurethane foam produced according to the present invention has an unusual combination of properties that make the foam particularly suitable for use in bedding, seating, and other "comfort" applications where the foam becomes exposed to the body heat of the human user's body and / or to water vapor evaporating from the human user's body. These properties include very low compression set, good moisture wicking behavior, and appropriate density. In a preferred embodiment, the properties also exhibit good airflow and / or non-zero latent heat in the temperature range of 25°C to 37°C. Good airflow and non-zero latent heat each produce the "cool touch" characteristic of the foam. The foam or an article containing the foam can support at least a portion of the body weight of the human user in such applications.
[0029] The present invention also provides a method for preparing a flexible polyurethane foam, the method comprising:
[0030] A. Form a reaction mixture by combining:
[0031] a) an isocyanate mixture comprising
[0032] a-1) a first isocyanate functional prepolymer which is the reaction product of at least one hydroxyl terminated polymer of ethylene oxide and optionally a hydroxyl functional branching agent and / or a hydroxyl functional chain extender with an excess of diphenylmethane diisocyanate, wherein at least 50% by weight of the diphenylmethane diisocyanate is 4,4′-diphenylmethane diisocyanate;
[0033] a-2) optionally diphenylmethane diisocyanate, wherein components a-1) and a-2) together have an isocyanate content of 5 to 15 wt. % and contain 30 to 75 wt. % of ethylene oxide units, based on the combined weight of components a-1) and a-2), and components a-1) and a-2) together constitute 40 to 60 % of the total weight of the isocyanate mixture;
[0034] a-3) a second isocyanate functional prepolymer which is the reaction product of at least one hydroxyl terminated polymer of ethylene oxide and a hydroxyl functional branching agent having at least three hydroxyl groups per molecule and a hydroxyl equivalent weight of up to 250 grams / equivalent, and an excess of toluene diisocyanate; and
[0035] a-4) optionally toluene diisocyanate, wherein a-3) and a-4) together have an isocyanate content of 5% to 15% by weight and contain 30% to 75% by weight, based on the combined weight of components a-3) and a-4), of ethylene oxide units and 2% to 5% by weight, based on the combined weight of components a-3) and a-4), of residues from the hydroxy-functional branching agent; components a-3) and a-4) together constitute 40% to 60% of the total weight of the isocyanate mixture; and components a-1), a-2), a-3) and a-4) together make up the entire weight of the isocyanate mixture;
[0036] b) water;
[0037] c) at least one polymer polyol comprising polymer particles dispersed in at least one base polyol, the base polyol being a polyether having at least 50 wt% oxypropylene units and a hydroxyl equivalent weight of 500 g / equivalent to 3000 g / equivalent;
[0038] d) optionally poly(ethylene oxide) which is a homopolymer of ethylene oxide or a random and / or block copolymer of at least 80% by weight of ethylene oxide and up to 20% by weight of another alkylene oxide, the poly(ethylene oxide) having a number average molecular weight of from 400 g / mol to 1200 g / mol;
[0039] At least one of e) and f), wherein e) is at least one silicone surfactant; and f) is at least one ethylene oxide / higher alkylene oxide block copolymer containing 40 to 90 wt% of ethylene oxide units and having a number average molecular weight of 1500 to 12,000 g / mol; and optionally
[0040] g) at least one phase change material having a melting or glass transition temperature of 25° C. to 37° C. and containing no isocyanate groups or isocyanate-reactive groups;
[0041] in
[0042] i) the isocyanate mixture comprises 40% to 65% by combined weight of components ag;
[0043] ii) water comprises from 15% to 41% by weight of the combined weight of components ag;
[0044] iii) the at least one polymer polyol comprises from 8% to 20% of the combined weight of components ag, and the polymer particles comprise from 0.5% to 10% of the combined weight of components ag;
[0045] iv) when present, the poly(ethylene oxide) comprises up to 5% by combined weight of components ag;
[0046] v) the at least one silicone surfactant comprises from 0% to 3% by combined weight of components ag;
[0047] vi) the at least one ethylene oxide / higher alkylene oxide block copolymer comprises from 0% to 3% of the combined weight of components ag;
[0048] vii) the at least one phase change material comprises up to 15% by combined weight of components ag; and
[0049] viii) component ag comprises at least 95% by weight of the reaction mixture; and
[0050] B. reacting the reaction mixture to produce the foam.
[0051] Component a-1) of the isocyanate mixture is a first isocyanate-terminated prepolymer, which is the reaction product of at least one hydroxyl-terminated polymer of ethylene oxide and optionally a hydroxyl-containing branching agent and / or chain extender with an excess of diphenylmethane diisocyanate (MDI). At least 50% by weight of the MDI is the 4,4'-isomer. In some embodiments, the 4,4'-isomer accounts for at least 60% or at least 70% of the weight of the diphenylmethane diisocyanate used to prepare the prepolymer. Up to 100% of the diphenylmethane diisocyanate can be the 4,4'-isomer. If present, the 2,4'-isomer can account for at least 5%, at least 10%, or at least 15% of the weight of the diphenylmethane diisocyanate. If present, the 2,2'-isomer can constitute up to 5% or up to 2% of the weight of the diphenylmethane diisocyanate used to prepare the prepolymer.
[0052] The polymer of ethylene oxide is preferably a hydroxyl-terminated homopolymer of ethylene oxide or a hydroxyl-terminated random or block copolymer of ethylene oxide and 1,2-propylene oxide. The polyether may contain, for example, at least 50% by weight or at least 60% by weight of ethylene oxide groups and up to 100% by weight of ethylene oxide groups. A polyether of particular interest is a poly(ethylene oxide) homopolymer. Another is a random or block copolymer of ethylene oxide and 1,2-propylene oxide containing 50% to 99%, preferably 60% to 95% of ethylene oxide groups and correspondingly 5% to 50%, preferably 5% to 40% of methylethylene oxide (propylene oxide) groups.
[0053] The polyethers may nominally contain, for example, an average number of hydroxyl groups per molecule of 2 to 4. Preferred nominal average hydroxyl functionalities are 2 to 3, and more preferred nominal average hydroxyl functionalities are 2 to 2.5 or 2 to 2.25. The nominal functionality refers to the number of alkoxylatable groups on the initiator compound used to produce the polyether(s). For purposes of the present invention, a primary amino group is considered to contain 2 alkoxylatable sites.
[0054] The hydroxyl equivalent weight of the polyether is preferably at least 300 or at least 450, and may be, for example, up to 6000, up to 3000 or up to 2000 g / equivalent. An especially preferred equivalent weight range is 500 g / equivalent to 1800 g / equivalent. All hydroxyl equivalent weights herein are determined by titration methods such as ASTM D4274-99.
[0055] A mixture of two or more polyethers as described above may be used to prepare the first isocyanate-terminated prepolymer.
[0056] The first isocyanate functional prepolymer is preferably prepared by mixing MDI with a polyether and subjecting the mixture to certain conditions under which a portion of the isocyanate groups react with the hydroxyl groups of one or more polyethers to form urethane bonds. When forming the first isocyanate functional prepolymer, a hydroxyl-containing branching agent and / or chain extender is optionally present. Such a branching agent or chain extender may have a hydroxyl equivalent weight of up to 250 or up to 125, and in the case of a branching agent, may have at least 3 (preferably 3-8, 3-6 or 3-4) hydroxyl groups per molecule, and in the case of a chain extender, may have exactly two hydroxyl groups per molecule. If these are present, then they are preferably present in an amount of up to 5, preferably up to 2 parts by weight per 100 parts by weight of the one or more polyethers.
[0057] The prepolymer forming reaction is preferably carried out at an elevated temperature (e.g., 60° C. to 180° C.) and preferably under an inert atmosphere (e.g., nitrogen, helium, or argon). An excess of isocyanate groups over hydroxyl groups is provided; in some embodiments, MDI, polyether, and optional branching agent and / or chain extender are mixed in a ratio of 0.95 to 1.5 moles, especially 0.95 to 1.25 moles of polyisocyanate per equivalent of hydroxyl groups. The reaction is generally continued until the prepolymer reaches a constant isocyanate content, which indicates that substantially all of the hydroxyl groups of the polyether have been consumed.
[0058] The first isocyanate-terminated prepolymer is preferably prepared in the substantial absence of a urethane catalyst (i.e., a catalyst for the reaction of isocyanate groups with hydroxyl groups to form a urethane). Specifically, the reaction mixture used to form the first isocyanate-functional prepolymer preferably contains no more than 1 part per million by weight of a metal and no more than 100 parts per million by weight of an amine compound. The resulting first isocyanate-terminated prepolymer correspondingly contains similarly small amounts of such materials, if present. The one or more polyethers are preferably not initiated by an amine and do not otherwise contain amine groups that exhibit activity as a urethane catalyst.
[0059] The product of the prepolymer forming reaction may include an amount of unreacted MDI, which, when present, forms all or part of component a-2 of the isocyanate mixture. If desired, the MDI may be combined separately with the first isocyanate functional prepolymer and / or other ingredients of the isocyanate mixture.
[0060] The first isocyanate functional prepolymer and any free MDI in the isocyanate mixture together have an isocyanate content of 5% to 15%, based on the combined weight of the first isocyanate functional prepolymer and free MDI. On the same basis, the isocyanate content can be at least 6% by weight or at least 7% by weight, and can be, for example, up to 12% by weight or up to 10% by weight. The isocyanate content can be determined using well-known titration methods.
[0061] The first isocyanate functional prepolymer and any free MDI in the isocyanate mixture together contain 30 wt% to 70 wt% ethylene oxide units, based on the combined weight of the first isocyanate functional prepolymer and free MDI. On the same basis, the content of ethylene oxide units can be at least 40 wt%, at least 50 wt%, or at least 55 wt%, and 70 wt% or up to 65 wt%. The percentage of ethylene oxide units is a calculated value determined using the following relationship:
[0062]
[0063] Ethylene oxide a1,a2 % is the weight percentage of ethylene oxide groups in components a-1 and a-2 of the isocyanate mixture, ethylene oxide pe % is the weight percentage of ethylene oxide groups in the polyether used to prepare the first isocyanate functional prepolymer, wt pe is the weight of the polyether used to prepare the first isocyanate functional prepolymer, wt br,ce is the weight of all branching agents and chain extenders used to prepare the first isocyanate functional prepolymer and wt MDI is the weight of MDI used to prepare the first isocyanate functional prepolymer plus any other MDI present in the isocyanate mixture.
[0064] Component a-3) of the isocyanate mixture is a second isocyanate-terminated prepolymer, which is the reaction product of at least one hydroxyl-terminated polymer of ethylene oxide and a hydroxyl-containing branching agent with an excess of toluene diisocyanate (TDI). TDI can be a 2,4-isomer, a 2,5-isomer, or a 2,6-isomer or a mixture of any two or more thereof. In some embodiments, TDI is a mixture of 50% to 85% 2,4-isomers, with the remainder being 2,6-isomers.
[0065] The hydroxyl terminated polymer of ethylene oxide is as described above in conjunction with the first isocyanate functional prepolymer.
[0066] The branching agent is generally as described for the first isocyanate functional prepolymer. The branching agent has at least 3 hydroxyl groups per molecule, and in some embodiments, has 3-8, 3-6, or 3-4 hydroxyl groups per molecule. The hydroxyl equivalent weight of the branching agent may be up to 250, up to 125, or up to 80. Examples include glycerol, trimethylolpropane, trimethylolethane, sorbitol, mannitol, sucrose, pentaerythritol, erythritol, triethanolamine, and alkoxylates of any one or more of the above having the aforementioned hydroxyl equivalent weights.
[0067] The amount of branching agent is selected so that the residues of the branching agent represent 2% to 5%, preferably 3% to 5%, of the combined weight of components a-3) and a-4). The weight of the residue is calculated from those weights of the starting materials used to prepare components a-3) and a-4), as follows:
[0068]
[0069] Where Wt br is the weight of the branching agent used to prepare component a-3), Wt pe is the weight of the polyether used to prepare component a-3), Wt ce is the weight of any chain extender used to prepare component a-3), and Wt TDI is the combined weight of TDI used to prepare component a-3) plus the weight of component a-4) (if present).
[0070] The second isocyanate functional prepolymer is conveniently prepared in a manner similar to that described above for preparing the first isocyanate functional prepolymer, with TDI replacing MDI. It is also preferred to prepare the second isocyanate-terminated prepolymer in the absence of a carbamate catalyst (i.e., a catalyst for isocyanate groups to react with hydroxyl groups to form carbamate). Specifically, the reaction mixture for forming the second isocyanate functional prepolymer preferably contains no more than 1 part per million by weight of metal and no more than 100 parts per million by weight of amine compounds. The resulting second isocyanate functional prepolymer accordingly contains a similar small amount of such substances (if present). As previously mentioned, one or more polyethers are preferably not initiated by amines, and do not contain additional amine groups that exhibit activity as carbamate catalysts.
[0071] The product of the prepolymer forming reaction may include an amount of unreacted TDI which, when present, forms all or part of component a-4 of the isocyanate mixture. If desired, TDI may be combined separately with the second isocyanate functional prepolymer and / or other ingredients of the isocyanate mixture.
[0072] The second isocyanate functional prepolymer and any free TDI in the isocyanate mixture together have an isocyanate content of 5% to 15%, based on the combined weight of the second isocyanate functional prepolymer and free TDI. On the same basis, the isocyanate content can be at least 6% by weight or at least 7% by weight, and can be, for example, up to 12% by weight or up to 10% by weight.
[0073] The second isocyanate functional prepolymer and any free TDI in the isocyanate mixture together contain 30 wt % to 70 wt % ethylene oxide units, based on the combined weight of the second isocyanate functional prepolymer and free TDI. On the same basis, the content of ethylene oxide units can be at least 40 wt % or at least 50 wt %. The percentage of ethylene oxide units is a calculated value, calculated in a manner similar to that described above, substituting the weight of TDI for the weight of MDI.
[0074] The isocyanate mixture comprises 40% to 65% of the combined weight of components ag. In some embodiments, the isocyanate mixture comprises at least 45% and up to 62.5%, up to 60%, or up to 55% of the combined weight of components ag.
[0075] Water (component b)) comprises 15%-41% of the combined weight of components ag. Water may comprise at least 17%, at least 19% or at least 20% thereof, and may comprise up to 35% or up to 30% thereof.
[0076] The polymer polyol (component c)) is a dispersion of a liquid base polyol containing polymer particles, the base polyol forming a continuous phase. Some or all of the polymer particles may be grafted to the base polyol. The polymer polyol may also include one or more stabilizers, some or all of the polymer particles may be grafted to the stabilizer.
[0077] The base polyol is one or more polyethers having a hydroxyl equivalent weight of 500 g / equivalent to 3000 g / equivalent. The hydroxyl equivalent weight may be at least 800 g / equivalent, at least 1000 g / equivalent or at least 1200 g / equivalent, and may be, for example, at most 2500 g / equivalent, at most 2000 g / equivalent or at most 1800 g / equivalent. The base polyol is a polymer or copolymer of propylene oxide containing at least 50% by weight of propylene oxide units. Homopolymers of propylene oxide and random and / or block copolymers of 50 to 99% by weight propylene oxide and 1 to 50% ethylene oxide are particularly suitable base polyols.
[0078] The nominal functionality of the base polyol may be from 2 to 6, particularly from 2 to 4, and most preferably from 2 to 3. In some cases the actual functionality may be slightly lower than the nominal functionality.
[0079] A particularly preferred type of base polyol is made by homopolymerizing propylene oxide or randomly copolymerizing 75-99.9 weight percent propylene oxide and correspondingly 0.1 to 25 weight percent ethylene oxide onto a difunctional or trifunctional initiator and optionally capping the resulting polyether with up to 30 weight percent (based on the total product weight) of ethylene oxide to form a base polyol having predominantly primary hydroxyl groups.
[0080] The dispersed polymer particles may constitute, for example, at least 1%, at least 5% or at least 10% of the total weight of the polymer polyol, and may constitute, for example, up to 60%, up to 50%, up to 40%, up to 30% or up to 20% of the total weight thereof.
[0081] In some embodiments, the dispersed polymer particles have a particle size of 100 nm to 25 μm, more typically 250 nm to 10 μm, preferably, at least 90% by volume of the dispersed polymer particles have a size within these ranges. The particle size is considered to be the diameter of a sphere with an equivalent volume. Particle size measurements can be obtained by laser diffraction methods using an apparatus such as the LX 13320 laser diffraction particle size analyzer from Beckman-Coulter.
[0082] The dispersed polymer particles can be, for example, polyureas, polyurethanes and / or polyhydrazides and / or polymers of one or more vinyl monomers. Suitable vinyl monomers include, for example, various polyolefins (such as polymers and copolymers of ethylene), various polyesters, various polyamides, various polycarbonates, various polymers and copolymers of acrylic acid and / or methacrylate, homopolymers or copolymers of styrene, homopolymers or copolymers of acrylonitrile, etc. In some embodiments, the dispersed particles are styrene-acrylonitrile copolymer particles.
[0083] At least a portion of the dispersed polymer particles are preferably grafted to at least a portion of the stabilizer and / or base polyol molecules forming the continuous phase.
[0084] Dispersions of polyurea particles can be prepared by reacting a primary or secondary amine with a polyisocyanate in the presence of a base polyol. Methods for producing polyurea dispersions are described, for example, in WO 2012 / 154831.
[0085] Dispersions of polyurethane particles can be prepared by reacting a low equivalent weight polyol or amino alcohol with a polyisocyanate in the presence of a base polyol. Methods for producing such dispersions are described in, for example, US 4,305,857, WO 94 / 20558 and WO 2012 / 154820.
[0086] Dispersions of polymerized vinyl monomers can be prepared by in-situ polymerization of such monomers in a base polyol. Such methods are described in, for example, USP 4,513,124, USP 4,588,830, USP 4,640,935, and USP 5,854,386. Alternatively, dispersions of this type can be formed in a melt dispersion process, in which a preformed vinyl polymer is melted and dispersed into the base polyol. Such methods are described in USP 6,613,827 and WO 2009 / 155427.
[0087] The polymer polyols comprise at least 8% of the combined weight of components ag. In some embodiments, the polymer polyols comprise at least 9%. One or more polymer polyols comprise up to 20% of the combined weight of components ae, and may comprise up to 18%, up to 15%, or up to 12%.
[0088] The dispersed polymer particles comprise from 0.5% to 10% of the combined weight of components ag. The dispersed polymer particles may comprise at least 1%, at least 2% or at least 4% thereof and up to 8% thereof.
[0089] The polymer polyol preferably contains no more than 5 parts per million by weight or no more than 1 part per million by weight of metals and no more than 100 parts per million of amine compounds. The one or more base polyols are preferably not initiated by an amine and do not otherwise contain amine groups that exhibit activity as a urethane catalyst.
[0090] Poly(ethylene oxide) (component d)) is a homopolymer of ethylene oxide or a random and / or block copolymer of an alkylene oxide, wherein at least 80% by weight of the alkylene oxide is ethylene oxide and up to 20% by weight is one or more other alkylene oxides. When present, the other alkylene oxides may include or be 1,2-propylene oxide. By GPC, the poly(ethylene oxide) may have a molecular weight of 400 g / mol to 1200 g / mol. The poly(ethylene oxide) preferably contains at least 1 hydroxyl group per molecule. The poly(ethylene oxide) more preferably nominally contains at least 2 hydroxyl groups per molecule and up to 6, up to 4 or up to 3 hydroxyl groups per molecule.
[0091] Useful silicone surfactants (component e)) are self-dispersible and / or water-soluble. Among useful silicone surfactants are block copolymers having at least one polysiloxane block and at least one polyether block. Such block copolymers may be, for example, AB or BAB type copolymers, wherein A represents a polysiloxane block and each B represents a polyether block. Such block copolymers may be side-grafted structures, wherein a plurality of polyether blocks depend on the polysiloxane block. Each polyether block is preferably a homopolymer or copolymer of ethylene oxide. The copolymer of ethylene oxide may be a copolymer of ethylene oxide and propylene oxide.
[0092] The silicone surfactant may contain, for example, 20 to 80 wt% polysiloxane, 20 to 75 wt% polymerized ethylene oxide, and 0 to 50 wt% polymerized propylene oxide, based on the total weight of the silicone surfactant. More preferred silicone surfactants contain 20 to 80 wt% polysiloxane, 20 to 75 wt% polymerized ethylene oxide, and 0 to 20 wt% polymerized propylene oxide. Even more preferred silicone surfactants contain 25 to 50 wt% polysiloxane, 50 to 75 wt% polymerized ethylene oxide, and 0 to 10 wt% polymerized propylene oxide.
[0093] Suitable silicone surfactants are commercially available and include, for example, those sold under the product name TRIOXIDE® by Momentive Performance Products. Water-soluble surfactants are commercially available. This includes, for example L-7002, L-7200, L-7230, L-7600, L-7604, L-7605 and L7657 surfactants.
[0094] The silicone surfactant comprises 0% to 3% of the combined weight of components ag. The silicone surfactant may comprise at least 0.5%, at least 0.75%, or at least 1%, and may comprise up to 2.5% or 2%.
[0095] Block copolymers of ethylene oxide and higher carbon alkylene oxides (component f)) contain one or more ethylene oxide blocks and one or more blocks of polymerized higher carbon alkylene oxides. The higher carbon alkylene oxide can be, for example, 1,2-propylene oxide, 1,2-butylene oxide, or a mixture thereof. Such block copolymers may contain, for example, 40% to 90% by weight of ethylene oxide units and a number average molecular weight of 1500 g / mol to 12,000 g / mol (by gel permeation chromatography with reference to polystyrene standards). Such block copolymers may have one or more hydroxyl groups, such as 1 to 4 hydroxyl groups or 2 to 4 hydroxyl groups. Examples of suitable block copolymers include those manufactured by The Dow Chemical Company under the name TergitolTM Block copolymers sold under the trade name Pluronics and by BASF as Pluronics TM Those block copolymers sold under the trade name ANTI-PROPYLENE®.
[0096] The block copolymer of ethylene oxide and a higher alkylene oxide preferably contains no more than 5 parts per million by weight or no more than 1 part per million by weight of a metal and no more than 100 parts per million of an amine compound. It is preferably not initiated by an amine.
[0097] The block copolymer of ethylene oxide and higher carbon alkylene oxide may account for 0% to 3% of the combined weight of component ag. The block copolymer of ethylene oxide and higher carbon alkylene oxide may account for at least 0.5%, at least 0.75% or at least 1%, and may account for up to 2.5% or up to 2%.
[0098] The phase change material (component g)) is one or more materials having a melting or glass transition temperature of 25°C to 37°C and containing no isocyanate groups or isocyanate reactive groups. The phase change material may be or contain, for example, any one or more of natural or synthetic waxes, such as polyethylene wax, beeswax, lanolin, carnauba wax, candelilla wax, coconut wax, sugarcane wax, jojoba wax, cuticle wax, coconut wax, petroleum wax or paraffin. The phase change material preferably has a melting temperature of 25°C to 32°C, especially 28°C to 32°C.
[0099] The phase change material is preferably not encapsulated, ie, not contained within a film or other container that forms a physical barrier between the phase change material and the remaining components of the reaction mixture.
[0100] When present, the phase change material comprises up to 15% of the combined weight of components ag. In some embodiments, the phase change material comprises at least 1%, at least 2%, or at least 2.5%, and in some embodiments, the phase change material comprises up to 12.5% or up to 10%.
[0101] In addition to components ag as described above, the reaction mixture may contain one or more optional ingredients. If present, such optional ingredients together constitute no more than 5% by weight of the reaction mixture.
[0102] Among suitable optional ingredients are one or more branching agents and / or chain extenders as previously described with respect to the preparation of the quasi-prepolymer, but these may be omitted.
[0103] The reaction mixture may also contain various ingredients such as colorants, antioxidants, preservatives, biocides, fragrances, thickeners (such as xanthan gum, various water-soluble cellulose ethers or polyacrylamides), mixing aids, wetting agents (when fillers are present), etc. If present, these preferably constitute at most 10% or at most 5% of the total weight of the reaction mixture.
[0104] The reaction mixture used to prepare the polyurethane foam is preferably substantially free of a curing catalyst, i.e., a catalyst for the reaction of isocyanate groups with water and / or alcohol groups. Specifically, the reaction mixture preferably contains no more than 5 parts per million, preferably no more than 1 part per million, by weight of a metal and no more than 100 parts per million by weight of an amine compound.
[0105] In addition to components ag, the reaction mixture may also contain one or more solid components, such as fillers and reinforcing materials. Examples of fillers include clay, diatomaceous earth, calcium carbonate, wollastonite, ground polymer particles, wood flour, cork flour, glass or other ceramic particles, and various types of natural and synthetic fibers, which may be woven, knitted or entangled as desired. Such solid components may account for up to 75% of the total weight of the reaction mixture.
[0106] The polyurethane foam is prepared by combining the ingredients to form a reaction mixture and subjecting the resulting reaction mixture to conditions under which the isocyanate-functional quasi-prepolymer and one or more of components bg react to form a flexible polyurethane foam.
[0107] Components ag may be combined in any order, but preferably the polyisocyanate mixture is added last or simultaneously with the other components to avoid premature reaction before the remaining components can be added. Thus, for example, components bg may be mixed first and the polyisocyanate mixture subsequently added. Alternatively, components ag may be combined all at once. Components be may also be formed into various sub-combinations that are combined when the polyisocyanate mixture is added. Optional ingredients that are reactive or water-soluble may be added with water or separately.
[0108] After mixing water with the polyisocyanate mixture, curing occurs spontaneously, and therefore a wide range of conditions are suitable for carrying out the reaction. The curing temperature may be as low as 0°C or as high as, for example, 100°C. Temperatures close to room temperature or slightly elevated temperatures are fully suitable and generally preferred. Thus, the curing temperature may be at least 15°C or at least 20°C and at most 50°C, at most 40°C or at most 35°C. The curing reaction produces carbon dioxide gas, which forms cells and expands the reaction mixture as curing occurs.
[0109] The curing step may be carried out in an open container, where the rising foam expands against the weight of the atmosphere and / or the weight of the film. Such a free foaming process may be carried out by dispensing the reaction mixture into a trough where it rises and cures.
[0110] The curing step may alternatively be carried out in a closed container, such as a closed mold, wherein expansion is constrained by the interior dimensions of the cavity to produce a foam having a size and shape corresponding to the size and shape of the mold cavity.
[0111] The amount of water in the reaction mixture far exceeds the amount of isocyanate groups of the polyisocyanate mixture. Because of this, the cured foam typically contains a significant amount of moisture, which may be at least partially in the form of a liquid contained in the cells of the foam. A drying step may be performed to remove some or all of this excess water.
[0112] Such a drying step can be performed, for example, by passing a drying gas through the foam, by allowing the foam to stand under a dry atmosphere, and / or by heating the foam to a temperature of, for example, 50 to 150° C. Drying can be performed until any desired moisture content is reached. In some embodiments, drying is performed until a constant foam weight is reached, indicating that all residual water is removed from the foam.
[0113] The foam density of the foam of the present invention after drying may be, for example, 40 kg / m 3 Up to 144kg / m 3 The significant advantage of the present invention is that it is easy to obtain 80kg / m 3 In some embodiments, the foam density is 48 kg / m 3 Up to 80kg / m 3 .
[0114] When dry, the foam of the present invention exhibits low compression set in addition to low foam density. Compression set is measured on 5×5×2.54 cm skinless specimens according to ASTM D-3774: D. The thickness of the specimen is measured with a micrometer. The specimen is then placed between steel plates, compressed 90% of its original thickness, and aged under compression at 70° C. for 22 hours. The specimen is then removed from the test apparatus and allowed to recover at room temperature for 30 minutes before its thickness is measured again. Compression set is calculated as [100%×(original thickness-final thickness)]÷original thickness. Compression set is typically less than 10%. The compression set in a preferred embodiment may be 8% or less, 6% or less or less, or even 5% or less.
[0115] When dried to constant weight as described above, the foam of the present invention including the phase change material (component g)) may exhibit a latent heat of at least 2.5 J / g at 27°C, as measured by differential scanning calorimetry. The latent heat of the foam may be at least 4 J / g, at least 8 J / g, at least 10 J / g, or at least 14 J / g at this temperature. In some embodiments, the latent heat may be as much as 25 J / g or as much as 30 J / g, or even higher at this temperature.
[0116] The foams of the present invention may exhibit an airflow of at least 0.8 liters / second as measured according to ASTM D3574 Test G. The airflow may be at least 1.2 liters / second or at least 1.4 liters / second, and may be, for example, at most 5 liters / second or at most 4 liters / second.
[0117] In some embodiments, the foam exhibits a Wet Absorption Time of 5 seconds or less, preferably 4 seconds or less. The Wet Absorption Time is measured on a 5×5×2.54 cm skinless sample dried to constant weight. 3 mL of room temperature water is slowly dripped from a pipette onto the top surface of the foam sample, and the amount of time required for the foam to absorb the water is recorded as the Wick Time.
[0118] The foams of the present invention are suitable for use in bedding, seating, and other "comfort" applications. Comfort applications include those applications in which the foam becomes exposed to body heat from the body of a human user or water vapor evaporating from the body of a human user during use. In such applications the foam or article containing the foam typically supports at least a portion of the body weight of the human user and is compressed during use. Examples of such comfort applications include pillows; mattress topper, mattress, comforter, furniture and / or car seats; quilts; insulation garments, etc. Another application of interest is the filling of prosthetic limbs.
[0119] The following examples are provided to illustrate the present invention but are not intended to limit the scope of the present invention. Unless otherwise indicated, all parts and percentages are by weight.
[0120] Polyisocyanate 1 was prepared by first preheating a mixture of 57.9 parts of a poly(ethylene oxide) homopolymer having a number average molecular weight of 1000 g / mol and 3.8 parts of trimethylolpropane to 80°C. Separately, 33.8 parts of an 80 / 20 mixture of 2,4- and 2,6-toluene diisocyanate (TDI) were heated to 40°C. 0.004 parts of benzoyl chloride were added to the TDI. A polyol mixture was added to the TDI, and the resulting reaction mixture was heated to 74°C until a constant isocyanate content of 8% was reached. Another 4.4 parts of TDI were mixed. The resulting product was cooled to less than 60°C. The isocyanate content was measured to be 9.45wt%-10.3wt% according to ASTM D5155. The viscosity was measured to be 18,000mPa-s-21,000mPa-s at 25°C according to ASTM D4065. Polyisocyanate 1 contains about 95.6% by weight of a prepolymer of TDI and polyol, about 3.8% by weight of residues of a branching agent (trimethylolpropane) and about 4.4% by weight of free TDI. Polyisocyanate 1 contains 57.9% by weight of ethylene oxide units by calculation.
[0121] Polyisocyanate 2 was prepared by first preheating a mixture of 32 parts of a poly(ethylene oxide) homopolymer having a number average molecular weight of 1000 g / mol and 13 parts of a trifunctional random copolymer of nominally propylene oxide and ethylene oxide having a number average molecular weight of 5000 g / mol to 80°C, the polyisocyanate containing 75% ethylene oxide units. Separately, 35 parts of a 79 / 21 mixture of 4,4'- and 2,4'-diphenylmethane diisocyanate (MDI) were heated to 55°C. 0.003 parts of benzoyl chloride were added to the MDI. The polyol mixture and MDI were combined, and the resulting reaction mixture was heated to 75°C until a constant isocyanate content was reached. The resulting product was cooled to less than 60°C. The isocyanate content was measured to be 7 wt% according to ASTM D5155. Polyisocyanate 2 contained a prepolymer of MDI and a polyol and a small amount of free MDI. By calculation, polyisocyanate 2 contains 61.75% of ethylene oxide units. The viscosity of polyisocyanate 2 is about 20,000 cps at 25°C.
[0122] Polyisocyanate 3 is prepared by first preheating a mixture of 71.1 parts of a poly(ethylene oxide) homopolymer having a number average molecular weight of 1000 and 1.1 parts of trimethylolpropane to 80°C. Separately, 27.8 parts of an 80 / 20 mixture of 2,4- and 2,6-toluene diisocyanate (TDI) are heated to 40°C. 0.007 parts of benzoyl chloride are added to the TDI. The polyol mixture is added to the TDI, and the resulting reaction mixture is heated to 74°C until a constant isocyanate content of 6.25% is reached. The resulting product is cooled to below 60°C. Polyisocyanate 3 contains a prepolymer of TDI and a polyol. A small amount of free TDI may be present. Polyisocyanate 3 contains 66.2% of ethylene oxide units and about 1.1% by weight of residues of a branching agent.
[0123] Polyisocyanate 4 was prepared by first preheating a mixture of 66.2 parts of a poly(ethylene oxide) homopolymer having a number average molecular weight of 1000 and 2.4 parts of trimethylolpropane to 80°C. Separately, 30.4 parts of an 80 / 20 mixture of 2,4- and 2,6-toluene diisocyanate (TDI) were heated to 40°C. 0.05 parts of benzo-4,4-thiobis(6-tert-butyl-m-cresol) were added to the TDI. The polyol mixture was added to the TDI, and the resulting reaction mixture was heated to 74°C until a constant isocyanate content was reached. A portion of dicyclohexylmethane-4,4'-diisocyanate was mixed. The resulting product was cooled to less than 60°C. The isocyanate content was measured to be 6.8wt% according to ASTM D5155. Polyisocyanate 3 contains a prepolymer of TDI and a polyol and may contain a small amount of free TDI and / or a small amount of free dicyclohexylmethane-4-4'-diisocyanate. Polyisocyanate 4 contains about 66.2% by weight of ethylene oxide units and about 2.4% of residues from a branching agent.
[0124] Polyisocyanate 5 is prepared by first preheating 1000 equivalents of a nominally difunctional propylene oxide homopolymer to 80°C. Separately, 35 parts of a 69 / 31 mixture of 4,4'- and 2,4'-diphenylmethane diisocyanate (MDI) are heated to 55°C. 0.003 parts of benzoyl chloride are added to the MDI. The polyol mixture and MDI are combined, and the resulting reaction mixture is heated to 75°C until a constant isocyanate content of 7% is reached. The resulting product is cooled to below 60°C. Polyisocyanate 5 contains prepolymers of MDI and polyols and free MDI. Polyisocyanate 5 does not contain ethylene oxide units.
[0125] Surfactant A is produced by Momentive High-Tech Products Company under the trade name Silicone surfactants for sale.
[0126] Surfactant B is an ethylene oxide / propylene oxide / ethylene oxide triblock copolymer. The central poly(propylene oxide) block of the copolymer has a molecular weight of 1750. The outer poly(ethylene oxide) blocks comprise 80% of the total weight of the copolymer. The nominal hydroxyl functionality of the copolymer is 2.
[0127] The PCM (Phase Change Material) is a non-encapsulated paraffin wax with a melting temperature of 28°C.
[0128] CPP is a polymer polyol with a hydroxyl number of about 22. The base polyol is a nominally trifunctional 36.5 hydroxyl number copolymer of propylene oxide and ethylene oxide, and the ethylene oxide content of the base polyol is about 20% by weight. The dispersed phase is styrene-acrylonitrile particles. The solid content (weight of the styrene-acrylonitrile particles) is about 40% by weight.
[0129] Poly(EO) is a glycerol initiated, nominally trifunctional ethylene oxide homopolymer having a hydroxyl number of 270 mg KOH / g and a number average molecular weight of 624 g / mol.
[0130] Polyurethane foams were prepared using the ingredients indicated in Tables 1-4 below. In each case, the polyisocyanate was combined with the remaining ingredients on a high-speed laboratory mixer at room temperature for 20 seconds. The resulting reaction mixture was poured into an open mold lined with a polyethylene sheet. The foam rose and solidified in the mold. When dimensionally stable, the foam was demoulded and solidified under ambient conditions for at least 24 hours. The skin was removed from the foam before sampling for property testing.
[0131] Wet absorption time was measured on 5 x 5 x 2.54 cm skinless samples dried to constant weight. 3 mL of room temperature water was slowly dripped from a pipette onto the top surface of the foam sample and the foam density was measured according to ASTM D3574A.
[0132] Compression set was determined from three 2" x 2" x 1" (5.08 cm x 5.08 cm x 2.54 cm) core specimens. The thickness of the specimens was measured using a Litematic micrometer and the specimens were placed between steel plates with 0.1" (2.54 mm) shims to measure the 90% deflection. The foams were aged in a 70°C oven for 22 hours. After 22 hours, the specimens were removed and allowed to recover for 30 minutes before final measurements were made according to ASTM D3574:D.
[0133] Air flow was measured on crushed foam samples according to ASTM D3574:G.
[0134] The latent heat was measured by differential scanning calorimetry.
[0135] The K-factor was measured using a Laser Comp heat flow meter at the average test temperature of the 75°F and 40°F test temperature differential.
[0136] Comparison sample AE
[0137] Comparative Samples AE were made from the formulations shown in Table 1. The foam test results for these samples are indicated in Table 1.
[0138] Table 1
[0139]
[0140] *Not an embodiment of the present invention.
[0141] These foams were made without phase change materials to simplify formulation and isolate the effects of different polyisocyanate compositions. In each case, the latent heat of zero at 27°C reflects the absence of phase change materials. As shown by the data in Table 1, the foam properties are highly dependent on the choice of polyisocyanate in an unpredictable manner.
[0142] Polyisocyanate 2 (Comparison A) by itself produces a foam with very high compression set. When polyisocyanates 1 and 2 are used together in a 30 / 70 ratio (Comparison B), the compression set is improved, but the compression set of 31.2% is too high for this foam to be used in bedding applications.
[0143] A 50 / 50 blend of polyisocyanate 2 with either polyisocyanate 3 (Comparison C) or polyisocyanate 4 (Comparison D) resulted in compression set; airflow was also reduced for Comparison D. A 50 / 50 blend of polyisocyanate 1 with polyisocyanate 5 (Comparison E) produced very poor compression set. Overall, these results show that there is a wide variation in foam properties due to changes in the polyisocyanate, and no single polyisocyanate can be used to achieve low compression set.
[0144] Examples 1-3
[0145] Comparative Samples 1-3 were made from the formulations shown in Table 2. The foam test results of these samples are indicated in Table 2.
[0146] Table 2
[0147]
[0148] These results demonstrate the effect of using a 50 / 50 mixture of polyisocyanates 1 and 2 and three different surfactant packages. Example 1 is a direct comparison to Comparative Sample C (Table 1), except that the TDI prepolymer of Example 1 (Prepolymer 1, 3.8 wt% branching agent) has a higher level of branching than the TDI prepolymer of Comparative Sample C (Prepolymer 3, 1.1 wt% branching agent). The more highly branched Prepolymer 1 results in a significantly lower compression set (9.7% vs. 84.6% for Comparative Sample C).
[0149] Comparison of Example 1 with Comparative Sample B shows the effect of the ratio of components a-1) plus a-2) to components a-3) plus a-4). Too much components a-3) plus a-4) results in a large increase in compression set (31.2 for Comparative Sample B vs. only 9.7% for Example 1).
[0150] Examples 2 and 3 show the effect of using only one of Surfactants A and B. Very low compression sets are obtained in all Examples 1-3, but the airflow is much lower when only one of the surfactants is present, as in Examples 2 and 3. Due to the absence of phase change material, the latent heat at 27°C is zero.
[0151] Comparison of samples F and G
[0152] Comparative samples F and G were made from formulations as shown in Table 3. The foam test results of these samples are indicated in Table 3.
[0153] Table 3
[0154]
[0155] *Not an embodiment of the present invention.
[0156] Comparative Examples F and G illustrate the effect of increasing (Comparative F) or decreasing (Comparative G) the amount of polymer polyol and the 50 / 50 blend of polyisocyanates 1 and 2 compared to Example 1 (Table 2). The compression set of Comparative Sample F increases. Even at this modestly increased level, the compression set is higher than that required for bedding applications. The compression set in Comparative Sample G becomes very high. Again, due to the lack of phase change material, the latent heat is zero in all cases.
[0157] Embodiment 4-8
[0158] Examples 4-8 were made from the formulations shown in Table 4. The foam test results for these samples are indicated in Table 4.
[0159] Table 4
[0160]
[0161] *Not an embodiment of the present invention.
[0162] All of Examples 4-8 exhibit very low compression set.
[0163] The presence of the phase change material in Example 4 has three effects, as shown in comparison to Example 1. The compression set becomes even lower than Example 1, and a positive latent heat is seen at 27° C. Some airflow loss is seen.
[0164] Example 5 shows the effect of including component d) in the reaction mixture in the absence of a phase change material. The compression set is significantly reduced and a higher airflow is obtained when compared to Example 1. Due to the absence of a phase change material, the latent heat at 27°C is zero.
[0165] Examples 6-8 show the effect of including component d) and a phase change material. The compression set is very low and the airflow is improved relative to Example 4 which has a phase change material but no component d). This is seen even at very high levels of phase change material (Example 7). Despite the presence of the phase change material, the airflow of Examples 6 and 8 is comparable to or higher than that of Example 1.
Claims
1. A flexible polyurethane foam comprising the reaction product of a reaction mixture comprising a) an isocyanate mixture, the isocyanate mixture comprising a-1) a first isocyanate functional prepolymer, which is the reaction product of at least one hydroxyl-terminated polymer of ethylene oxide and optionally a hydroxyl-functional branching agent and / or a hydroxyl-functional chain extender with an excess of diphenylmethane diisocyanate, wherein at least 50% by weight of the diphenylmethane diisocyanate is 4,4′-diphenylmethane diisocyanate; a-2) optionally diphenylmethane diisocyanate, wherein components a-1) and a-2) together have an isocyanate content of 5 to 15 wt. % and contain 30 to 75 wt. % of ethylene oxide units, based on the combined weight of components a-1) and a-2), and components a-1) and a-2) together constitute 40 to 60 % of the total weight of the isocyanate mixture; a-3) a second isocyanate functional prepolymer, which is the reaction product of at least one hydroxyl-terminated polymer of ethylene oxide and a hydroxyl-functional branching agent with an excess of toluene diisocyanate, the hydroxyl-functional branching agent having at least three hydroxyl groups per molecule and a hydroxyl equivalent weight of up to 250 grams per equivalent; as well as a-4) optionally toluene diisocyanate, wherein a-3) and a-4) together have an isocyanate content of 5% to 15% by weight and contain 30% to 75% by weight of ethylene oxide units, based on the combined weight of components a-3) and a-4), and 2% to 5% by weight of residues from the hydroxy-functional branching agent, based on the combined weight of components a-3) and a-4); components a-3) and a-4) together constitute 40% to 60% of the total weight of the isocyanate mixture; and components a-1), a-2), a-3) and a-4) together make up the entire weight of the isocyanate mixture; b) water; c) at least one polymer polyol comprising polymer particles dispersed in at least one base polyol, the base polyol being a polyether having at least 50 wt% oxypropylene units and a hydroxyl equivalent weight of 500 g / equivalent to 3000 g / equivalent; d) optionally poly(ethylene oxide) which is a homopolymer of ethylene oxide or a random or block copolymer of at least 80% by weight of ethylene oxide and up to 20% by weight of another alkylene oxide, said poly(ethylene oxide) having a number average molecular weight of from 400 g / mol to 1200 g / mol; At least one of e) and f), wherein e) is at least one silicone surfactant; and f) is at least one ethylene oxide / higher alkylene oxide block copolymer, the block copolymer containing 40 wt% to 90 wt% ethylene oxide units and having a number average molecular weight of 1500 g / mol to 12,000 g / mol, wherein the higher alkylene oxide is 1,2-propylene oxide, 1,2-butylene oxide or a mixture thereof; and optionally g) at least one phase change material, the at least one phase change material having a melting or glass transition temperature of 25°C to 37°C and being free of isocyanate groups or isocyanate-reactive groups, wherein the phase change material comprises any one or more of natural or synthetic waxes; in i) the isocyanate mixture comprises 40% to 65% of the combined weight of components ag; ii) water comprises from 15% to 41% by weight of the combined weight of components ag; iii) the at least one polymer polyol comprises from 8% to 20% of the combined weight of components ag, and the polymer particles comprise from 0.5% to 10% of the combined weight of components ag; iv) when present, said poly(ethylene oxide) comprises up to 5% by combined weight of components ag; v) the at least one silicone surfactant comprises from 0% to 3% by combined weight of components ag; vi) the at least one ethylene oxide / higher alkylene oxide block copolymer comprises 0% to 3% of the combined weight of component ag; vii) the at least one phase change material comprises up to 15% by combined weight of components ag; and viii) Component ag comprises at least 95% by weight of the reaction mixture.
2. The flexible polyurethane foam according to claim 1, wherein the phase change material comprises any one or more of the following: polyethylene wax, beeswax, lanolin, carnauba wax, candelilla wax, cocoa wax, sugar cane wax, jojoba wax, cuticle wax, coconut wax or paraffin wax.
3. The flexible polyurethane foam according to claim 1 or 2, wherein the phase change material accounts for 2.5% to 10% of the total weight of component ag.
4. The flexible polyurethane foam according to claim 1 or 2, wherein components a-1) and a-2) together constitute 45% to 55% by weight of the isocyanate mixture, and components a-3) and a-4) together constitute 55% to 45% by weight of the isocyanate mixture.
5. The flexible polyurethane foam according to claim 1 or 2, wherein the silicone surfactant and the ethylene oxide / higher carbon alkylene oxide block copolymer each constitute 0.5% to 3% of the combined weight of component ag.
6. The flexible polyurethane foam according to claim 1 or 2, wherein the silicone surfactant contains 25 to 70 wt% of polysiloxane, 10 to 75 wt% of polymerized ethylene oxide, and 0 to 10 wt% of polymerized propylene oxide, based on the weight of the silicone surfactant.
7. The flexible polyurethane foam according to claim 1 or 2, wherein the ethylene oxide / higher alkylene oxide block copolymer contains 40% to 90% of ethylene oxide units and has a number average molecular weight of 1,500 to 12,000.
8. The flexible polyurethane foam of claim 1 or 2, wherein the poly(ethylene oxide) comprises from 0.5% to 5% of the combined weight of components ag.
9. A method for preparing a flexible polyurethane foam, the method comprising A. Form a reaction mixture by combining: a) an isocyanate mixture, the isocyanate mixture comprising a-1) a first isocyanate functional prepolymer, which is the reaction product of at least one hydroxyl-terminated polymer of ethylene oxide and optionally a hydroxyl-functional branching agent and / or a hydroxyl-functional chain extender with an excess of diphenylmethane diisocyanate, wherein at least 50% by weight of the diphenylmethane diisocyanate is 4,4′-diphenylmethane diisocyanate; a-2) optionally diphenylmethane diisocyanate, wherein components a-1) and a-2) together have an isocyanate content of 5 to 15 wt. % and contain 30 to 75 wt. % of ethylene oxide units, based on the combined weight of components a-1) and a-2), and components a-1) and a-2) together constitute 40 to 60 % of the total weight of the isocyanate mixture; a-3) a second isocyanate functional prepolymer, which is the reaction product of at least one hydroxyl-terminated polymer of ethylene oxide and a hydroxyl-functional branching agent with an excess of toluene diisocyanate, the hydroxyl-functional branching agent having at least three hydroxyl groups per molecule and a hydroxyl equivalent weight of up to 250 grams per equivalent; as well as a-4) optionally toluene diisocyanate, wherein a-3) and a-4) together have an isocyanate content of 5% to 15% by weight and contain 30% to 75% by weight of ethylene oxide units, based on the combined weight of components a-3) and a-4), and 2% to 5% by weight of residues from the hydroxy-functional branching agent, based on the combined weight of components a-3) and a-4); components a-3) and a-4) together constitute 40% to 60% of the total weight of the isocyanate mixture; and components a-1), a-2), a-3) and a-4) together make up the entire weight of the isocyanate mixture; b) water; c) at least one polymer polyol comprising polymer particles dispersed in at least one base polyol, the base polyol being a polyether having at least 50 wt% oxypropylene units and a hydroxyl equivalent weight of 500 g / equivalent to 3000 g / equivalent; d) optionally poly(ethylene oxide) which is a homopolymer of ethylene oxide or a random or block copolymer of at least 80% by weight of ethylene oxide and up to 20% by weight of another alkylene oxide, said poly(ethylene oxide) having a number average molecular weight of from 400 g / mol to 1200 g / mol; At least one of e) and f), wherein e) is at least one silicone surfactant; and f) at least one ethylene oxide / higher alkylene oxide block copolymer containing 40 to 90 wt% ethylene oxide units and having a number average molecular weight of 1500 to 12,000 g / mol, wherein the higher alkylene oxide is 1,2-propylene oxide, 1,2-butylene oxide or a mixture thereof; and optionally g) at least one phase change material having a melting or glass transition temperature of 25°C to 37°C and containing no isocyanate groups or isocyanate reactive groups, wherein the phase change material comprises any one or more of natural or synthetic waxes; in i) the isocyanate mixture comprises 40% to 65% of the combined weight of components ag; ii) water comprises from 15% to 41% by weight of the combined weight of components ag; iii) the at least one polymer polyol comprises from 8% to 20% of the combined weight of components ag, and the polymer particles comprise from 0.5% to 10% of the combined weight of components ag; iv) when present, said poly(ethylene oxide) comprises up to 5% by combined weight of components ag; v) the at least one silicone surfactant comprises from 0% to 3% by combined weight of components ag; vi) the at least one ethylene oxide / higher alkylene oxide block copolymer comprises 0% to 3% of the combined weight of component ag; vii) the at least one phase change material comprises up to 15% by combined weight of components ag; and viii) component ag comprises at least 95% by weight of the reaction mixture; and B. reacting the reaction mixture to produce the foam.
10. The method according to claim 9, wherein the phase change material accounts for 2.5% to 10% of the total weight of component ag, and the phase change material includes any one or more of the following: polyethylene wax, beeswax, lanolin, carnauba wax, candelilla wax, cocoa wax, sugar cane wax, jojoba wax, cuticle wax, coconut wax or paraffin wax.
11. The method according to any one of claims 9 to 10, wherein the silicone surfactant and the ethylene oxide / higher alkylene oxide block copolymer each account for 0.5% to 3% of the combined weight of component ag, the silicone surfactant containing 25% to 70% by weight of polysiloxane, 10% to 75% by weight of polymerized ethylene oxide and 0% to 10% by weight of polymerized propylene oxide based on the weight of the silicone surfactant, and the ethylene oxide / higher alkylene oxide block copolymer contains 40% to 90% of ethylene oxide units and has a number average molecular weight of 1,500 to 12,000.
12. A cushion comprising the flexible polyurethane foam according to claim 1 or 2.
13. The cushion of claim 12, wherein the cushion is a pillow, a mattress topper, a mattress, a comforter, a furniture seat or backrest, a car seat or backrest; an insulating garment or a prosthetic pad.
14. The cushion of claim 12, wherein the flexible polyurethane foam has a hardness of 48 kg / m 3 Up to 80kg / m 3 density and a compression set of 10% or less.
15. The pad of claim 12, wherein the flexible polyurethane foam exhibits a latent heat of at least 2.5 J / g at 27°C and a moisture wicking time of 5 seconds or less when dried to constant weight.
Citation Information
Patent Citations
Process for the preparation of stable dispersions of polyisocyanate-polyaddition products in hydroxyl containing compounds
US4305857A
Polymer polyols
WO1994020558A1
Melt dispersion process for making polymer polyols
WO2009155427A2
Seeding process for the manufacture of polymer modified polyols