Method for manufacturing grain-oriented electrical steel sheet

By combining hot rolling, cold rolling, primary recrystallization annealing and shot peening in the manufacturing process of grain-oriented electromagnetic steel sheets, elements such as Cu are used to contact precipitates such as MnS to solve the problem of magnetic flux density and In order to solve the problem of insufficient excellence in magnetic properties, oriented electromagnetic steel sheets with high magnetic flux density and uniform appearance have been realized to meet the stability and reliability requirements of transformers.

CN115135780BActive Publication Date: 2024-10-29NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202180014834.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-23
Publication Date
2024-10-29
Estimated Expiration
2041-06-23

AI Technical Summary

Technical Problem

It is difficult to achieve high magnetic flux density and excellent stability of magnetic properties in grain-oriented electromagnetic steel sheets with existing technology, especially in terms of iron loss reduction and appearance uniformity in transformers.

Method used

In the manufacturing process of steel plates, hot rolling, cold rolling, primary recrystallization annealing and final annealing are adopted, and the surface is coated with annealing separation agent, combined with shot peening or leveling processing, using elements such as Cu and MnS etc. Precipitate contact improves the heat resistance and magnetic properties of the inhibitor, while controlling the heating rate and atmosphere conditions to optimize grain orientation and film properties.

Benefits of technology

A directional electromagnetic steel plate with high magnetic flux density and excellent magnetic properties has been realized, which reduces the iron loss value and ensures the uniformity and stability of the appearance of the steel plate to meet the reliability requirements of the transformer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003799296370000221
    Figure BDA0003799296370000221
  • Figure BDA0003799296370000241
    Figure BDA0003799296370000241
  • Figure BDA0003799296370000261
    Figure BDA0003799296370000261
Patent Text Reader

Abstract

The present invention provides a novel and improved method for manufacturing a directional electromagnetic steel sheet capable of manufacturing a directional electromagnetic steel sheet having high magnetic flux density and excellent magnetic properties. One embodiment of the present invention provides a method for manufacturing a directional electromagnetic steel sheet, characterized in that it includes a hot rolling process, a cold rolling process, a primary recrystallization annealing process, a final annealing process, and a flattening annealing process, and performs shot peening and / or leveling processing and a treatment of contacting with a solution, wherein the solution contains a predetermined amount of Cu, etc., has a pH of 1.5 or more and less than 7, a liquid temperature of 15°C or more and 100°C or less, and the steel sheet is immersed in the solution for a time of 5 seconds or more and 200 seconds or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a grain-oriented electromagnetic steel sheet. Background Art

[0002] Grain-oriented electrical steel sheets contain about 2 to 5 mass% of Si, and the grain orientation of the steel sheet is highly concentrated in the {110} so-called Goss orientation. <001> Oriented steel sheet. Oriented electrical steel sheet has excellent magnetic properties and is used, for example, as a core material for static inductors such as transformers.

[0003] Various developments have been made to improve the magnetic properties of grain-oriented electromagnetic steel sheets. In particular, with the recent demand for energy conservation, grain-oriented electromagnetic steel sheets are required to have lower iron loss. To reduce the iron loss of grain-oriented electromagnetic steel sheets, it is effective to increase the concentration of the grains of the steel sheets toward the Goss orientation to increase the magnetic flux density and thus reduce the hysteresis loss.

[0004] Here, in the production of grain-oriented electrical steel sheets, the control of crystal orientation is performed by utilizing a catastrophic grain growth phenomenon called secondary recrystallization. However, in order to appropriately control the crystal orientation by secondary recrystallization, it is important to improve the heat resistance of fine precipitates in the steel called inhibitors.

[0005] For example, a method can be cited in which the inhibitor is completely dissolved when the steel slab is heated before hot rolling, and then finely precipitated during hot rolling and the subsequent annealing process. Specifically, a method can be cited in which MnS and AlN are used as inhibitors and rolling is performed at a reduction ratio exceeding 80% in the final cold rolling process, as exemplified in the following Patent Document 1, or a method can be cited in which MnS and MnSe are used as inhibitors and a second cold rolling process is performed, as exemplified in the following Patent Document 2.

[0006] In addition, Patent Documents 3 and 4 disclose a technology for manufacturing a directional electromagnetic steel sheet with excellent film properties by controlling the conditions of hot-rolled sheet annealing and pickling treatment. Furthermore, Patent Document 5 discloses a technology for manufacturing a directional electromagnetic steel sheet with excellent film properties by controlling the conditions of pickling treatment, the addition conditions of annealing separators, and the final annealing conditions. Patent Document 6 discloses a technology for manufacturing a directional electromagnetic steel sheet with excellent magnetic properties by controlling carbides through heat treatment before cold rolling. Furthermore, Patent Document 7 discloses a technology for manufacturing a directional electromagnetic steel sheet with excellent magnetic properties by controlling the heating process of primary recrystallization annealing and introducing a small amount of strain during the heating process.

[0007] In addition, the following Patent Document 8 discloses a technology for manufacturing a grain-oriented electrical steel sheet with low iron loss over the entire length of the coil by controlling the heating pattern in the temperature rise process of the primary recrystallization annealing. Furthermore, the following Patent Document 9 discloses a technology for reducing the iron loss value of the grain-oriented electrical steel sheet by strictly controlling the average grain size and the deviation angle from the ideal orientation of the grains after the secondary recrystallization.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Publication No. 40-15644

[0011] Patent Document 2: Japanese Patent Publication No. 51-13469

[0012] Patent Document 3: Japanese Patent Application Publication No. 2019-99827

[0013] Patent Document 4: Japanese Patent Application Publication No. 2003-193141

[0014] Patent Document 5: Japanese Patent Application Publication No. 2014-196559

[0015] Patent Document 6: Japanese Patent Application Publication No. 2016-156068

[0016] Patent Document 7: Japanese Patent Application Laid-Open No. 6-212274

[0017] Patent Document 8: International Publication No. 2014 / 049770

[0018] Patent Document 9: Japanese Patent Application Laid-Open No. 7-268567 Summary of the invention

[0019] Problems to be solved by the invention

[0020] In recent years, due to the progress of transformer efficiency restrictions internationally, the demand for reducing iron loss in grain-oriented electromagnetic steel sheets has become even greater. On the other hand, transformers have been important equipment and machines that support the foundation of society for a long time, so it is important to operate them stably and continuously. Therefore, grain-oriented electromagnetic steel sheets, which are the main components, are also required to have reliability that helps to ensure the stable operation of transformers. In particular, the appearance of grain-oriented electromagnetic steel sheets without color unevenness and uniformity has become an important factor in gaining the trust of consumers.

[0021] The above-mentioned Patent Documents 3 to 5 disclose a technique for improving film adhesion by creating a difference in the concentration of Mn and Cu between the steel plate surface and the center of the plate thickness. However, the technique of concentrating a specific component on the steel plate surface is only for the purpose of improving film properties, and a technique for stably obtaining good magnetic properties has not been studied.

[0022] Patent Document 6 discloses that the change from cementite to graphite is promoted by heat treatment before cold rolling to improve the texture obtained in the subsequent primary recrystallization. However, the heating process and pickling of the primary recrystallization annealing follow the conventional methods and no new research is conducted.

[0023] In addition, as disclosed in the above-mentioned Patent Document 7, it is confirmed that in the heating process of the primary recrystallization annealing, by rapidly heating to a temperature of 700°C or more at a rate of 100°C / s or more, and introducing a small strain of 0.1% or more of nominal strain in the rapid heating, the magnetic properties of the grain-oriented electrical steel sheet are greatly affected. In addition, in the above-mentioned Patent Document 8, it is confirmed that in the heating process of the primary recrystallization annealing, by rapidly heating between 500°C and 600°C at a rate of 100°C / s or more, the magnetic properties of the grain-oriented electrical steel sheet are greatly affected. In the above-mentioned Patent Document 9, it is disclosed that in the heating process of the primary recrystallization annealing, the heating temperature to 850°C is set to 300°C / s or 450°C / s.

[0024] However, in the above-mentioned Patent Documents 7 to 9, no detailed study is conducted on how the magnetic properties of the grain-oriented electrical steel sheet are affected when the inhibitor is changed in the thickness direction of the steel sheet.

[0025] The present invention has been made in view of the above problems and the like, and an object of the present invention is to provide a novel and improved method for manufacturing a grain-oriented electrical steel sheet capable of manufacturing a grain-oriented electrical steel sheet that achieves a high magnetic flux density and has excellent magnetic properties.

[0026] Means for solving problems

[0027] In order to solve the above-mentioned problems, according to one aspect of the present invention, there is provided a method for manufacturing a grain-oriented electrical steel sheet, characterized by comprising the following steps:

[0028] A process of obtaining a hot-rolled steel sheet by heating and hot-rolling a slab, or obtaining a hot-rolled annealed steel sheet by hot-rolling the hot-rolled steel sheet, wherein the slab contains, in terms of mass%, C: 0.01% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.50%, a total of one or more of S, Se and Te: 0.001% to 0.050%, acid-soluble Al: more than 0% to 0.05%, N: more than 0% to 0.015%, and the remainder is Fe and impurities;

[0029] A step of obtaining a cold-rolled steel sheet by cold-rolling the hot-rolled steel sheet or the hot-rolled annealed steel sheet;

[0030] A step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet;

[0031] A step of applying an annealing separator containing MgO to the surface of a primary recrystallization annealed sheet and then performing final annealing to obtain a final annealed sheet;

[0032] wherein at least one of the hot-rolled steel sheet, the hot-rolled annealed steel sheet, the cold-rolled steel sheet, and the primary recrystallization annealed steel sheet is subjected to a shot peening treatment and a treatment of contacting with a solution;

[0033] After the insulating film is applied to the above-mentioned final annealed sheet, a planarization annealing step is performed.

[0034] In the shot peening treatment, the average particle size of the shot material is 0.1 mm or more and 5.0 mm or less, and the shot speed is 10 m / s or more and 150 m / s or less.

[0035] The solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is 0.00001% to 1.0000%, the pH is -1.5 to 7, the liquid temperature is 15°C to 100°C, and the steel plate is immersed in the solution for 5 seconds to 200 seconds.

[0036] According to one aspect of the present invention, there is provided a method for manufacturing a grain-oriented electrical steel sheet, characterized in that:

[0037] Instead of or in addition to the above-mentioned shot peening, a leveling treatment may be performed.

[0038] In the flattening treatment, the hot-rolled steel sheet is bent twice or more, the bending angle is 10 degrees or more and 90 degrees or less, and the bending radius is 10 mm or more and 200 mm or less.

[0039] Furthermore, according to one aspect of the present invention, there is provided a method for manufacturing a grain-oriented electrical steel sheet, characterized in that:

[0040] In the rapid heating of the primary recrystallization annealing, the average heating rate in the temperature range of 550° C. to 700° C. is 100° C. / s or more and 3000° C. / s or less.

[0041] Furthermore, according to one aspect of the present invention, there is provided a method for manufacturing a grain-oriented electrical steel sheet, characterized in that:

[0042] The slab contains one or more selected from the group consisting of Cu: 1.0% or less, Sn: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Sb: 1.0% or less, and Bi: 1.0% or less, in place of a portion of the Fe.

[0043] Furthermore, according to one aspect of the present invention, there is provided a method for manufacturing a grain-oriented electrical steel sheet, characterized in that:

[0044] The primary recrystallization annealing includes a step of heating, a step of performing an intermediate treatment between heating and decarburization annealing, and a step of performing decarburization annealing.

[0045] In the intermediate treatment, the dew point temperature of the atmosphere is -40°C to 0°C and the residence time of the steel sheet temperature is 700°C to 950°C for 1 second to 20 seconds.

[0046] In the above decarburization annealing, the oxygen partial pressure ratio (P H2O / P H2 ) is greater than or equal to 0.35 and less than or equal to 0.60.

[0047] Effects of the Invention

[0048] According to the present invention, a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni (sometimes referred to as "Cu, etc." in this specification) is brought into contact with an electromagnetic steel sheet. The electromagnetic steel sheet contains MnS, MnSe, MnTe (sometimes referred to as "MnS, etc." in this specification) as precipitates, and the precipitates such as MnS act as inhibitors. In the present invention, the heat resistance of the precipitates is improved by effectively utilizing the phenomenon that when MnS, etc. comes into contact with a solution containing Cu, etc., a portion of Mn in MnS, etc., especially Mn in the surface layer of MnS, etc., is replaced by Cu, etc., thereby improving the inhibitor strength of the grain-oriented electromagnetic steel sheet. Through this mechanism of action, a new and improved method for manufacturing a grain-oriented electromagnetic steel sheet that can achieve a high magnetic flux density and has excellent magnetic properties can be provided.

[0049] According to another aspect of the present invention, by combining a technique for increasing Goss-oriented grains near the surface layer by performing a rapid heating process in the temperature rise process of the primary recrystallization annealing, it is possible to further achieve a higher magnetic flux density.

[0050] Furthermore, according to another aspect of the present invention, by combining a technique of adding an additive element to the slab to stabilize the secondary crystallization, it is possible to further achieve a higher magnetic flux density.

[0051] Furthermore, the present inventors have found that the phenomenon that the Mn in the surface layer of MnS or the like is replaced by Cu or the like may sometimes cause color unevenness in the final product, but this can be eliminated by controlling and improving the atmosphere and temperature conditions in the intermediate treatment of the primary recrystallization annealing (rapid heating treatment, intermediate treatment and decarburization annealing) and the atmosphere conditions in the decarburization annealing. Based on this knowledge, another embodiment of the present invention can suppress this color unevenness. DETAILED DESCRIPTION

[0052] The preferred embodiments of the present invention are described in detail below. It should be noted that, unless otherwise specified, with respect to numerical values ​​A and B, a description such as "A to B" means "above A and below B". In the case where only numerical value B is marked with a unit in the description, the unit also applies to numerical value A.

[0053] [Method for producing grain-oriented electrical steel sheet]

[0054] The present inventors have conducted intensive studies on a method for producing a grain-oriented electrical steel sheet in order to improve the magnetic properties of the grain-oriented electrical steel sheet, and as a result, have found the following findings.

[0055] Specifically, the inventors have found that the heat resistance of MnS etc. can be improved by effectively utilizing the phenomenon that when an electromagnetic steel sheet containing MnS etc. is brought into contact with a solution containing Cu etc., a part of Mn in MnS etc., especially Mn in the surface layer of MnS etc., is replaced by Cu etc., thereby improving the inhibitor strength and improving the magnetic properties. In addition, it has been found that when the electromagnetic steel sheet containing MnS etc. is brought into contact with the solution, the inhibitor can be controlled in the thickness direction of the steel sheet by making efforts in the pre-treatment of shot peening or leveling treatment, thereby further improving the magnetic properties.

[0056] Furthermore, the inventors have found that the magnetic properties can be further improved by increasing the number of Goss-oriented grains near the surface layer by performing a rapid heating process in the temperature rise process of the primary recrystallization annealing.

[0057] Furthermore, it was found that the magnetic properties can be further improved by adding additive elements to the slab to stabilize the secondary crystals.

[0058] It was further discovered that the phenomenon in which Mn in the surface layer of MnS or the like is replaced by Cu or the like sometimes causes color unevenness in the final product, but that the color unevenness can be eliminated by controlling and improving the atmosphere and temperature conditions in the intermediate treatment of the primary recrystallization annealing (rapid heating treatment, intermediate treatment and decarburization annealing) and the atmosphere conditions in the decarburization annealing.

[0059] The present inventors have come up with the present invention after considering the above findings. One embodiment of the present invention is a method for manufacturing a grain-oriented electrical steel sheet having the following configuration, which includes the following steps:

[0060] A process of obtaining a hot-rolled steel sheet by heating and hot-rolling a slab, or obtaining a hot-rolled annealed steel sheet by hot-rolling the hot-rolled steel sheet, wherein the slab contains, in terms of mass%, C: 0.01% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.50%, a total of one or more of S, Se and Te: 0.001% to 0.050%, acid-soluble Al: more than 0% to 0.05%, N: more than 0% to 0.015%, and the remainder is Fe and impurities;

[0061] A step of obtaining a cold-rolled steel sheet by cold-rolling the hot-rolled steel sheet or the hot-rolled annealed steel sheet;

[0062] A step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet;

[0063] A step of applying an annealing separator containing MgO to the surface of a primary recrystallization annealed sheet and then performing final annealing to obtain a final annealed sheet;

[0064] After the insulating film is applied to the above-mentioned final annealed sheet, a planarization annealing step is performed.

[0065] wherein at least one of the hot-rolled steel sheet, the hot-rolled annealed steel sheet, the cold-rolled steel sheet, and the primary recrystallization annealed steel sheet is subjected to a shot peening treatment and a treatment of contacting with a solution;

[0066] In the shot peening treatment, the average particle size of the shot material is 0.1 mm or more and 5.0 mm or less, and the shot speed is 10 m / s or more and 150 m / s or less.

[0067] The solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is 0.00001% to 1.0000%, the pH is -1.5 to 7, the liquid temperature is 15°C to 100°C, and the steel plate is immersed in the solution for 5 seconds to 200 seconds.

[0068] Instead of or in addition to the above-mentioned shot peening, a leveling treatment may be performed.

[0069] In the leveling treatment, the steel sheet is bent twice or more, the bending angle is 10 degrees or more and 90 degrees or less, and the bending radius is 10 mm or more and 200 mm or less.

[0070] Furthermore, the temperature rise process of the primary recrystallization annealing may be set to rapid heating, and in the rapid heating, the average heating rate in the temperature range of 550° C. to 700° C. may be set to 100° C. / s or more and 3000° C. / s or less.

[0071] Furthermore, the primary recrystallization annealing may include a step of heating, a step of performing an intermediate treatment between heating and decarburization annealing, and a step of performing decarburization annealing.

[0072] In the intermediate treatment, the dew point temperature of the atmosphere is -40°C to 0°C and the residence time of the steel sheet temperature is 700°C to 950°C for 1 second to 20 seconds.

[0073] In the above decarburization annealing, the oxygen partial pressure ratio (P H2O / P H2 ) is greater than or equal to 0.35 and less than or equal to 0.60.

[0074] Hereinafter, a method for producing a grain-oriented electrical steel sheet according to the present embodiment will be described in detail.

[0075] [Slab composition]

[0076] First, the composition of the slab used in the grain-oriented electrical steel sheet of the present embodiment is described. It should be noted that, unless otherwise specified, the description of "%" is set to represent "mass %". In addition, the remainder of the slab other than the elements described below is Fe and impurities. Here, the so-called impurities refer to components contained in the raw materials or components mixed in the manufacturing process and are not intentionally contained in the steel sheet. In addition, the chemical composition of the slab as the raw material of the grain-oriented electrical steel sheet becomes a chemical composition that basically depends on the composition of the grain-oriented electrical steel sheet. However, in the manufacture of general grain-oriented electrical steel sheets, a part of the elements contained in the manufacturing process is discharged to the outside of the system through decarburization annealing and purification annealing, so the chemical composition of the slab as the raw material and the grain-oriented electrical steel sheet as the final product becomes different. In order to make the characteristics of the grain-oriented electrical steel sheet as desired, the slab composition can be appropriately adjusted in consideration of the influence of decarburization annealing and purification annealing in the manufacturing process.

[0077] The C (carbon) content is not less than 0.01% and not more than 0.10%. C has various functions, but when the C content is less than 0.01%, the grain size becomes excessively large when the slab is heated, thereby increasing the iron loss value of the final directional electromagnetic steel sheet, which is not preferred. When the C content exceeds 0.10%, the decarburization time becomes long during decarburization after cold rolling, and the manufacturing cost increases, which is not preferred. In addition, when the C content exceeds 0.10%, decarburization tends to become incomplete, and magnetic aging may be caused in the final directional electromagnetic steel sheet, which is not preferred. Therefore, the C content is not less than 0.01% and not more than 0.10%, preferably not less than 0.05% and not more than 0.09%.

[0078] The content of Si (silicon) is 2.5% or more and 4.5% or less. Si reduces eddy current loss, which is one of the causes of iron loss, by increasing the electrical resistance of the steel sheet. When the content of Si is less than 2.5%, it becomes difficult to fully suppress the eddy current loss of the final directional electromagnetic steel sheet, so it is not preferred. When the content of Si exceeds 4.5%, the workability of the directional electromagnetic steel sheet decreases, so it is not preferred. Therefore, the content of Si is 2.5% or more and 4.5% or less, preferably 2.7% or more and 4.0% or less.

[0079] The content of Mn (manganese) is 0.01% or more and 0.50% or less. Mn forms inhibitors that affect secondary recrystallization, such as MnS, MnSe, and MnTe. When the content of Mn is less than 0.01%, the absolute amount of MnS, MnSe, and MnTe that produce secondary recrystallization is insufficient, so it is not preferred. When the content of Mn exceeds 0.50%, the solid solution of Mn becomes difficult when the slab is heated, so it is not preferred. In addition, when the content of Mn exceeds 0.15%, the precipitation size of MnS, MnSe, and MnTe as inhibitors tends to coarsen, and the optimal size distribution as inhibitors is damaged, so it is not preferred. Therefore, the content of Mn is 0.01% or more and 0.50% or less, preferably 0.01% or more and 0.30% or less. More preferably, it is 0.03% or more and 0.15% or less.

[0080] The total content of one or more of S (sulfur), Se (selenium) and Te is 0.001% or more and 0.050% or less. S, Se and Te form inhibitors together with the above-mentioned Mn. Two or more of S, Se and Te may be contained in the slab, but it is sufficient as long as at least one of them is contained in the slab. When the total content of S, Se and Te deviates from the above range, a sufficient inhibitor effect cannot be obtained, so it is not preferred. Therefore, the total content of S, Se and Te is 0.001% or more and 0.050% or less, preferably 0.002% or more and 0.040% or less.

[0081] The content of acid-soluble Al (acid-soluble aluminum) is more than 0% and less than 0.05%. Acid-soluble Al constitutes an inhibitor required for manufacturing a directional electromagnetic steel sheet with a high magnetic flux density. When the content of acid-soluble Al is 0, AlN does not exist, and sometimes the inhibitor strength is insufficient to obtain good magnetic properties, so it is not preferred. When the content of acid-soluble Al exceeds 0.05%, AlN precipitated as an inhibitor coarsens, which reduces the inhibitor strength, so it is not preferred. Therefore, the content of acid-soluble Al is more than 0% and less than 0.05%, preferably more than 0% and less than 0.04%.

[0082] The content of N (nitrogen) is more than 0% and less than 0.015%. N forms AlN as an inhibitor together with the above-mentioned acid-soluble Al. When the content of N deviates from the above range, a sufficient inhibitor effect cannot be obtained, which is not preferred. Therefore, the content of N is more than 0% and less than 0.015%, preferably more than 0% and less than 0.012%.

[0083] P (phosphorus) may also be contained in an amount exceeding 0% and below 1.0%. P has the effect of increasing strength without reducing magnetic flux density. However, if P is contained excessively, the toughness of the steel is impaired, and fractures are more likely to occur in the steel plate. Therefore, the upper limit of the P amount is set to 1.0%. It is preferably below 0.150%, and more preferably below 0.120%. The lower limit of the P amount is not particularly limited, but if the manufacturing cost is also taken into consideration, it becomes 0.001% or more.

[0084] In addition, the slab used in the manufacture of the grain-oriented electrical steel sheet of the present embodiment may contain any one or more of Cu, Sn, Ni, Cr, Sb, or Bi as an element that stabilizes secondary recrystallization in addition to the above-mentioned elements. When the slab contains the above-mentioned elements, the magnetic flux density of the manufactured grain-oriented electrical steel sheet can be further improved.

[0085] The molten steel adjusted to the above-described component composition is cast to form a slab. It should be noted that the casting method of the slab is not particularly limited. In addition, during research and development, even if a steel ingot is formed by a vacuum melting furnace or the like, the same effect as that of the case of forming a slab can be confirmed with respect to the above-described components.

[0086] [Process of producing hot-rolled steel sheets]

[0087] Next, the slab is heated and hot-rolled to form a hot-rolled steel sheet. The slab heating temperature is not particularly limited. In the case where the inhibitor components in the slab are completely dissolved, for example, it can be heated to 1280°C or above. It should be noted that the upper limit of the slab heating temperature at this time is not particularly specified, but it is preferably 1450°C from the viewpoint of equipment protection. For example, the slab heating temperature can be above 1280°C and below 1450°C. On the other hand, in the case where the inhibitor components in the slab are not completely dissolved, for example, the slab heating temperature can be set to below 1280°C. In this case, the steel sheet can also be nitrided in any process from the hot rolling process or the hot rolled sheet annealing process to the final annealing process.

[0088] Next, the heated slab is hot rolled to be processed into a hot-rolled steel plate. The thickness of the processed hot-rolled steel plate may be, for example, 1.8 mm or more and 3.5 mm or less. When the thickness of the hot-rolled steel plate is less than 1.8 mm, the shape of the steel plate after hot rolling may become inferior, which is not preferred. When the thickness of the hot-rolled steel plate exceeds 3.5 mm, the rolling load in the cold rolling process becomes large, which is not preferred.

[0089] The hot rolled steel sheet may be subjected to hot rolled sheet annealing to obtain a hot rolled annealed sheet. When hot rolled sheet annealing is performed, the shape of the steel sheet becomes better, and thus the possibility of the steel sheet being broken during the subsequent cold rolling process can be reduced.

[0090] [Process of manufacturing cold-rolled steel sheets]

[0091] Next, the obtained hot-rolled steel sheet or hot-rolled annealed sheet is processed into a cold-rolled steel sheet by rolling with one cold rolling or multiple cold rolling with intermediate annealing. It should be noted that, in the case of rolling with multiple cold rolling with intermediate annealing and / or pickling, the hot-rolled sheet annealing in the front section may be omitted. From the viewpoint of reducing the wear of the rolls in the cold rolling, it is preferred to implement the pickling treatment before each cold rolling process. In addition, both the hot-rolled sheet annealing and the intermediate annealing may be implemented.

[0092] In addition, the steel plate may be heat treated below about 300°C between cold rolling passes, between roll stands, or during rolling. In this case, the magnetic properties of the final directional electromagnetic steel plate can be improved. It should be noted that the hot-rolled steel plate may also be rolled by more than three cold rollings, but multiple cold rollings will increase the manufacturing cost, so the hot-rolled steel plate is preferably rolled by one or two cold rollings. In the case of cold rolling by reversible rolling such as a Sendzimir mill, the number of passes in each cold rolling is not particularly limited, but from the viewpoint of manufacturing cost, it is preferably 9 or less.

[0093] [Step of performing primary recrystallization annealing]

[0094] Next, the cold-rolled steel sheet is heated and then subjected to decarburization annealing. These processes are also referred to as primary recrystallization annealing and are preferably performed continuously. By setting the temperature rise of the primary recrystallization annealing to be rapid, the Goss oriented grains before the secondary recrystallization can be increased in the cold-rolled steel sheet, and in the secondary recrystallization process, the oriented grains close to the ideal Goss orientation can be expected to undergo secondary recrystallization.

[0095] (Heating process)

[0096] In the present invention, during the heating process in the primary recrystallization annealing, the average heating rate between 550°C and 700°C can also be set to a rapid rate of 100°C / s or more and 3000°C / s or less. As a result, the Goss-oriented grains before the secondary recrystallization of the cold-rolled steel sheet can be increased, and the magnetic flux density of the final directional electromagnetic steel sheet can be improved. The temperature range of rapid heating is 550°C to 700°C. When the starting temperature of rapid heating exceeds 550°C, the recovery of dislocations in the steel sheet progresses greatly, and the primary recrystallization of oriented grains other than the Goss-oriented grains begins, so the effect of increasing the Goss-oriented grains is reduced, which is not preferred. When the ending temperature of rapid heating is lower than 700°C, the primary recrystallization of other oriented grains is completed before the primary recrystallization of the Goss-oriented grains is completed, so the effect of increasing the Goss-oriented grains is reduced, which is not preferred.

[0097] In addition, when the average heating rate between 550°C and 700°C is set to 400°C / s or more, the Goss oriented grains before the secondary recrystallization can be further increased, and the magnetic flux density of the final grain-oriented electrical steel sheet can be further improved, so it is more preferred. When the average heating rate between 550°C and 700°C is set to 700°C / s or more, the magnetic flux density of the grain-oriented electrical steel sheet can be further improved, so it is extremely preferred. When the average heating rate between 550°C and 700°C is lower than 100°C / s, sufficient Goss oriented grains cannot be obtained for improving the magnetic properties by secondary recrystallization, so it is not preferred. On the other hand, the upper limit of the average heating rate between 550°C and 700°C is not particularly limited, but from the viewpoint of equipment and manufacturing cost, it can be set to 3000°C / s, for example. It should be noted that the heating start temperature of the primary recrystallization annealing, the heating mode other than the rapid heating of 550°C to 700°C, and the reaching temperature are not particularly limited.

[0098] The increase in inhibitor strength on the surface side of the steel plate and in a certain depth range of the surface of the steel plate brought about by the treatment of bringing the solution into contact with the steel plate (solution contact treatment) described later and the increase in Goss-oriented grains brought about by the rapid temperature increase of the primary recrystallization annealing have a synergistic effect on the improvement of magnetic properties. As a mechanism, it is believed that due to the increase in inhibitor strength, the growth of abnormal grains other than Goss-oriented grains near the surface can be suppressed during the final annealing temperature increase, resulting in the promotion of abnormal grain growth of many Goss-oriented grains.

[0099] Such rapid temperature increase can be performed by, for example, using an electric heating method or an induction heating method.

[0100] Here, the heating process may be implemented by multiple devices. For example, maintaining or slowly cooling at a low temperature compared to 550°C, which causes recovery of the steel plate, i.e., a reduction in the dislocation density in the steel, can also improve the temperature uniformity of the steel plate before heating, and thus may be implemented. Furthermore, a heating process including heating from 550°C to 700°C may be implemented by one or more devices.

[0101] The point where the temperature rise starts is the point where the temperature of the steel plate changes from a state where the temperature is lowered to a state where the temperature of the steel plate rises on the low temperature side below 550°C (i.e., the point where the temperature change takes a minimum value). In addition, the point where the temperature rise ends is the point where the temperature of the steel plate changes from a state where the temperature is raised to a state where the temperature of the steel plate falls on the high temperature side above 700°C (i.e., the point where the temperature change takes a maximum value).

[0102] However, by configuring a plurality of heating devices, the temperature of the steel plate may continue to rise on the high temperature side compared to the heating process including 700° C. In such a case, for example, the rapid heating end point may be set to a point above 700° C. where the rate of change of the heating rate becomes negative and minimum.

[0103] Here, the method for determining the starting point of the temperature increase and the end point of the rapid temperature increase is not particularly limited. For example, it can be determined by measuring the temperature of the steel plate using a radiation thermometer or the like. It should be noted that there is no particular limitation on the method for measuring the temperature of the steel plate. In addition, regardless of whether the end temperature of the temperature increase of the primary recrystallization becomes a low temperature or a high temperature compared to the subsequent decarburization annealing temperature, the effect of the present invention will not be impaired. In the case where the end temperature of the temperature increase of the primary recrystallization becomes a low temperature compared to the decarburization annealing temperature, heating can also be performed through the decarburization annealing process. In the case where the end temperature of the temperature increase of the primary recrystallization becomes a high temperature compared to the decarburization annealing temperature, an exothermic treatment or a gas cooling treatment can also be performed to cool the temperature of the steel plate. Furthermore, after cooling to a low temperature compared to the decarburization annealing temperature, reheating can also be performed through the decarburization annealing process.

[0104] However, when it is difficult to measure the temperature of the steel plate and it is difficult to estimate the exact positions of the heating start point and the rapid heating end point, these positions can be estimated by analogy with each heating mode of the heating process and the cooling process. In addition, the inlet side temperature and outlet side temperature of the steel plate in the heating device during the heating process can be set as the heating start point and the rapid heating end point.

[0105] (Intermediate processing)

[0106] In addition, in one embodiment of the present invention, an intermediate treatment step may be provided between the heating step and the decarburization annealing step in the primary recrystallization annealing, the dew point temperature of the atmosphere in the intermediate treatment step is greater than -40°C and less than 0°C, and the residence time at which the steel plate temperature is greater than 700°C and less than 950°C is set to greater than 1 second and less than 20 seconds.

[0107] As described in detail in the following paragraph, by modifying the conditions of the solution contact treatment, the inhibitor can be controlled in the thickness direction of the steel sheet to improve the magnetic properties. On the other hand, the solution contact treatment sometimes generates a new disadvantage of uneven color of the steel sheet appearance. The uneven color of the steel sheet appearance is caused by the state of oxide film formation after decarburization annealing. More specifically, if internal oxidation occurs unevenly, the steel sheet appearance will have uneven color. The inventors have found that the occurrence of uneven color can be suppressed by controlling the atmosphere and temperature conditions before decarburization annealing, that is, during the intermediate treatment.

[0108] When the dew point temperature of the atmosphere in the intermediate treatment step is lower than -40°C, the oxide film formation becomes uneven in the subsequent decarburization annealing, and the appearance of the grain-oriented electrical steel sheet obtained as the final product becomes uneven in color, which is not preferable. When the dew point temperature of the atmosphere in the intermediate treatment step exceeds 0°C, the oxide film formation becomes uneven in the subsequent decarburization annealing, and the appearance of the grain-oriented electrical steel sheet obtained as the final product becomes uneven in color, which is not preferable.

[0109] If the residence time during the intermediate treatment when the steel sheet temperature is 700°C or higher and 950°C or lower is less than 1 second, the oxide film formation becomes uneven in the subsequent decarburization annealing, and the appearance of the grain-oriented electrical steel sheet obtained as the final product becomes uneven in color, which is not preferred. The upper limit of the residence time during the intermediate treatment when the steel sheet temperature is 700°C or higher and 950°C or lower is not particularly limited, but if it exceeds 20 seconds, the equipment becomes large, which is not preferred.

[0110] Although the mechanism of the influence of the oxide film formation in the subsequent decarburization annealing by the intermediate treatment is not necessarily clear, it is presumed as follows. If a treatment (solution contact treatment) is performed in which a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni (Cu, etc.) is brought into contact with the steel sheet, Mn in a part of MnS, MnSe or MnTe on the surface side of the steel sheet is replaced with these elements. Cu, Hg, Ag, Pb, Cd, Co, Zn or Ni becomes unevenly distributed on the surface of the steel sheet and is locally present in the portion where MnS, etc. is present. Therefore, in the portion where these elements are locally present, internal oxidation in the subsequent decarburization annealing is hindered, and a difference is generated in the amount of internal oxidation from the portion where Cu, Hg, Ag, Pb, Cd, Co, Zn or Ni is not present. Here, it is considered that if a certain amount of oxide film is formed in advance by intermediate treatment before decarburization annealing, internal oxidation sites in the subsequent decarburization annealing are formed over the entire surface of the steel sheet, so that internal oxidation proceeds relatively uniformly.

[0111] When the dew point temperature in the intermediate treatment is lower than -40°C, the amount of oxide film formed in the intermediate treatment becomes insufficient, especially in the portion where Cu, Hg, Ag, Pb, Cd, Co, Zn or Ni is locally present, which is not preferable. On the other hand, it is estimated that when the dew point temperature in the intermediate treatment exceeds 0°C, an externally oxidized silicon dioxide film is formed in the intermediate treatment, and the progress of internal oxidation is suppressed in the subsequent decarburization annealing, and the oxide film becomes thinner, so that the insufficient oxidation amount in the portion where Cu, Hg, Ag, Pb, Cd, Co, Zn or Ni is locally present becomes obvious, and color unevenness remains even in the final product.

[0112] When the steel sheet temperature in the intermediate treatment is 700°C to 950°C, the residence time is less than 1 second because the amount of oxide film formed in the intermediate treatment is insufficient. When the residence time exceeds 20 seconds, the equipment becomes large and therefore is not preferred.

[0113] (Decarburization annealing)

[0114] Next, the cold rolled steel sheet is subjected to decarburization annealing. From the viewpoint of decarburization performance, decarburization annealing may be performed in a moist atmosphere containing hydrogen and nitrogen at a temperature below 900°C. Here, in order not to hinder decarburization performance, the oxygen partial pressure ratio of the atmosphere for decarburization annealing, that is, the water vapor partial pressure P in the atmosphere may be set to 0.1%. H2O With hydrogen partial pressure P H2 Ratio P H2O / P H2 Set to 0.35 or more.

[0115] In addition, from the viewpoint of suppressing the occurrence of color unevenness, the water vapor partial pressure P in the atmosphere may be set toH2O With hydrogen partial pressure P H2 Ratio P H2O / P H2 It is set to be greater than 0.35 and less than 0.60. When the oxygen partial pressure ratio of the atmosphere of decarburization annealing is less than 0.35, the oxide film becomes thinner, and the insufficient oxidation amount in the parts where Cu, Hg, Ag, Pb, Cd, Co, Zn or Ni are locally present becomes obvious, and even color unevenness remains in the final product, so it is not preferred. When the oxygen partial pressure ratio of the atmosphere of decarburization annealing exceeds 0.60, the magnetic properties deteriorate, so it is not preferred. Therefore, the oxygen partial pressure ratio of the atmosphere of decarburization annealing is greater than 0.35 and less than 0.60.

[0116] In addition, in the process of primary recrystallization annealing, the cold-rolled steel sheet may be subjected to reduction annealing immediately after decarburization annealing for the purpose of improving magnetic properties and film properties.

[0117] [Step of performing final annealing]

[0118] After that, the cold rolled steel sheet after the primary recrystallization annealing is subjected to final annealing. At this time, an annealing separator containing MgO as the main component may be applied before the final annealing for the purpose of preventing sintering between steel sheets, forming a primary film, controlling the secondary recrystallization behavior, etc. The annealing separator is generally applied to the surface of the steel sheet in the form of a water slurry and dried, but an electrostatic coating method or the like may also be used.

[0119] Next, final annealing is performed for the purpose of primary film formation and secondary recrystallization. Final annealing can also be performed by heat treating the coiled steel sheet using a batch heating furnace, etc. Furthermore, in order to further reduce the iron loss value of the final grain-oriented electromagnetic steel sheet, a purification treatment can be performed in which the coiled steel sheet is heated to a temperature of about 1200°C and then maintained.

[0120] The final annealing is generally heated from room temperature. The heating rate of the final annealing is various, but it is not particularly limited in the present invention, and general final annealing conditions can be used. For example, from the perspective of productivity and general equipment constraints, it can also be set to 5°C / h to 100°C / h. In addition, it can also be carried out in other well-known heating modes. During the cooling process, the heating mode is not particularly limited.

[0121] The atmosphere gas composition in the final annealing is not particularly limited. During the secondary recrystallization process, it can also be a mixed gas of nitrogen and hydrogen. It can be a dry atmosphere or a wet atmosphere. Purification annealing can also be dry hydrogen.

[0122] [Step of performing planarization annealing]

[0123] Next, after the final annealing, an insulating film having aluminum phosphate or colloidal silica as a main component is applied to the surface of the steel sheet for the purpose of imparting insulation and tension to the steel sheet. Thereafter, a flattening annealing is performed for the purpose of sintering the insulating film and flattening the shape of the steel sheet by the final annealing. It should be noted that the composition of the insulating film is not particularly limited as long as insulation and tension are imparted to the steel sheet. It should be noted that in this embodiment, of course, magnetic domain control treatment may be performed on the grain-oriented electromagnetic steel sheet according to the purpose of the demander.

[0124] [Step of subjecting the steel sheet to shot peening and / or leveling treatment and contacting it with a solution]

[0125] In this process, at least one of the hot-rolled steel sheet, the hot-rolled annealed steel sheet, the cold-rolled steel sheet, and the primary recrystallization annealed steel sheet is subjected to shot peening and / or leveling treatment and then immersed in a solution. The treatment of contacting with a solution (hereinafter sometimes referred to as "solution contact treatment") is carried out at least once after hot rolling and before final annealing in order to control the plate thickness direction inhibitor described later. It should be noted that the shot peening and / or leveling treatment and the step of contacting with a solution may also be carried out in different steps.

[0126] (Solution contact treatment)

[0127] The steps are sequential, and first, the solution contact treatment is described. The solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni (sometimes referred to as "Cu, etc." in this specification), the total concentration of each element is 0.00001% or more and 1.0000% or less by mass%, the pH is -1.5 or more and less than 7, the liquid temperature is 15°C or more and 100°C or less, and the steel plate is immersed in the solution for 5 seconds or more and 200 seconds or less.

[0128] When the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the solution is less than 0.00001%, the inhibitor control effect in the thickness direction becomes insufficient, which is not preferred. When the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the solution exceeds 1.0000%, in addition to the saturation of the effect of improving magnetism, the cost of the solution increases, which is not preferred. Therefore, the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the solution is 0.00001% or more and 1.0000% or less.

[0129] In addition, when the pH of the solution is lower than -1.5, the acidity becomes too strong and the solution handling becomes difficult, which is not preferred. When the pH of the solution is 7 or more, the inhibitor control effect in the plate thickness direction by the solution contact treatment becomes insufficient, which is not preferred. Therefore, the pH of the solution is -1.5 or more and lower than 7.

[0130] In addition, when the liquid temperature of the solution is lower than 15°C, the inhibitor control effect in the plate thickness direction by the solution contact treatment becomes insufficient, which is not preferred. When the liquid temperature of the solution exceeds 100°C, the solution handling becomes difficult, which is not preferred. Therefore, the liquid temperature of the solution is 15°C or higher and 100°C or lower.

[0131] In addition, when the time for immersing the steel plate in the solution during the solution contact treatment is less than 5 seconds, the inhibitor control effect in the plate thickness direction by the solution contact treatment becomes insufficient, which is not preferred. When the time for immersing the steel plate in the solution during the solution contact treatment exceeds 200 seconds, the equipment becomes large, which is not preferred. Therefore, the time for immersing the steel plate in the solution during the solution contact treatment is 5 seconds or more and 200 seconds or less.

[0132] The mechanism of the inhibitor that can control the thickness direction of the plate by solution contact treatment is estimated as follows. If one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni (sometimes referred to as "Cu, etc." in this specification) are contained in the solution, the affinity of the element with S, Se and Te in the solution is very high, so it replaces Mn of the precipitates of MnS, MnSe and MnTe (sometimes referred to as "MnS, etc." in this specification) exposed on the surface of the steel plate to form a compound. This reaction is easily caused on the surface side of the precipitates such as MnS, especially in contact with the solution. It is believed that if Mn is replaced with other metal elements (Cu, etc.) on the surface side of precipitates such as MnS, the compounds on these surface sides become obstacles, which can inhibit the dissolution of Mn, S, Se and Te on the central side of precipitates such as MnS into steel, thereby inhibiting the Ostwald growth of MnS, etc. in the final annealing process, and the heat resistance of precipitates such as MnS, that is, the inhibitor strength increases. If a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni (Cu, etc.) contacts MnS, MnSe or MnTe (MnS, etc.), this reaction will occur. Therefore, it is believed that if there are defects such as cracks and voids in the surface layer of the steel plate through shot peening and leveling, the solution penetrates into the steel plate through these spaces, reacting not only with MnS, etc. exposed on the outermost surface of the steel plate, but also with MnS, etc. in a certain depth range of the surface layer of the steel plate, thereby increasing the inhibitor strength.

[0133] (Shot Peening)

[0134] By introducing defects such as cracks and voids into the surface of the steel plate through shot peening and other treatments, the solution penetrates into the steel plate through these spaces through the subsequent solution contact treatment, and the solution not only reaches the outermost surface of the steel plate, but also reaches a certain depth. Through the above-mentioned solution treatment, the Mn on the surface of MnS, MnSe and MnTe (sometimes referred to as "MnS, etc." in this specification) which are precipitates and act as inhibitors is replaced with Cu, etc., which can improve the heat resistance of the inhibitor. Therefore, by shot peening, the solution can penetrate not only to the outermost surface of the steel plate, but also to a certain depth of the steel plate, and the strength of the inhibitors such as MnS present here can be strengthened.

[0135] The conditions for shot peening are: the average particle size of the projection material is greater than 0.1 mm and less than 5.0 mm, and the projection speed is greater than 10 m / s and less than 150 m / s. As a result, fine cracks infiltrated by the solution are introduced into the surface of the steel plate. As the projection material (projection material), general materials can be used, or iron balls with a hardness of about Hv500 can be used. When the average particle size of the projection material is less than 0.1 mm, fine cracks cannot be fully obtained. When the average particle size of the projection material exceeds 5.0 mm, the shape of the steel plate is deformed and it is difficult to deform uniformly during cold rolling, and good magnetic properties cannot be obtained. In addition, when the projection speed is less than 10 m / s, fine cracks cannot be fully obtained. When the projection speed exceeds 150 m / s, the shape of the steel plate is deformed and it is difficult to deform uniformly during cold rolling, and good magnetic properties cannot be obtained. The shape of the projection material is generally roughly divided into a spherical shape and an angular shape. Generally speaking, the angular-shaped projection material has a high grinding ability and can quickly introduce cracks on the surface of the steel plate. In the present invention, either the angular injection material or the spherical injection material can be used. The angular injection material and the spherical injection material can also be mixed and used.

[0136] (Leveling Processing)

[0137] As a method of introducing defects such as cracks and voids into the surface of a steel plate, leveling treatment can be used in addition to shot peening. Leveling treatment can also be used instead of shot peening, and shot peening and leveling can also be used together.

[0138] Leveling ensures the flatness of the steel sheet by bending and rebending the steel sheet along the leveling roller while applying tension to the steel sheet. Through the bending and rebending during leveling, defects such as cracks and voids can be introduced into the surface of the steel sheet. Therefore, through the subsequent solution contact treatment, the solution penetrates into the steel sheet through spaces such as cracks and voids, and the solution can reach not only the outermost surface of the steel sheet, but also a certain depth.

[0139] The conditions for leveling are: the bending number of the steel plate is more than 2 times, the bending angle is more than 10 degrees and less than 90 degrees, and the bending radius is more than 10 mm and less than 200 mm. As a result, fine cracks infiltrated by the solution are introduced into the surface of the steel plate. When the bending number is less than 2 times, fine cracks cannot be fully obtained. In addition, when the bending angle is less than 10 degrees, fine cracks cannot be fully obtained. When the bending angle exceeds 90 degrees, the shape of the steel plate is deformed and it is difficult to deform uniformly during cold rolling, and good magnetic properties cannot be obtained. Furthermore, when the bending radius is less than 10 mm, the shape of the steel plate is deformed and it is difficult to deform uniformly during cold rolling, and good magnetic properties cannot be obtained. When the bending radius exceeds 200 mm, fine cracks cannot be fully obtained.

[0140] (Method for confirming that the surface of "MnS, etc." precipitates is replaced by "Cu, etc.")

[0141] A method for confirming that the surface of precipitates such as MnS is replaced by Cu or the like will be described.

[0142] First, the steel plate sample to be confirmed is mirror-polished and SEM-EDX observed. In the observation image using SEM, the presence of precipitates such as MnS can be confirmed. In the observation image, the element mapping and intensity ratio of EDX of Cu, such as Mn, S, and Cu are overlapped. Thus, the constituent elements of the precipitate particles can be confirmed. In a typical example, if the precipitate particles and their vicinity are observed, the mapping intensity ratio of Mn to S rises in the part of the precipitate particles, and it can be confirmed that the particle is a MnS particle, and if the mapping intensity ratio of Cu also rises in the part near the surface of the particle, it is inferred that the surface of the precipitate is replaced by Cu.

[0143] Then, the element distribution state in the precipitate particles is confirmed by Auger electron spectroscopy. More specifically, by performing Ar sputtering at several nm intervals (typically 1 nm intervals) on the surface of precipitates such as MnS using Auger electron spectroscopy, element analysis can be performed, and the distribution of constituent elements can be confirmed from the surface of the precipitate particles to the inside thereof. If Cu etc. is detected at a high concentration only in the surface of precipitates such as MnS, and the concentration of Cu etc. in the inside of the precipitate is reduced, it can be regarded as that the surface of the precipitate is replaced by Cu etc.

[0144] In addition, in the present embodiment, it is believed that since cracks, voids, etc. are introduced into the surface of the steel plate by shot peening and leveling, the solution penetrates into the steel plate through these spaces, and reacts not only with the MnS, etc. exposed on the outermost surface of the steel plate, but also with the MnS, etc. within a certain depth range of the surface of the steel plate. Through the above-mentioned confirmation method, it is possible to confirm the depth at which the surface of the "MnS, etc." precipitates is replaced by "Cu, etc.". From the perspective of strengthening the strength of the inhibitor, it is preferred that the surface of the "MnS, etc." precipitates is replaced by "Cu, etc." to a deeper range. Typically, it is preferred that the replacement occurs within a depth range of 10 to 500 μm from the surface of the steel plate.

[0145] For SEM, EDS and Auger electron spectroscopy analysis, the devices and measurement conditions used can be appropriately selected according to the measurement object. In the analysis in this specification, the SEM device is FE-SEM manufactured by JEOL, model JEOL7001F is set to WD10mm, and used at an acceleration voltage of 15kV. The Auger electron spectroscopy analyzer is FE-AES PHI-700 manufactured by PHI, and is used with electron beam: 10kV, 10nA, and ion beam: Ar / 2kV.

[0146] Generally speaking, in the manufacturing process of steel sheets, pickling treatment is performed before the subsequent process for the purpose of removing oxide scale and cleaning the surface of the steel sheet. Typically, pickling treatment may be performed before each cold rolling process from the viewpoint of reducing roll wear during cold rolling, and pickling treatment may be performed before the primary recrystallization annealing from the viewpoint of controlling oxidation of the steel sheet surface during the primary recrystallization annealing, and pickling treatment may be performed before the final annealing from the viewpoint of improving the coating property of the annealing separator, or these pickling treatments may be performed in combination.

[0147] Correspondingly, the pickling process of the steel plate may include a solution contact treatment, and the above-mentioned pH value, liquid temperature, and contact time (pickling time) may be used as the pickling conditions. It should be noted that the inhibitor (precipitate) heat resistance improvement effect of the present technology may also be applied to other steel grades, for example, it may also be applied to non-oriented electromagnetic steel sheets. When applied to other steel grades, the slab composition and process conditions are not limited.

[0148] The final grain-oriented electrical steel sheet can be manufactured through the above steps. According to the manufacturing method of the present embodiment, a grain-oriented electrical steel sheet having excellent magnetic properties can be manufactured.

[0149] In the directional electromagnetic steel sheet of the present embodiment, the magnetic flux density B8 value may also be further controlled. Specifically, in the directional electromagnetic steel sheet of the present embodiment, the magnetic flux density B8 value may also be 1.91T or more, preferably 1.92T or more, more preferably 1.93T or more, further preferably 1.94T or more, and further preferably 1.95T or more. Here, the magnetic flux density B8 value is the magnetic flux density when a magnetic field of 800A / m is applied to the directional electromagnetic steel sheet at 50Hz. When the magnetic flux density B8 value is low, the iron loss value (especially hysteresis loss) of the directional electromagnetic steel sheet becomes large, so it is not preferred. The upper limit of the magnetic flux density B8 value is not particularly limited, but in reality, it can also be set to 2.0T, for example. It should be noted that the magnetic properties of the directional electromagnetic steel sheet such as the magnetic flux density can be measured by a known method. For example, the magnetic properties of a directional electrical steel sheet can be measured by using a method based on the Epstein test specified in JIS C2550, or a single sheet magnetic property test method (Single Sheet Tester: SST) specified in JIS C2556. It should be noted that in research and development, when a steel ingot is formed by a vacuum melting furnace, etc., it becomes difficult to collect a test piece of the same size as that of actual machine manufacturing. In this case, for example, a test piece may be collected in a manner to be 60 mm wide × 300 mm long, and the measurement may be performed according to the single sheet magnetic property test method. Furthermore, in order to obtain a measurement value equivalent to that based on the Epstein test, a correction coefficient may be added to the obtained result. In the present embodiment, the measurement is performed by a measurement method based on the single sheet magnetic property test method.

[0150] The directional electromagnetic steel sheet obtained in this way is processed into a wound core or a laminated core during transformer manufacturing. Here, the appearance of the directional electromagnetic steel sheet is uniform without color unevenness, which is an important factor in gaining the trust of the demander. In one embodiment of the present invention, a color sample can be prepared by dividing the concentration of the color from white to black into 8 equal parts, and the area of ​​50mm×50mm of the steel plate can be subdivided. The color concentration of each subdivided area is determined by the above-mentioned 8-divided color sample, and the case where a color difference of more than 2 levels occurs between these areas is determined as color unevenness. For example, by scanning steel plate samples with various color tones and white and black color samples at the same time, and using commercially available image analysis software to divide the brightness from white to black into 8 equal parts and classify the samples, a color sample can be prepared. By comparing the color sample with the steel plate, it is possible to analyze whether a color difference of more than 2 levels occurs in the area of ​​50mm×50mm of the steel plate.

[0151] The grain-oriented electromagnetic steel sheet of the present embodiment has been described above. The grain-oriented electromagnetic steel sheet of the present embodiment can be manufactured by the above-mentioned method for manufacturing the grain-oriented electromagnetic steel sheet of the present embodiment. However, the present invention is not limited to this method.

[0152] Example

[0153] Hereinafter, a method for manufacturing a grain-oriented electromagnetic steel sheet and a grain-oriented electromagnetic steel sheet according to an embodiment of the present invention will be described in more detail while showing examples. It should be noted that the examples shown below are merely examples of grain-oriented electromagnetic steel sheets according to the present embodiment, and the grain-oriented electromagnetic steel sheets according to the present embodiment are not limited to the examples shown below.

[0154] (Example 1)

[0155] <Manufacturing of Grain-Oriented Electrical Steel Sheet>

[0156] First, a steel ingot containing, by mass%, C: 0.04%, Si: 3.3%, Mn: 0.09%, S: 0.002%, Se: 0.001%, Te: 0.001%, acid-soluble Al: 0.005%, N: 0.003%, and the remainder consisting of Fe and impurities was prepared. The steel ingot was annealed at 1200°C for 1 hour and then hot-rolled to obtain a hot-rolled steel sheet with a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1000°C for 140 seconds, pickled, and then cold-rolled twice with intermediate annealing, shot peening, and solution contact treatment, to obtain a cold-rolled steel sheet with a thickness of 0.23 mm. Here, the shot peening and solution contact treatment conditions after the intermediate annealing were performed according to the conditions shown in Table 1.

[0157] Next, the obtained cold-rolled steel sheet is subjected to a primary recrystallization annealing at 850°C for 180 seconds in a wet hydrogen atmosphere. Here, the heating rate is set to the conditions shown in Table 1. Next, an annealing separator containing MgO is applied to the surface of the steel sheet after the primary recrystallization annealing in the form of a water slurry and dried. Thereafter, a final annealing is performed, and the steel sheet after the final annealing is washed with water. Thereafter, an insulating film having aluminum phosphate and colloidal silica as the main components is applied to the surface of the steel sheet, and then a flattening annealing is performed for the purpose of sintering the insulating film and flattening the steel sheet.

[0158] After the flattened annealed grain-oriented electrical steel sheet obtained above was sheared and strain relief annealed, the magnetic flux density B8 value of the grain-oriented electrical steel sheet of each of the present invention examples and comparative examples was measured using a single plate magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm × 300 mm. Here, the B8 value is the magnetic flux density of the grain-oriented electrical steel sheet when the grain-oriented electrical steel sheet is excited at 800 A / m at 50 Hz. In the present invention, it is set as the average value of 5 samples.

[0159] Here, the condition that the magnetic flux density B8 value of the grain-oriented electromagnetic steel sheet is 1.91 T or more is judged as good (B), the condition that it is 1.92 T or more is judged as better (A), and the condition that it is 1.93 T or more is judged as very good. In addition, other conditions are judged as bad (C).

[0160] Table 1 shows the production conditions, measurement results, and evaluations of the above-mentioned examples of the present invention and comparative examples.

[0161]

[0162] With reference to the results in Table 1, it can be seen that the grain-oriented electrical steel sheets satisfying the conditions of the present embodiment are judged to be good.

[0163] (Example 2)

[0164] First, a steel ingot containing C: 0.08%, Si: 3.2%, Mn: 0.08%, S: 0.024%, acid-soluble Al: 0.03%, N: 0.008%, and the remainder consisting of Fe and impurities was prepared. The steel ingot was annealed at 1350°C for 1 hour and then hot rolled to obtain a hot-rolled steel sheet with a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1100°C for 140 seconds, flattened and subjected to solution contact treatment, and then cold rolled to obtain a cold-rolled steel sheet with a thickness of 0.23 mm. Here, the flattening treatment and the solution contact treatment conditions after the hot-rolled sheet annealing were performed according to the conditions shown in Table 2.

[0165] Next, the obtained cold-rolled steel sheet is subjected to a primary recrystallization annealing at 850°C for 180 seconds in a wet hydrogen atmosphere. Here, the heating rate is set to the conditions shown in Table 2. Next, an annealing separator containing MgO is applied to the surface of the steel sheet after the primary recrystallization annealing in the form of a water slurry and dried. Thereafter, a final annealing is performed, and the steel sheet after the final annealing is washed with water. Thereafter, an insulating film having aluminum phosphate and colloidal silica as main components is applied to the surface of the steel sheet, and then a flattening annealing is performed for the purpose of sintering the insulating film and flattening the steel sheet.

[0166] After the flattened annealed grain-oriented electrical steel sheet obtained above was sheared and strain relief annealed, the magnetic flux density B8 value of the grain-oriented electrical steel sheet of each of the present invention examples and comparative examples was measured using a single plate magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm × 300 mm. Here, the B8 value is the magnetic flux density of the grain-oriented electrical steel sheet when the grain-oriented electrical steel sheet is excited at 800 A / m at 50 Hz. In the present invention, it is set as the average value of 5 samples.

[0167] Here, the condition that the magnetic flux density B8 value of the grain-oriented electrical steel sheet is 1.92 T or more is judged as good (B), the condition that it is 1.93 T or more is judged as better (A), and the condition that it is 1.94 T or more is judged as very good.

[0168] Table 2 shows the production conditions, measurement results, and evaluations of the above-mentioned examples of the present invention and comparative examples.

[0169]

[0170] Referring to the results in Table 2, it is understood that the grain-oriented electrical steel sheets satisfying the conditions of the present embodiment are judged to be good.

[0171] (Example 3)

[0172] First, a steel ingot containing, by mass%, C: 0.08%, Si: 3.3%, Mn: 0.08%, S: 0.025%, acid-soluble Al: 0.03%, N: 0.008%, and the remainder consisting of the components shown in Table 3, Fe, and impurities was prepared. The steel ingot was annealed at 1350°C for 1 hour and then hot-rolled to obtain a hot-rolled steel sheet with a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1100°C for 140 seconds, shot peened and subjected to solution contact treatment, and then cold-rolled to obtain a cold-rolled steel sheet with a thickness of 0.23 mm. Here, the conditions for shot peening and solution contact treatment after hot-rolled plate annealing are set as follows: average particle size of shot: 2 mm, projection speed: 50 m / s, shape: angular, Cu concentration in solution: 0.001%, solution (basic component): hydrochloric acid, pH of solution: 3, solution temperature: 70°C, contact time between solution and steel plate: 30 seconds.

[0173] Next, the obtained cold-rolled steel sheet is subjected to a primary recrystallization annealing at 850°C for 180 seconds in a wet hydrogen atmosphere. Here, the heating rate is carried out under the conditions shown in Table 3. Next, an annealing separator containing MgO is applied to the surface of the steel sheet after the primary recrystallization annealing in the form of a water slurry and dried. Thereafter, a final annealing is performed, and the steel sheet after the final annealing is washed with water. Thereafter, an insulating film having aluminum phosphate and colloidal silica as the main components is applied to the surface of the steel sheet, and then a flattening annealing is performed for the purpose of sintering the insulating film and flattening the steel sheet.

[0174] After the flattened annealed grain-oriented electrical steel sheet obtained above was sheared and strain relief annealed, the magnetic flux density B8 value of the grain-oriented electrical steel sheet of each of the present invention examples and comparative examples was measured using a single plate magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm × 300 mm. Here, the B8 value is the magnetic flux density of the grain-oriented electrical steel sheet when the grain-oriented electrical steel sheet is excited at 800 A / m at 50 Hz. In the present invention, it is set as the average value of 5 samples.

[0175] Here, the condition that the magnetic flux density B8 value of the grain-oriented electromagnetic steel sheet is 1.92 T or more is judged as good (B), the condition that it is 1.93 T or more is judged as better (A), the condition that it is 1.94 T or more is judged as very good (S), and the condition that it is 1.95 T or more is judged as the best (SS).

[0176] Table 3 shows the production conditions, measurement results, and evaluations of the above-mentioned examples of the present invention and comparative examples.

[0177] Table 3

[0178]

[0179] With reference to the results in Table 3, it can be seen that the grain-oriented electrical steel sheets satisfying the conditions of the present embodiment are judged to be good.

[0180] (Example 4)

[0181] The grain-oriented electrical steel sheets were manufactured under the same conditions as those of Examples 1 to 3, except that various conditions were used for the intermediate treatment between the heating of the primary recrystallization annealing and the decarburization annealing (dew point temperature of the atmosphere, residence time at a steel sheet temperature of 700°C or higher and 950°C or lower) and the decarburization annealing (oxygen partial pressure ratio of the atmosphere).

[0182] The sample of the grain-oriented electrical steel sheet obtained above was cut, and it was determined whether a color tone difference of two levels or more occurred in the case of dividing the brightness from white to black into 8 equal parts in an area of ​​50 mm×50 mm. If the color tone difference was one level or less, it was determined that the color unevenness was good, and if the color tone difference was two levels or more, it was determined that the color unevenness was poor.

[0183] In addition, after the flattening annealed grain-oriented electrical steel sheet sample was sheared and strain relief annealed, the magnetic flux density B8 value of the grain-oriented electrical steel sheet of each of the present invention examples and comparative examples was measured using a single plate magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm × 300 mm. Here, the B8 value is the magnetic flux density of the grain-oriented electrical steel sheet when the grain-oriented electrical steel sheet is excited at 800 A / m at 50 Hz. In the present invention, it is set to the average value of 5 samples.

[0184] Here, the condition that there is no color tone difference of two or more levels and the magnetic flux density B8 value of the grain-oriented electrical steel sheet is 1.91 T or more is judged as the best (B). In addition, other conditions are judged as poor (C).

[0185] It is known that in the intermediate treatment, the dew point temperature of the atmosphere is -40°C or higher and 0°C or lower, and the residence time of the steel plate temperature is 700°C or higher and 950°C or lower is 1 second or higher and 20 seconds or lower, and in the decarburization annealing, the oxygen partial pressure ratio (P H2O / P H2 ) is 0.35 or more and 0.60 or less, a good determination result (B) is obtained in which there is no color tone difference of two or more levels and the magnetic flux density B8 value of the grain-oriented electrical steel sheet is 1.91 T or more.

Claims

1. A method for manufacturing a grain-oriented electromagnetic steel sheet, characterized in that: Including the following processes: A process of obtaining a hot-rolled steel sheet by heating and hot-rolling a slab, or obtaining a hot-rolled annealed steel sheet by hot-rolling the hot-rolled steel sheet, wherein the slab contains, by mass%, C: 0.01% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.50%, a total of one or more of S, Se and Te: 0.001% to 0.050%, acid-soluble Al: more than 0% to 0.05%, N: more than 0% to 0.015%, and the remainder is Fe and impurities; A step of obtaining a cold-rolled steel sheet by cold-rolling the hot-rolled steel sheet or the hot-rolled annealed steel sheet; A step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet; A step of applying an annealing separator containing MgO to the surface of the primary recrystallization annealed sheet and then performing final annealing to obtain a final annealed sheet; and After the insulating film is applied to the final annealed sheet, a planarization annealing step is performed. wherein at least one of the hot-rolled steel sheet, the hot-rolled annealed steel sheet, the cold-rolled steel sheet, and the primary recrystallization annealed steel sheet is subjected to a shot peening treatment and a treatment of contacting with a solution, In the shot peening, the average particle size of the shot material is 0.1 mm or more and 5.0 mm or less, and the shot speed is 10 m / s or more and 150 m / s or less. The solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is greater than 0.00001% and less than 1.0000%, the pH is greater than -1.5 and less than 7, the liquid temperature is greater than 15°C and less than 100°C, and the steel plate is immersed in the solution for a time of greater than 5 seconds and less than 200 seconds.

2. A method for manufacturing a grain-oriented electromagnetic steel sheet, characterized in that: Including the following processes: A process of obtaining a hot-rolled steel sheet by heating and hot-rolling a slab, or obtaining a hot-rolled annealed steel sheet by hot-rolling the hot-rolled steel sheet, wherein the slab contains, by mass%, C: 0.01% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.50%, a total of one or more of S, Se and Te: 0.001% to 0.050%, acid-soluble Al: more than 0% to 0.05%, N: more than 0% to 0.015%, and the remainder is Fe and impurities; A step of obtaining a cold-rolled steel sheet by cold-rolling the hot-rolled steel sheet or the hot-rolled annealed steel sheet; A step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet; A step of applying an annealing separator containing MgO to the surface of the primary recrystallization annealed sheet and then performing final annealing to obtain a final annealed sheet; and After the insulating film is applied to the final annealed sheet, a planarization annealing step is performed. wherein at least one of the hot-rolled steel sheet, the hot-rolled annealed steel sheet, the cold-rolled steel sheet, and the primary recrystallization annealed steel sheet is subjected to a flattening treatment and a treatment of contacting with a solution, In the leveling process, the steel sheet is bent twice or more, the bending angle is 10 degrees or more and 90 degrees or less, and the bending radius is 10 mm or more and 200 mm or less. The solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is greater than 0.00001% and less than 1.0000%, the pH is greater than -1.5 and less than 7, the liquid temperature is greater than 15°C and less than 100°C, and the steel plate is immersed in the solution for a time of greater than 5 seconds and less than 200 seconds.

3. The method for manufacturing a grain-oriented electrical steel sheet according to claim 1 or 2, wherein: In the rapid heating of the primary recrystallization annealing, the average heating rate in the temperature range of 550° C. to 700° C. is 100° C. / s or more and 3000° C. / s or less.

4. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 3, wherein: The slab contains one or more selected from the group consisting of Cu: 1.0% or less, Sn: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Sb: 1.0% or less, and Bi: 1.0% or less, in place of a portion of the Fe.

5. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 4, wherein: The primary recrystallization annealing includes a step of heating, a step of performing an intermediate treatment between heating and decarburization annealing, and a step of performing decarburization annealing. In the intermediate treatment, the dew point temperature of the atmosphere is -40°C to 0°C and the residence time of the steel sheet temperature is 700°C to 950°C for 1 second to 20 seconds. In the decarburization annealing, the oxygen partial pressure ratio of the atmosphere, i.e., P H2O / P H2 It is 0.35 or more and 0.60 or less.

Citation Information

Patent Citations

  • JP1976013469B2

  • Production of grain-oriented silicon steel sheet having extremely low iron loss

    JP1994212274A

  • Grain oriented silicon steel sheet having extremely low iron loss

    JP1995268567A

  • Method of producing grain oriented silicon steel sheet having excellent coating property

    JP2003193141A

  • Method for producing grain-oriented silicon steel sheet

    JP2016156068A