A high-density all-silk anti-velvet jacquard fabric
By grafting antibacterial aerogel on the surface of silk fibers and filling the fiber gaps, the problem of poor anti-foil effect of silk fiber braided base fabric is solved, the combination of high density and breathability is achieved, and the antibacterial properties of silk fibers are imparted.
Patent Information
- Application Number
- CN202210781670.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-07-05
AI Technical Summary
The base fabric woven by silk fiber cannot achieve good anti-lint effect due to the large pores between the fibers.
Graft the antibacterial aerogel (lightweight porous nanoparticles composed of SiO2 and TiO2) on the surface of silk fibers, and the silk fibers are pretreated and woven into cloth, filling the fiber gaps for high density and anti-lint effects while maintaining Breathability.
The preparation of high-density all-silk anti-shell jacquard fabrics is achieved, which significantly reduces down escape and imparts photoant antibacterial properties to silk fibers.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile fibers, and in particular relates to a high-density all-silk anti-velvet jacquard fabric. Background Art
[0002] With the intensification of market competition and the rapid changes in consumers' aesthetic concepts, popular fabrics tend to be high-count, high-density, and light and thin. High-count and high-density products are the preferred products for clothing fabrics. High-count and high-density cotton products require light texture, delicate and soft touch, and bright luster like silk, while maintaining the unique comfort of high-density cotton fabrics. The market's requirements for ultra-high-end clothing and home textile fabrics are getting higher and higher. They are no longer limited to novel colors and patterns, but also require comfortable wearing, smooth touch and soft luster. This requires that the production of high-end clothing and home textile fabrics must take a product development route with high-end varieties and high technical content.
[0003] In the prior art, waterproof and breathable fabrics made of synthetic fiber nylon or polyester can be made into down-proof fabrics by a calendering finishing process to minimize down escape. However, real silk cannot be calendered, and the base cloth woven from silk fibers cannot achieve a good down-proof effect due to the large pores between the fibers. Therefore, the present invention provides a high-density all-silk down-proof jacquard fabric to solve the problems existing in the prior art. Summary of the invention
[0004] The purpose of the present invention is to provide a high-density all-silk anti-down jacquard fabric. By grafting antibacterial aerogel (lightweight porous nanoparticles composed of SiO2 and TiO2) onto the surface of silk fibers, the gaps on the surface of silk fibers are reduced to prevent down from escaping. The antibacterial aerogel has a porous structure and does not affect the air permeability of the material, and gives the silk fibers light-induced antibacterial properties.
[0005] The technical problem to be solved by the present invention is that real silk cannot be calendered, and the base cloth woven from silk fibers cannot achieve a good down-proof effect due to the large pores between the fibers.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A high-density all-silk anti-velvet jacquard fabric is prepared by the following steps:
[0008] S1, pre-treating the silk fibers to remove sericin, thereby obtaining pre-treated silk fibers, wherein the pre-treatment is specifically as follows: boiling the silk in a sodium carbonate solution for 0.5 h, then rinsing with deionized water for 2-3 times, and repeating the above steps for 2 times, thereby effectively removing the sericin;
[0009] S2, grafting antibacterial aerogel on the surface of the pretreated silk fiber to obtain silk fiber grafted with antibacterial aerogel;
[0010] S3, weaving the silk fibers grafted with antibacterial aerogel into cloth to obtain a high-density all-silk anti-velvet jacquard fabric;
[0011] The antibacterial aerogel is a lightweight porous nanoparticle composed of SiO2 and TiO2.
[0012] Furthermore, the usage ratio of silk to sodium carbonate solution is 0.005-0.01 g: 1-2 mL.
[0013] Furthermore, the antibacterial aerogel is prepared by the following steps:
[0014] Tetrabutyl titanate, acetic acid and tetraethyl orthosilicate are added to anhydrous ethanol under stirring, and then a mixture of acetic acid and distilled water is added dropwise to form a sol, which gradually transforms into a wet gel. After aging at room temperature for 24 hours, the wet gel is immersed in a mixed solution consisting of ethanol and ammonia for 72 hours. Thereafter, the gel is washed in ethanol at 60°C for 72 hours, dried at 60°C for 48 hours, and then heat treated at 400-800°C for 5 hours to obtain an antibacterial aerogel.
[0015] Furthermore, the usage ratio of tetrabutyl titanate, acetic acid, tetraethyl orthosilicate and anhydrous ethanol is 3-4 mL: 0.5-0.6 mL: 3-4 mL: 10-15 mL.
[0016] Further, the wet gel was immersed in a mixed solution consisting of ethanol and ammonia for 72 hours, with the solution being replaced every 24 hours, and the gel was washed in ethanol at 60° C. for 72 hours, with the solution being replaced every 24 hours.
[0017] Further, heat treatment was then performed at 400-800° C. for 5 hours with a heating rate of 5° C. / min.
[0018] Furthermore, the antibacterial aerogel is grafted onto the surface of the pretreated silk fiber by ultrasonically dispersing the pretreated silk in ethanol, adding the antibacterial aerogel, and stirring and mixing for 3-6 hours.
[0019] Furthermore, the dosage ratio of the pretreated silk, ethanol and antibacterial aerogel is 0.05-0.1 g: 10-20 mL: 0.01-0.03.
[0020] Beneficial effects of the present invention:
[0021] (1) In the technical solution of the present invention, antibacterial aerogel is grafted onto the surface of pretreated silk fibers. The antibacterial aerogel is a lightweight porous nanoparticle composed of SiO2 and TiO2. The surface of the pretreated silk fibers contains a large number of oxygen-containing functional groups. The lightweight porous nanoparticles can be adsorbed onto the surface of the silk fibers by interacting with these oxygen-containing functional groups. After being woven into cloth in the later stage, the nanoparticles can fill the gaps in the fibers, thereby realizing the preparation of high-density all-real silk and achieving a better anti-down effect.
[0022] (2) In the technical scheme of the present invention, an antibacterial aerogel is grafted onto the surface of pretreated silk fibers, wherein the antibacterial aerogel uses tetraethoxysilane and tetrabutyl titanate as precursors to prepare a SiO2 / TiO2 nanocomposite aerogel (Si / Ti=1:1) with a high surface area, without the need for surface modification using organic silane. The antibacterial mechanism is as follows: the oxidized ROS is obtained by the photocatalytic reaction of TiO2 under light, in particular, ROS such as superoxide anion radicals (•O 2- ), hydroxyl radicals (•OH) and hydrogen peroxide (H2O2) are the main substances that cause bacterial death. These ROS can penetrate the bacterial cell membrane and oxidize the mediated proteins, resulting in the loss of enzyme function associated with the biofilm. Therefore, the microbial cells are degraded and killed. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1
[0025] The antibacterial aerogel is prepared by the following steps:
[0026] 3mL of tetrabutyl titanate, 0.5mL of acetic acid and 3mL of tetraethyl orthosilicate were added to 10mL of anhydrous ethanol under stirring, and then a mixture of 0.5mL of acetic acid and 1mL of distilled water was added dropwise to form a sol, which gradually turned into a wet gel. After aging at room temperature for 24 hours, the wet gel was immersed in a mixed solution consisting of ethanol and ammonia for 72 hours, and the solution was replaced every 24 hours. After that, the gel was washed in ethanol at 60°C for 72 hours, and the solution was replaced every 24 hours. It was dried at 60°C for 48 hours and then heat treated at 400°C for 5 hours with a heating rate of 5°C / min to obtain an antibacterial aerogel.
[0027] Example 2
[0028] The antibacterial aerogel is prepared by the following steps:
[0029] 3.5 mL of tetrabutyl titanate, 0.55 mL of acetic acid and 3.5 mL of tetraethyl orthosilicate were added to 12 mL of anhydrous ethanol under stirring, and then a mixture of 0.55 mL of acetic acid and 1.5 mL of distilled water was added dropwise to form a sol, which gradually turned into a wet gel. After aging at room temperature for 24 hours, the wet gel was immersed in a mixed solution consisting of ethanol and ammonia for 72 hours, and the solution was replaced every 24 hours. After that, the gel was washed in ethanol at 60°C for 72 hours, and the solution was replaced every 24 hours. It was dried at 60°C for 48 hours and then heat treated at 600°C for 5 hours with a heating rate of 5°C / min to obtain an antibacterial aerogel.
[0030] Example 3
[0031] The antibacterial aerogel is prepared by the following steps:
[0032] 4 mL of tetrabutyl titanate, 0.6 mL of acetic acid and 4 mL of tetraethyl orthosilicate were added to 15 mL of anhydrous ethanol under stirring, and then a mixture of 0.6 mL of acetic acid and 2 mL of distilled water was added dropwise to form a sol, which gradually turned into a wet gel. After aging at room temperature for 24 hours, the wet gel was immersed in a mixed solution consisting of ethanol and ammonia for 72 hours, and the solution was replaced every 24 hours. After that, the gel was washed in ethanol at 60°C for 72 hours, and the solution was replaced every 24 hours. It was dried at 60°C for 48 hours and then heat treated at 800°C for 5 hours with a heating rate of 5°C / min to obtain an antibacterial aerogel.
[0033] Example 4
[0034] A high-density all-silk anti-velvet jacquard fabric is prepared by the following steps:
[0035] S1, boiling 0.005 g of silk in 1 mL of sodium carbonate solution for 0.5 h, rinsing with deionized water twice, and repeating the above steps twice, thereby effectively removing sericin to obtain pretreated silk fibers;
[0036] S2, ultrasonically dispersing 0.05 g of pretreated silk in 10 mL of ethanol, adding 0.01 g of the antibacterial aerogel prepared in Example 1, stirring and mixing for 3 h, to obtain silk fibers grafted with antibacterial aerogel;
[0037] S3. Weaving the silk fibers grafted with antibacterial aerogel into cloth to obtain high-density all-silk anti-velvet jacquard fabric.
[0038] Example 5
[0039] A high-density all-silk anti-velvet jacquard fabric is prepared by the following steps:
[0040] S1, boiling 0.008 g of silk in 1.5 mL of sodium carbonate solution for 0.5 h, rinsing with deionized water twice, and repeating the above steps twice, thereby effectively removing sericin to obtain pretreated silk fibers;
[0041] S2, ultrasonically dispersing 0.08 g of pretreated silk in 15 mL of ethanol, adding 0.02 g of the antibacterial aerogel prepared in Example 2, stirring and mixing for 4 h, to obtain silk fibers grafted with antibacterial aerogel;
[0042] S3. Weaving the silk fibers grafted with antibacterial aerogel into cloth to obtain high-density all-silk anti-velvet jacquard fabric.
[0043] Example 6
[0044] A high-density all-silk anti-velvet jacquard fabric is prepared by the following steps:
[0045] S1, boiling 0.01 g of silk in 2 mL of sodium carbonate solution for 0.5 h, then rinsing with deionized water 3 times, and repeating the above steps 2 times, thereby effectively removing the sericin to obtain pretreated silk fibers;
[0046] S2, ultrasonically dispersing 0.1 g of pretreated silk in 20 mL of ethanol, adding 0.03 g of the antibacterial aerogel prepared in Example 3, stirring and mixing for 6 h, to obtain silk fibers grafted with antibacterial aerogel;
[0047] S3. Weaving the silk fibers grafted with antibacterial aerogel into cloth to obtain high-density all-silk anti-velvet jacquard fabric.
[0048] Comparative Example
[0049] The difference between this comparative example and Example 6 is that the antibacterial aerogel prepared in Example 3 is not added, and the other steps and raw materials are the same as those in Example 6.
[0050] The high-density all-silk anti-down jacquard fabrics prepared in Examples 4-6 and the comparative example were subjected to performance tests: 1) the anti-down performance of the fabrics was tested in accordance with GB / T 12705.2-2009. If more than 15 drilled piles escaped from the surface of the fabric, the anti-down property of the anti-down fabric was poor; 2) the air permeability was tested in accordance with GB / T 1193-2012. The test results are shown in Table 1 below.
[0051] Table 1
[0052] project Anti-down property (number of escaping from the surface) Air permeability (mm / s) Example 4 3 7 Example 5 5 5 Example 6 4 6 Comparative Example 17 28
[0053] It can be seen from Table 1 above that the high-density all-silk anti-down jacquard fabric prepared in the embodiment of the present invention has better anti-down property and air permeability than that of the comparative example.
[0054] The high-density silk anti-velvet jacquard fabrics prepared in Examples 4-6 and the comparative example were tested for antibacterial properties according to GB / T 20944. The test results are shown in Table 2 below.
[0055] Table 2
[0056] project Escherichia coli antibacterial rate (%) Antibacterial rate of Staphylococcus aureus (%) Example 4 99.2 98.6 Example 5 99.6 98.5 Example 6 99.7 99.2 Comparative Example N N
[0057] Note: N means no antibacterial properties.
[0058] Combining Table 1 and Table 2, it can be seen that by grafting the antibacterial aerogel onto the surface of silk fiber, the gaps on the surface of silk fiber are reduced to prevent down from escaping. The antibacterial aerogel has a porous structure, which does not affect the air permeability of the material and gives the silk fiber photo-induced antibacterial properties.
[0059] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0060] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high-density all-silk anti-velvet jacquard fabric, characterized in that: The method comprises the following steps: S1, pre-treating silk fibers to remove sericin to obtain pre-treated silk fibers; S2, grafting antibacterial aerogel on the surface of pretreated silk fiber to obtain silk fiber grafted with antibacterial aerogel; the pretreatment of silk fiber surface grafting antibacterial aerogel specifically comprises: ultrasonically dispersing the pretreated silk in ethanol, adding the antibacterial aerogel, and stirring and mixing for 3-6 hours; S3, weaving the silk fibers grafted with antibacterial aerogel into cloth to obtain a high-density all-silk anti-velvet jacquard fabric; The antibacterial aerogel is a lightweight porous nanoparticle composed of SiO2 and TiO2; The antibacterial aerogel is prepared by the following steps: Tetrabutyl titanate, acetic acid and tetraethyl orthosilicate are added to anhydrous ethanol under stirring, and then a mixture of acetic acid and distilled water is added dropwise to form a sol, which gradually transforms into a wet gel. After aging at room temperature for 24 hours, the wet gel is immersed in a mixed solution consisting of ethanol and ammonia for 72 hours. Thereafter, the gel is washed in ethanol at 60°C for 72 hours, dried at 60°C for 48 hours, and then heat-treated at 400-800°C for 5 hours with a heating rate of 5°C / min to obtain an antibacterial aerogel; the dosage ratio of tetrabutyl titanate, acetic acid, tetraethyl orthosilicate and anhydrous ethanol is 3-4mL:0.5-0.6mL:3-4mL:10-15mL.
2. The high-density all-silk anti-velvet jacquard fabric according to claim 1, characterized in that: In step S1, the pretreatment is specifically as follows: the silk fibers are boiled in a sodium carbonate solution for 0.5 h, then rinsed with deionized water for 2-3 times, and the above steps are repeated twice, thereby effectively removing the sericin.
3. The high-density all-silk anti-velvet jacquard fabric according to claim 2, characterized in that: The usage ratio of silk fiber to sodium carbonate solution is 0.005-0.01 g: 1-2 mL.
4. The high-density all-silk anti-velvet jacquard fabric according to claim 1, characterized in that: The wet gel was immersed in a mixed solution consisting of ethanol and ammonia for 72 h, with the solution replaced every 24 h. The gel was washed in ethanol at 60 °C for 72 h, with the solution replaced every 24 h.