Method of forming a diamond product

By forming an sp2-bonded damage layer on the diamond material and using electrochemical etching technology with a high conductivity ionic solution, the problems of uneven diamond layer thickness and slow etching rate in the existing technology are solved, achieving efficient and uniform Preparation of thin diamond layers suitable for optical and electronic devices.

CN115151685BActive Publication Date: 2024-10-11ELEMENT SIX TECH LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180016418.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-06
Filing Date
2021-03-04
Publication Date
2024-10-11
Estimated Expiration
2041-03-04

AI Technical Summary

Technical Problem

It is difficult to efficiently produce thin diamond layers with existing technology, especially in optical and quantum electronic devices. Conventional methods result in uneven diamond film thickness, severe damage, slow etching rates, and cannot meet the demand for high-quality diamond layers.

Method used

By forming an sp2-bonded damage layer on the diamond material and removing the damage layer in an electrochemical etching technique in a solution containing high conductivity ions, high oxidation radicals are used to accelerate the etching process and significantly increase the etching rate.

Benefits of technology

It significantly improves the etching rate of the diamond layer, reduces production time and cost, and enables the preparation of more uniform and higher-quality thin diamond layers, which is suitable for optical and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115151685B_ABST
    Figure CN115151685B_ABST
Patent Text Reader

Abstract

A method of forming a diamond product. A diamond material is provided and a sp 2 The damaged layer defines a first diamond layer above and in contact with the damaged layer and a second diamond layer below and in contact with the damaged layer. The damaged layer is electrochemically etched to separate it from the first layer, wherein the electrochemical etching is performed in a solution containing ions, the solution having an electrical conductivity of at least 500 μS cm ‑1 , and wherein the ions are capable of forming free radicals during electrolysis. A diamond product is also described.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] The present invention relates to a method of forming a diamond product, in particular a thin diamond material and / or film.

[0002] introduce

[0003] Thin (submicrometer) diamond films find applications in emerging optical and quantum electronic devices, yet producing these films by conventional methods is extremely difficult.

[0004] Currently, commercially available diamond plates range in thickness from about 5 μm to several millimeters. To achieve such thicknesses, these plates are mechanically polished using diamond abrasives. Polishing to anything thinner than the lower limit is extremely challenging due to the hardness of diamond, and even at these achievable thicknesses, the diamond is wedge-shaped, with varying thickness across the sample. This sample roughness and inhomogeneity limits the manufacturable thickness of the film, ultimately resulting in higher-than-expected average film thicknesses, limiting its use in quantum applications.

[0005] Furthermore, due to the extreme hardness of diamond, abrasive polishing often results in subsurface damage to the diamond, requiring further processing steps if the material is to be used in quantum applications. While this may not be a big problem for bulk diamond, it is far from ideal for thin films such as those used in photonic applications, as it reduces the strength and optical clarity of the diamond. Although other methods such as chemically assisted polishing can be used to reduce this damage, it cannot be completely prevented.

[0006] One technique used to achieve the required submicron thickness is reactive ion etching (RIE). RIE is a dry etching technique that uses a chemically reactive plasma to remove material from the diamond surface. However, RIE is a slow process, typically etching at a rate of tens of nanometers per hour. Therefore, it is only feasible for samples whose thickness is already in the micrometer range. RIE etching is essentially isotropic, meaning that the final morphology is determined by the starting surface. Therefore, applying RIE to wedge-polished diamond will result in a thinner surface, but cannot address variable thickness.

[0007] Work by Parikh et al. (Appl. Phys. Lett. 1992, 61(26), 3124-3126) showed that a combination of ion implantation and etching (wet or dry) could be used to produce thin and uniform diamond films. This method involves the implantation of diamond ions, thereby forming a damaged layer within the diamond where the ions come to rest, at a depth that depends on the energy used. The implantation is followed by an annealing at 950°C for 30 minutes, during which the damaged layer at the end of the range becomes graphitic in nature. The graphitic layer can then be removed using either a wet etch consisting of hot chromium sulphuric acid or a dry etch annealed at 550°C in oxygen. Both removal techniques release a thin layer of diamond above the graphitic layer. The main advantage of this technique is that the ion implantation step produces an etchable layer at a controlled and fixed distance below the surface, thereby ensuring uniform film thickness, even if the two sides of the substrate are not polished parallel. If a thicker or higher quality diamond layer is desired, the substrate can have an additional diamond layer grown on top of it before electrochemical etching and stripping occurs. If desired, the diamond on the original substrate can then be removed by RIE etching, leaving only the higher quality overgrown material.

[0008] Marchywka et al. (Appl. Phys. Lett. 63, 3521 (1993)) have shown that similar membranes can be achieved by using electrochemical etching rather than chemical etching to remove the graphite layer. Here, the sample was placed between platinum electrodes, spaced 2 cm apart, and immersed in distilled water to a depth of 1 cm, with enough chromic acid added to allow only 100 mA of current when a 200 V bias was applied. This voltage was then applied until complete separation of the membrane was achieved. However, under these conditions, the etching rate was extremely slow, requiring 10 hours to separate a 3×3 mm membrane. This produced a 0.9 mm 2 hr -1 The approximate area etch rate of material removed.

[0009] In a subsequent work (J. Electrochem. Soc., 140, 2, (1993)), the same authors specifically advocated the use of high resistivity dielectrics, arguing that in a true bipolar arrangement this would result in a greater portion of the current flowing through the graphite layer implanted within the diamond, thereby increasing the etch rate.

[0010] In a more recent work by Parikh et al. (Nanoscale, 2016, 8, 6860), the authors used 1 MeV helium implantation followed by annealing at 1300 °C. The authors reported an area electrochemical etch rate of 0.25 mm when using a saturated boric acid solution mixed in equal parts with deionized water. 2 hr -1Little explanation is given for the choice of boric acid as the electrolyte. When the experiment was repeated using a 3.5 × 3.5 mm HPHT substrate, implanted with 2 MeV carbon as described more fully in the diamond sample preparation section, a slightly higher rate was found (0.8 ± 0.04 mm 2 hr -1 ).

[0011] In addition to producing thin films, this process using a stripping technique after implantation is applicable to many diamond processing procedures. These include the manufacture of micro-suspended single crystal devices, which require structures that are difficult to make in diamond by traditional methods. Such processes can also be used to separate homoepitaxial CVD diamond from the growth substrate. In particular, the growth of high-quality single crystal diamond requires the use of a high-quality diamond substrate to seed its growth. However, due to the hardness of diamond, it is difficult to remove such a substrate and this results in material loss. Using a stripping technique to remove diamond from the substrate after implantation is a promising approach to alleviate this problem.

[0012] While implantation and stripping techniques have been studied for many different applications, little is known about the etching process. Several etching solutions and electrolytes have been used in the literature, such as boric acid, chromic acid, and tap water, and the common factor in all these studies is that the etching rate is very slow. US5891575A also describes several etching solutions and emphasizes that these solutions should flow 1-100nA cm at an applied potential of 50-300V. -2 When used in an electric current state, this indicates a solution with extremely low conductivity.

[0013] There is a need for an improved process in which the etch rate is increased so that the separation time is reduced. SUMMARY OF THE INVENTION

[0015] Clearly, there is a need for an improved process for producing thin diamond layers having a thickness that makes them suitable for use in optical and electronic devices.

[0016] Against this background, according to a first aspect, there is provided a method of forming a diamond product, the method comprising:

[0017] Provide diamond materials;

[0018] Formation containing sp 2 a damaged layer of bonded carbon, wherein the presence of the damaged layer defines a first diamond layer above and in contact with the damaged layer and a second diamond layer below and in contact with the damaged layer; and

[0019] electrochemically etching the damaged layer to separate the first diamond layer therefrom, wherein the electrochemical etching is performed in a solution containing ions having an electrical conductivity of at least 500 μS cm -1, and wherein the ions are capable of forming free radical species during electrolysis.

[0020] More specifically, the inventors surprisingly found that in the step of electrochemically etching the damaged layer, the selection and concentration of the etchant are important for ensuring a high etching rate, in particular a suitably high conductivity (e.g., above 500 μS cm -1 ) and the appropriate chemistry of the solution are critical. This is in stark contrast to previous work, which only advocated high resistivity dielectrics (J. Electrochem. Soc., 140, 2, (1993)) without considering the chemistry employed. One of the key aspects is the ability of the ions to form free radical species under the applied potential, with the etchant producing more or more highly oxidized free radicals, resulting in a higher etch rate.

[0021] It also directly contrasts with the teaching of US5891575A, which describes conditions where the solution has the conductivity of deionized water (0.5 μS cm) (i.e., extremely high resistance). In order to match this conductivity with a dilute H2SO4 solution, the solution must be prepared at a concentration of about 100 nM, as suggested by US5891575A.

[0022] If the correct ions are selected, the etch rate is significantly increased compared to known electrochemical etching processes. In particular, the inventors have observed bulk etch rates that are more than an order of magnitude faster than can be achieved using the disclosed methods. This is advantageous because it significantly reduces production time, and therefore costs.

[0023] As used herein, the term "damaged layer" refers to a carbon layer having a different crystal structure than the surrounding diamond material. In contrast to forming an isolated region within the diamond material, the term "layer" is used to define a region extending substantially from one face of the diamond material to the other face. However, it should be understood that there may be minor discontinuities in the layer and / or the damaged layer may not be fully exposed to the diamond material face. However, in order for electrochemical etching to be effective, active etchant species need to enter the damaged layer. 3 Compared with the bonded carbon structure, the damaged layer is mainly sp 2 Layers of bonded carbon.

[0024] The presence of the damaged layer means that there are two distinct regions within the diamond material; a first diamond layer above and in contact with the damaged layer and a crystalline diamond layer below and in contact with the damaged layer.

[0025] The size of the diamond material provided in step (a) is not limited. Typically, the thickness of the diamond material is in the range of about 10 to about 1000 μm, preferably in the range of 100 to 500 μm.

[0026] The diamond material provided in step (a) may have been produced by a chemical vapour deposition (CVD) process or a high pressure high temperature (HPHT) process. The bulk etch rate of HPHT diamond material is generally faster than that of CVD diamond material, which may be due to a lower structural defect density.

[0027] Prior to the electrochemical etching step, the diamond material may be annealed to convert the damaged regions into sp 2 Steps to bond successive layers of carbon.

[0028] The diamond material provided may be doped or undoped. When it is doped, the dopant atoms may produce an n-type or p-type semiconductor. P-type doping may be achieved by implanting the material with, for example, boron atoms. N-type doping may be achieved by implanting the material with, for example, nitrogen, phosphorus or lithium atoms. Doping may be achieved by ion implantation, and those skilled in the art will be familiar with suitable techniques.

[0029] The diamond material provided may be single crystal or polycrystalline. In addition, the diamond material provided may be HPHT or CVD diamond material.

[0030] The size of the diamond material is not limited and will depend on the end use of the diamond product.Examples of suitable sizes for single crystal diamond include a maximum linear dimension of at least 6 mm, at least 8 mm, at least 10 mm, at least 15 mm and at least 20 mm.

[0031] Optionally, the provided diamond material may be polished, in particular mechanically polished, before the formation of the damaged layer. Where a polishing step is included, the surface of the diamond material through which the ions are to pass is preferably polished to a Ra roughness value selected from the group consisting of less than 100 nm, less than 50 nm, less than 20 nm, and less than 10 nm.

[0032] The damaged layer may be formed by ion implantation. During ion implantation, an implantation layer is formed below the surface of the diamond material. Those skilled in the art will be familiar with ion implantation techniques. In particular, ion implantation may be performed using a high-speed ion beam. The ion beam is generated by a gaseous plasma that contains a mixture of ions and electrons. The ions are separated from the mixture by a small electric field and may then be accelerated and directed to the diamond material by a stronger electric and / or magnetic field. The use of a strong magnetic field enables the selection of a single ion species for implantation. Examples of suitable ions include, but are not limited to, helium, carbon, nitrogen and boron.

[0033] The depth to which the implanted layer is formed within the diamond material will depend on the energy of the ion beam used. Typically, the kinetic energy of a suitable ion beam is in the range of 1×10 4 About 1×10 7eV, which provides an implantation layer with a depth ranging from about 10 nm to about 5 μm. The depth of the implantation layer can be calculated by SRIM Simulations (Stopping Range of Ions in Matter, (Ziegler, JF et al., SRIM-The Stopping and Range of Ions in Matter (2010). Nucl. Instruments Methods Phys. Res. Sect. B Beam Interact. with Mater. Atoms 2010, 268 (11-12), 1818-1823)). The minimum dose of ions is about 10 15 Ions / cm 2 And typically around 10 16 to about 10 20 Ions / cm 2 The duration of the ion implantation step is typically in the range of 1 minute to 5 hours, more typically in the range of 2 to 10 minutes, depending on the desired dose. The ion current and the duration of the step determine how many ions are implanted. The ion implantation step is typically performed under vacuum. Ion implantation is usually performed between -200°C and room temperature, although higher temperatures can be used.

[0034] The ion implantation step produces a damaged layer below the surface of the diamond material. The thickness of the damaged layer is typically in the range of 10 to 1000 nm, preferably in the range of 20 to 500 nm. The thickness of the damaged layer can be controlled by adjusting the ion beam energy, ion current and / or duration of the ion implantation step.

[0035] As mentioned above, the damaged layer is a layer of carbon material having a different crystal structure than the surrounding diamond material. However, it may also contain small amounts of other atoms depending on the ions used during the implantation step. Examples of other atoms that may be present in the damaged layer include helium, boron, nitrogen and hydrogen.

[0036] After the ion implantation step, the diamond material may be annealed. Annealing the ion implanted diamond material has the effect of converting the damaged regions into sp 2 Effect of bonded carbon layer.

[0037] The annealing step may be performed at a temperature in the range of 500 to 1500° C., preferably 1000 to 1400° C. The duration of the annealing step may be in the range of 0.5 to 16 hours. The annealing is performed in an inert atmosphere (e.g. argon or nitrogen) or under vacuum (e.g. at a pressure of less than about 1 Pa).

[0038] The product obtained after the annealing step is a diamond material containing a damaged layer comprising sp 2 bonded carbon, and wherein the presence of the damaged layer defines a first diamond layer above and in contact with the damaged layer and a second diamond layer below and in contact with the damaged layer.

[0039] Optionally, an additional step may be included after the ion implantation step, the step comprising growing a diamond layer on the surface of the diamond material through which the ions are implanted by a chemical vapor deposition (CVD) process. The thickness of the grown layer (hereinafter referred to as the "epiphyseal layer") will depend on the intended final application of the diamond layer produced by the method of the present invention. In the case where the diamond layer produced by the method of the present invention is used for optical applications, preferably, the thickness of the epiphyseal layer is in the range of a few nanometers to about 10 mm. In the case where the diamond layer produced by the method of the present invention is used for electronic devices, the thickness of the epiphyseal layer is preferably in the range of about 1 nm to about 100 μm.

[0040] CVD methods for depositing diamond are now well established and are widely described in patents and other literature. The method generally involves providing a source gas that, when dissociated to form a plasma, is capable of providing reactive gas species, such as free radicals and other reactive species. The dissociation of the source gas is caused by an energy source such as microwaves, RF energy, flame, hot filament or jet-based techniques, and produces reactive gas species that are allowed to be deposited onto a substrate and form diamond.

[0041] Where this additional step is included, the first diamond layer produced in the diamond material comprises the portion of diamond material above the damaged layer and an overgrown diamond layer.

[0042] The diamond material containing the damaged layer may be cleaned prior to electrochemical etching. An exemplary cleaning step is in a concentrated sulfuric acid mixture saturated with potassium nitrate and heated to 200°C for about 30 minutes. This step is followed by boiling in sulfuric acid for 2 to 30 minutes followed by rinsing with ultrapure water.

[0043] As described above, the electrochemical etching step is performed in the presence of ions which generate an etchant species by electrolysis which selectively etches the sp 2 Examples of suitable ions include any of persulfate ions, sulfate ions, oxalate ions, chloride ions, carbonate ions, and metal ions. Alternatively, the ions may be present during electrochemical etching at a concentration between 0.01 M and the upper limit of the solubility of the ions in the electrolyte.

[0044] Optionally, the solution containing the ions has a relative humidity of at least 500 μS cm -1 conductivity.

[0045] Electrochemical etching is performed in an electrochemical cell comprising at least an anode, a cathode and an electrolyte. The above ions are present in a solution of the electrolyte.

[0046] Heretofore, it was believed that the key consideration for electrochemical etching processes was the resistivity of the electrolyte present in the electrochemical cell. However, the inventors are the first to present a different view. More specifically, as described in the following examples, the inventors investigated performing the etching step in the presence of several different salt solutions as electrolytes, all with higher conductivity than previously disclosed. Although all solutions tested were used as etching solutions, it was surprising that some solutions (with comparable conductivity) performed significantly better than other solutions. Therefore, the inventors' findings not only contradict the published data that low resistivity is preferred, they also show that the choice of ions is important. In particular, ions that are capable of electrochemically forming free radicals are selected. Except for potassium nitrate, all electrolytes (K2CO3, KCl, K2C2O4 and K2SO4) provide improved etching rates compared to the disclosed processes. The contribution of such ions to the etching process is not just to increase the conductivity of the etching solution.

[0047] The fastest solution of all the solutions tested contained sulfate ions. The source of sulfate ions is not limited, and suitable examples include potassium sulfate (K2SO4) and other water-soluble sulfates, such as Na2SO4.

[0048] The nature of the electrochemical cell used in the electrochemical etching step is not limited, and the skilled person will be familiar with suitable electrochemical cells. The anode and cathode can be formed of any conductive material. Preferably, the anode and cathode are formed of the same conductive material. Preferred conductive materials include carbon and noble metals, such as platinum. Preferably, the anode and cathode are formed of platinum. The positions of the anode and cathode in the liquid electrolyte are separated from each other. A voltage is then applied between the two electrodes to generate an electric field in the electrolyte. The applied voltage is typically in the range of 10 to 300V.

[0049] The electrolyte used is any electrolyte that can dissolve the ion source. Examples include dilute sulfuric acid and distilled water. In the case of a solution containing sulfate ions, the electrolyte is preferably acidic. In this regard, the inventors surprisingly found that in the case of an electrolyte comprising protons (H + ion) source, the bulk etch rate is further increased. Without wishing to be bound by theory, it is believed that H +Ions increase the rate at which sulfate ions interact with the solvent to form OH radicals, which are also active in the etching process. Therefore, advantageously, step (b) is also carried out at an acidic pH, i.e., at a pH less than about 7, preferably at a pH less than about 3. In view of the other advantages observed at acidic pH values, it is particularly preferred that the electrolyte comprises dilute sulfuric acid (H2SO4), thereby ensuring an acidic pH while also maximizing the concentration of sulfate ions present. This also has the other advantage that pure sulfuric acid is a liquid that is completely miscible with water and has a high boiling point to limit evaporation, and if evaporation of the solution occurs, the electrolyte does not leave salt residues.

[0050] The diamond material including the damaged layer is placed in a non-contact manner in the electrolyte between the anode and cathode. Preferably, it is positioned so that the exposed face of the damaged layer (or the surface closest to it) is approximately parallel to the electrodes. 2 The bonded carbon layers form a "channel" through which the active etchant species generated by the presence of active ions in the electrolyte pass, converting sp 2 The bonded carbon layer is converted to small carbon containing molecules such as CO2 and CH4. Removal of the non-diamond carbon results in the first diamond layer being separated from the damaged layer, thereby providing a diamond product as described above.

[0051] Transmission microscopy imaging can be used to monitor the bulk etch rate of the damaged layer. For example, a digital US microscope (VehoDiscovery VMS-001, 20-90x magnification) can be used to capture time-lapse images as the electrochemical etching step proceeds. Figure 1 An exemplary illustration of such a time-lapse image is shown. The time-lapse data can then be analyzed using a MATLAB script. Specifically, a target region is defined on the first image, and the script then calculates the proportion of that region that corresponds to the brighter etched region that matches the RGB value in the script. The proportion is then converted to an etched area, which can then be plotted as a function of time to generate an etching curve. Using this technique to generate an etching curve, the time resolution is typically 1 to 10 seconds, which can be used to accurately track the progress and rate of etching.

[0052] The etching curve usually has an S-shaped shape, such as Figure 2 As shown, it can be divided into three different parts: i) an initiation zone where little etching occurs; ii) a bulk etch zone, during which the etch rate is highest and most of the material is removed; and iii) a high volume limit, during which the limited amount of material remaining causes the rate to decrease, eventually reaching a limit where the amount of etching is negligible. In most cases, this limit is the point at which no more material remains, and since there is no (or negligible) amount of sp 2The bonded carbon material remains and the etch rate eventually drops to zero. To calculate the bulk etch rate, the bulk etch region ii) is assumed to be linear and the bulk etch rate is determined by the gradient of this region.

[0053] Using the method of the present invention, it was observed that 2 to 40 mm 2 hr -1 The bulk etch rate is within the range.

[0054] Depending on its final application, the first diamond layer may be very thin and therefore difficult to manipulate. However, those skilled in the art will be familiar with techniques for handling such thin materials. For example, one method is to float the first diamond layer from the second diamond layer in distilled water. The first diamond layer can then be floated onto a different substrate and the water beneath the film removed with a paper towel to provide a semi-permanent van der Waals bond to the new substrate. An alternative method is to attach the first diamond layer to a pre-grown diamond frame using an adhesive (e.g., a cyanoacrylate adhesive). This can be done before or after step (b). Once step (b) has been performed, the frame can be used to manipulate the diamond product without risk of damage.

[0055] The size of the diamond product is not limited. However, an advantage of the method of the present invention is that the increase in the electrochemical removal rate allows the separation of larger plates before the process becomes impractically slow.

[0056] In another aspect, the present invention provides a diamond product obtainable by a method described herein.

[0057] In another aspect, the present invention provides the use of a diamond product obtainable by the method described herein in an optical product.

[0058] In another aspect, the present invention provides the use of a diamond product obtainable by the method described herein in an electronic product.

[0059] In a further aspect, the present invention provides the use of a diamond product obtainable by the method described herein in an electrochemical product.

[0060] In another aspect, there is provided a diamond product comprising polycrystalline diamond material, wherein the diamond product has an average thickness of no greater than 30 μm and an average lateral grain size of the polycrystalline diamond material of no greater than 5 μm, as measured by scanning electron microscopy imaging. This combination of average thickness and average lateral grain size may be achieved by the techniques described above in the first aspect.

[0061] Alternatively, the average lateral grain size is selected from any of greater than 10 μm, greater than 15 μm, and greater than 20 μm.

[0062] According to another aspect, there is provided a composite body comprising a single crystal diamond plate having an average thickness of no more than 50 μm and a support structure attached to a surface of the single crystal diamond plate by a glue, the glue being substantially inert to ions capable of forming free radicals during electrolysis. The glue optionally comprises an epoxy resin. Optionally, the average thickness of the single crystal diamond plate is selected from any of the following: no more than 25 μm, no more than 10 μm, no more than 5 μm and no more than 1 μm.

[0063] The invention will now be further described with reference to the following figures and examples, which in no way limit the scope of the claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 is a visual representation of the electrochemical etching process of HPHT single crystal diamond material from t = 0 to t = 120 minutes. Each image is separated by etching in 0.3% v / v (0.05M) H2SO4 for about 8 minutes;

[0066] Figure 2 is an exemplary etching curve from in situ transmission microscopy imaging of a 4.1 mm CVD sample in 0.25 M K2SO4 solution;

[0067] Figure 3 (a) is a schematic diagram of the electrochemical cell used in step (b), showing the arrangement of the diamond material and electrodes;

[0068] Figure 3 (b) is an image of the apparatus used in step (b), showing the microscope camera, flow system and backlight;

[0069] Figure 3 (c) is an image captured from a microscope camera during etching;

[0070] Figure 4 is a comparison of bulk etch rates of different diamond materials in 0.25M supporting electrolyte solution as described in Example 1;

[0071] Figure 5 is a graph of bulk etch rate versus sulfate concentration for 3.5 mm CVD single crystal diamond material as described in Example 3;

[0072] Figure 6 is a graph showing the bulk etch rate of 4.1 mm CVD single crystal diamond material in a solution comprising K2SO4 and H2SO4, the solution having a constant sulfate concentration but decreasing pH;

[0073] Figure 7Microscope images showing etching of boron doped polycrystalline diamond. Each image is separated by etching for 25 minutes starting from t=0, as described in Example 4;

[0074] Figure 8 are microscope images of etching of optical grade polycrystalline diamond. Each image is separated by etching for 25 minutes starting from t=0, as described in Example 5;

[0075] Fig. 9 shows the electron paramagnetic resonance (EPR) data of various salt solutions after electrolysis;

[0076] Fig.10 is a flow chart showing exemplary steps for forming a diamond product; and

[0077] Fig.11 Exemplary steps for forming a diamond product are schematically illustrated. DETAILED DESCRIPTION OF THE INVENTION

[0079] Materials and solutions

[0080] All solutions were prepared from Milli-Q water (Millipore Corp.) with a resistivity of 18.2 MΩcm at 25°C.

[0081] The electrolyte used contained 0.25 M salt in deionized water. The salts tested were potassium nitrate (KNO3, 99.97%, Sigma Aldrich, UK), potassium chloride (KCl, ≥99%, Sigma Aldrich, UK), potassium sulfate (K2SO4, Pure, Acros Organics, USA), potassium carbonate (K2CO3, ACS reagents, Sigma Aldrich, UK) and potassium oxalate (K2C2O4, >98.5%, Sigma Aldrich, UK).

[0082] Sulfuric acid (H2SO4, >96%, Merck, UK) was used at 0.3% v / v (0.05 M) in deionized water.

[0083] Diamond sample preparation

[0084] For all studies, CVD and HPHT single crystal diamond plates with a thickness of about 500 μm (Element Six Technologies Ltd., Harwell, UK) were used as diamond materials unless otherwise stated. The front side of each sample was mechanically polished to a roughness of about nm, and the back side was ground to a roughness of about μm. The polished side was then implanted (Ion Beam Center, University of Surrey, UK) with 2×10 16carbon atoms (2 MeV), resulting in an end-of-range damage layer about 500 nm below the surface, calculated from SRIM simulations.

[0085] The implanted samples were then annealed at 1300 °C for two hours to convert the damaged layer produced by ion implantation into sp 2 Bonded carbon layer.

[0086] Figure 2 The data shown in were collected using 3.5 x 3.5 mm square CVD plates.

[0087] Figure 4 The data shown in were collected using 3.5 and 4.1 mm square CVD plates and 4.2 mm square HPHT plates.

[0088] Figure 5 The data shown in were collected using 3.5 mm square CVD plates.

[0089] Figure 6 The data shown in were collected using 4.1 mm square CVD plates.

[0090] Figure 8 The data shown in were collected using 5 mm square BDD CVD plates.

[0091] Implant characterization

[0092] The approximate depth and width of the end-of-range damage layer of the ion implantation were calculated using Stopping and Range of Ions in Matter (SRIM) simulations, yielding a damaged region with a thickness of approximately 1 μm for each sample.

[0093] Pickling

[0094] The diamond samples were pickled in a mixture of concentrated H2SO4 (Merck, >96%) saturated with KNO3 and then heated (200°C) for 30 minutes. They were then pickled in H2SO4 at 200°C for another 30 minutes and then rinsed in ultrapure water (>18 MΩcm, Millipore corp.).

[0095] Electrochemical cell

[0096] The electrochemical etching step (b) occurs in a custom designed 3D printed tank (Lulzbot Taz 6). The tank is designed to allow positive alignment of the diamond material containing the damage layer and the electrodes, and to provide an optical path for transmission imaging of the sample being etched ( Figure 3 (a) and (b)).

[0097] A digital USB microscope (Veho Discovery VMS-001, 20-90x magnification) was used to capture time-lapse images of the etching process. Figure 3 (c)). Unless otherwise stated, the electrodes used were 2 cm of 0.75 mm diameter platinum wire (total area 0.5 cm 2 ), with a spacing of 6 mm. A potential was applied between the two electrodes using a variable DC power supply (Elektro Automatik GmbH, EA-PS 9750-04), operated in potential-limited mode at 30 V, with the current depending on the solution composition. In order to maintain a constant solution composition and temperature, a flow system with a temperature-controlled reservoir of 5-90° C. was used. The electrolyte circulated from this reservoir into the tank and returned via the effluent.

[0098] Image analysis

[0099] A MATLAB script was used to analyze all the time-lapse data. Each frame of the video capture was extracted. A target region was defined on the first image, and the script then calculated the proportion of the area in that region that corresponded to the brighter etched regions, which matched the RGB values ​​in the script. This proportion was then converted to area, which was then plotted against the etch time to generate an etch curve. Table 1 compares the etch rates.

[0100] Table 1: Etch rate comparison

[0101]

[0102]

[0103]

[0104] Electron Paramagnetic Resonance (EPR)

[0105] The solution used for EPR contained 0.25 M salts including potassium nitrate, potassium chloride and potassium sulfate (K2SO4, analytical grade, Sigma-Aldrich, UK) in deionized water. Sulfuric acid (H2SO4, 96% Ultrapur, Merck, UK) was used at 0.3% v / v.

[0106] The electrolysis of solutions containing 0.05 M H2SO4, 0.25 M K2SO4, 0.25 M KCl or 0.25 M KNO3 was performed in a single compartment cell. A power supply (Elektro-Automatik GmbH, EA-PS9750-04) was used to generate a solution of 0.05 M H2SO4, 0.25 M K2SO4, 0.25 M KCl or 0.25 M KNO3. Two platinum electrodes (electrode area 0.5 cm2) placed in the solution were charged with a charge. 2, with the same geometry as the electrodes used in the etching tank) was applied with a voltage of 30 V. After a period of 15 minutes, about 20 mg of 5,5-dimethyl-1-pyrroline-N-oxide (DMPO; Enzo lifeSciences, USA) was added to the mixture and mixed thoroughly. An aliquot of the electrolytic mixture was sampled from the resulting solution and the EPR spectrum was recorded.

[0107] The EPR signals for DMPO spin adducts were recorded at 298 K on an X-band spectrometer (EMX; Bruker, Germany) equipped with a HS cylindrical resonator (4119HS / 0207; Bruker, Germany). Quartz (CFQ) EPR tube; Sigma-Aldrich, UK). For all measurements, the following spectrometer parameters were used: 20 mW non-saturated microwave power; central magnetic field of 3520 G; scan width of 100 G, and modulation amplitude of 0.5 G. All spectra reported are the average of 9 scans. The EPR spectra were fitted and simulated using the MATLAB software package EasySpin (version 5.2.25, Stoll, S.; Schweiger, A. EasySpin, a Comprehensive Software Package for Spectral Simulation and Analysis in EPR. J. Magn. Reson. 2006, 178 (1), 42-55. https: / / doi.org / 10.1016 / j.jmr.2005.08.013.).

[0108] Example 1

[0109] Effect of different anions on bulk etching rate of diamond material containing non-diamond carbon damage layer

[0110] The above electrolytes, each with a fixed concentration of 0.25M of the corresponding anion, were used as electrolytes in electrochemical etching processes on three different diamond materials, specifically 3.5 mm square CVD diamond material, 4.1 mm CVD diamond material and 3.5 mm HPHT diamond material, all of which had been processed as described above to include sp 2 The bulk etch rate observed is as follows Figure 4 shown.

[0111] All electrolytes except KNO3 provide improved etch rates relative to the published process. The fastest etching electrolyte is K2SO4, which has a bulk etch rate that is an order of magnitude faster than the published process. The significant improvement in bulk etch rate reduces processing time, resulting in significant savings in processing time and cost.

[0112] Example 2

[0113] Effect of sulfate ion concentration on the content of sp 2 Effect of bonded carbon damage layer on bulk etch rate of diamond material.

[0114] Having determined that favorable bulk etch rates are observed when using an electrolyte containing sulfate ions, Example 2 was conducted to investigate the effect of sulfate ion concentration on the bulk etch rate.

[0115] The bulk etch rate in K2SO4 solution was measured, where sulfate (SO4 2- ) concentration ranged from 0.03 to 0.25 M. The data for 0.25 M KNO3 are included for comparison (0 M sulfate ion) because it has the slowest bulk etch rate among the data measured in Example 1. The conductivity of the 0.25 M KNO3 solution is 25 mS cm -1 , the conductivity of the sulfate solution is 4 to 40 mS cm in the entire range -1 The results are shown in Figure 5 middle.

[0116] from Figure 5 It can be clearly seen that the bulk etch rate increases linearly with increasing sulfate concentration up to 0.06 M. The bulk etch rate then levels off above sulfate concentrations greater than 0.06 M, but the bulk etch rate is significantly faster than previously achieved. The initial linear relationship is likely due to the increase in sulfate ion concentration on the electrode surface, which ultimately results in the generation of a higher number of active etchant species, thus supporting the hypothesis in Example 1 that sulfate ions are directly involved in the generation of active etchant species.

[0117] The plateau in bulk etch rate can be explained by one or a combination of two factors. First, the concentration of active etchant species at the interface of the damage layer increases, making the active sites within the damage layer the rate limiting step for etching. Second, at higher concentrations of active etchant species, the chances of these species combining increase, so that the amount of active etchant species at the interface of the damage layer does not actually increase above 0.06M.

[0118] Since no additional electrolyte is added as the concentration of K2SO4 solution increases, the conductivity of the electrolyte also increases. However, in the region of 60 to 250 mM sulfate ions, although the conductivity decreases from 4 mS cm -1 Increased to 42 mS cm -1 , but the rate did not change significantly. This indicates that in this case, the conductivity has little effect on the bulk etch rate.

[0119] Example 3

[0120] The pH value has a sp 2 Effect of the bonded carbon damage layer on the bulk etch rate of diamond materials

[0121] In order to further improve the bulk etching rate of diamond materials, the effect of pH on the electrolyte solution containing sulfate ions was studied. A mixture of K2SO4 and H2SO4 was used to change the pH value while maintaining the total sulfate ion concentration at 0.25M.

[0122] The results are presented in Figure 6 middle.

[0123] A decrease in pH and its associated increase in conductivity (42 to 89 mS cm -1 ) has the effect of increasing the bulk etch rate. However, as shown in Example 2, the change in conductivity has little effect on the bulk etch rate, so the increase in the bulk etch rate can be attributed to the decrease in pH.

[0124] As protons (H + ) concentration increases, the observed bulk etch rate shows an overall upward trend, indicating that protons are also involved in the rate-limiting step. In particular, the bulk etch rate increases by a factor of 2 when the pH value decreases from 7 to 0.8, clearly indicating that the use of more acidic solutions as electrolytes provides further favorable improvements in the bulk etch rate.

[0125] Example 4

[0126] Use single crystal boron doped diamond (BDD) instead of optical grade single crystal diamond

[0127] To investigate whether this approach is suitable for doped diamond materials, we investigated 19 Boron atoms / cm 3 5mm 2 Electrochemical etching of CVD single crystal diamond material This material is implanted and annealed in the same manner as all the other materials discussed.

[0128] Although it is difficult to process optical etching data in the normal way, the color change is not obvious, and the sp2 The bonded carbon layer is being removed, e.g. Figure 7 In 0.25M H2SO4 solution, 5 mm was achieved within 60 minutes. 2 Complete separation of the plates yields separation times comparable to undoped material.

[0129] Example 5

[0130] Use multicrystalline optical grade materials instead of single crystal optical grade materials

[0131] To investigate whether this approach is suitable for polycrystalline diamond material, we investigated the electrochemical etching of a 4 mm square of CVD optical grade polycrystalline material. This material was implanted and annealed in the same way as all the other materials discussed.

[0132] It is obvious to the naked eye that sp 2 The bonded carbon layer is being removed, e.g. Fig. 9 In 0.25 M H2SO4 solution, complete separation of a 4 mm square plate was achieved within 60 min, yielding a separation time comparable to that of the undoped material.

[0133] As described above, EPR measurements were obtained from different salt solutions after electrolysis to determine the presence of hydroxyl radicals. The presence of hydroxyl radicals is believed to have an effect on the etch rate of the damaged layer. Fig. 9 Experimental and fitted data for potassium chloride and potassium sulfate solutions are shown. Fig. 9 The peaks shown in the three traces represent hydroxyl radicals, and the area under the peaks represents the amount of hydroxyl radicals present.

[0134] from Fig. 9 It can be seen that the sulfate solution forms far more hydroxyl radicals than the chloride solution. This corresponds to Figure 4 The etching rate shown in , where the etching rate of diamond in sulfate solution is faster than that in chloride solution.

[0135] The exemplary steps of the method are as follows Fig.10 The following numbers correspond to Fig. 9 Number:

[0136] S1. Provide diamond material. This may be single crystal or polycrystalline diamond material. If single crystal diamond material, it may be natural or HPHT diamond material. In addition, the diamond material may be doped with any of, for example, nitrogen, boron, phosphorus and silicon.

[0137] S2. Ion implantation of diamond material to form sp 2A damaged layer of bonded carbon, wherein the presence of the damaged layer defines a first diamond layer above and in contact with the damaged layer and a second diamond layer below and in contact with the damaged layer.

[0138] S3. As an optional step, the diamond material may be annealed to increase the sp 2 The amount of carbon.

[0139] S4. During the etching process, the damaged layer is electrochemically etched in the presence of ions capable of forming free radicals. Etching of the damaged layer allows the first layer and the second layer to be separated. Suitable ions include, but are not limited to, persulfate ions, sulfate ions, oxalate ions, chloride ions, carbonate ions, and metal ions.

[0140] Now turn to Fig.11 , illustrating Fig.10 Some of the steps in (not to scale).

[0141] Fig.11 a shows a provided diamond material 1 which has been subjected to ion implantation.

[0142] Fig.11 b shows the first diamond layer 2 and the second diamond layer 3 formed during the ion implantation step, each layer being composed of sp 2 The damaged layer 4 of the bonded carbon is separated.

[0143] Fig.11 c shows electrochemical etching in the presence of ions capable of forming free radicals during electrolysis. The electrochemical etching preferentially attacks the damaged layer 4.

[0144] Fig.11 d shows that the damaged layer 4 has been etched away, thereby separating the first layer 2 from the second layer 3.

[0145] When the separation layer is removed from the damaged layer, the separation layer may be very thin and difficult to manipulate without causing damage to the separation layer. One way to address this problem is to provide a support structure, such as that described in WO 2016 / 058037, wherein the support structure is attached to the diamond material by gluing, brazing, overlaying polycrystalline diamond, or any suitable means that can withstand the etching process. For example, a mask made of a material such as diamond can be glued to the diamond material, which allows the separation layer to be easily manipulated once it has been removed.

[0146] When preparing thin plates of polycrystalline CVD diamond, the present invention allows such plates to have larger average lateral grain sizes and lower sp than previously possible. 2A plate of polycrystalline CVD diamond material typically comprises a nucleation plane (the plane from which CVD growth begins) containing small grains of diamond material and a large amount of non-diamond sp 2 carbon (detectable by Raman spectroscopy); and growth faces, which contain larger grains of diamond material and, if growth conditions are properly controlled, non-diamond sp 2 The amount of carbon is relatively low. In moving across such a polycrystalline CVD diamond material wafer from the nucleation face to the growth face, the diamond grain size increases.

[0147] Using existing techniques, thin plates of polycrystalline CVD diamond are obtained, which are grown directly on a substrate and thus formed close to the nucleation plane. Such plates have a small average lateral grain size and a relatively high sp 2 Carbon content.

[0148] Relatively thick plates can be grown with growth faces having large average lateral grain sizes and low sp 2 Carbon content. Using the above techniques, a layer can be removed from the growth surface, leaving a thin layer with a relatively high average lateral grain size (greater than 5 μm) and a thickness of no more than 30 μm. The average lateral grain size can be greater than 10 μm, greater than 15 μm, greater than 20 μm.

[0149] The average lateral grain size of a polycrystalline CVD diamond surface is measured using a scanning electron microscope (SEM). SEM images of the surface of a polycrystalline CVD diamond material show the boundaries between the grains, enabling the identification and counting of individual grains. Thus, an area of ​​a polycrystalline CVD diamond surface can be imaged using a SEM and then the total number of diamond grains along a line across the image can be counted, the length of the line can then be divided by the number of grains along the line to obtain the average lateral grain size. Multiple lines across the SEM image can be analyzed in this way, optionally in the vertical direction, and the average value of the lateral grain size across the imaged area calculated.

[0150] While the invention has been particularly shown and described with reference to embodiments, it will be understood by those skilled in the art that various changes in form and details may be made without departing from the scope of the invention as defined by the appended claims.

Claims

1. A method of forming a diamond product, the method comprising: Provide diamond materials; Formation containing sp 2 a damaged layer of bonded carbon, wherein the presence of the damaged layer defines a first diamond layer above and in contact with the damaged layer and a second diamond layer below and in contact with the damaged layer; and electrochemically etching the damaged layer to separate the first layer therefrom, wherein the electrochemical etching is performed in a solution containing ions, the solution having an electrical conductivity of at least 500 μS cm -1 , and wherein the ions are capable of forming free radicals during electrolysis.

2. The method according to claim 1, wherein the ions are selected from any of persulfate ions, sulfate ions, oxalate ions, chloride ions, carbonate ions and metal ions.

3. The method according to claim 1, wherein the etching is performed at a depth of 2 to 40 mm. 2 hr -1 The etching rate occurs.

4. The method of claim 1, wherein the etch rate is measured by aligning the diamond material including the damaged layer with electrodes in an electrochemical cell to allow imaging of the diamond material and monitoring material loss of the diamond material over time. 5 . The method according to claim 1 , wherein the electrochemical etching is performed in an electrochemical cell, the electrochemical cell comprises at least an anode, a cathode and an electrolyte, and the ions are present in the electrolyte.

6. The method of claim 1, wherein during the electrochemical etching, the ion is present at a concentration between 0.01 M and an upper solubility limit of the ion in the electrolyte.

7. The method according to claim 1, wherein the electrochemical etching is performed at a temperature of 50°C to 90°C.

8. The method of claim 1, wherein the first diamond layer and the second diamond layer comprise diamond formed by chemical vapor deposition (CVD).

9. The method of claim 1, wherein the diamond material is single crystal diamond material.

10. A method according to claim 9, wherein the single crystal diamond material has a maximum linear dimension of from 6 mm to 20 mm.

11. The method of claim 1 , wherein the diamond material is polycrystalline diamond material.

12. The method of claim 1, wherein the diamond material comprises diamond prepared by any of a chemical vapor deposition (CVD) method and a high pressure high temperature (HPHT) method.

13. The method of claim 1, wherein the diamond material is doped.

14. The method of claim 13, wherein the diamond material is doped with any of nitrogen, boron, phosphorus and silicon. The method of claim 14 , wherein the damaged layer comprises a graphite material.

16. The method according to claim 1, further comprising forming the damaged layer by an ion implantation process.

17. The method of claim 1, further comprising attaching a support structure to the surface of the diamond material prior to the step of electrochemically etching the damaged layer, wherein the support structure and the means for attaching the support structure are formed of a material inert to a solution in which the electrochemical etching occurs.