Insulating flame-retardant release film and preparation method thereof

By introducing an inorganic flame retardant layer and polyimide/montmorillonite nanocomposite film into the release film, combined with strict raw material ratio and process control, the flame retardant performance and insulation of the existing release film are solved. The problem is that efficient flame retardant and electrical insulation effects are achieved, and the overall performance of the film is improved.

CN115157813BActive Publication Date: 2024-12-03DONGGUAN HENGCONG PACKAGING PROD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210844501.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-18
Publication Date
2024-12-03
Estimated Expiration
2042-07-18

AI Technical Summary

Technical Problem

The existing release membranes lack flame retardant properties and insulation in the electronics industry, have a single function, and do not have smoke suppression effects.

Method used

The insulated flame retardant release film structure consisting of a silicone oil layer, an antistatic coating, a substrate layer, an inorganic flame retardant layer and a polyimide/montmorillonite nanocomposite film are adopted. The raw material ratio and process steps are strictly controlled. , a film with excellent antistatic, flame retardant, transparency and mechanical properties is formed.

Benefits of technology

It achieves good flame retardant effect of the film, reduces the amount of smoke generated during burning of plastic, improves electrical insulation, heat resistance and mechanical strength, and enhances the overall performance of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115157813B_ABST
    Figure CN115157813B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of release films, and in particular to an insulating flame-retardant release film and a preparation method thereof, wherein the insulating flame-retardant release film comprises a silicone oil layer, an antistatic coating, a substrate layer, a flame-retardant layer, an insulating layer and a protective layer arranged in sequence from bottom to top, wherein the flame-retardant layer is an inorganic flame retardant layer, and the insulating layer is a polyimide / montmorillonite nanocomposite film. The insulating flame-retardant release film of the present invention has a good flame-retardant effect by adopting an inorganic flame retardant layer, and can also reduce the amount of smoke generated when the plastic is burned, thereby playing the role of a smoke suppressant; by adopting a polyimide / montmorillonite nanocomposite film as an insulating layer, the insulating flame-retardant release film has high electrical insulation, heat resistance, moisture resistance, and good mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of release films, and in particular to an insulating flame-retardant release film and a preparation method thereof. Background Art

[0002] Release film refers to a film with a distinguishable surface. When the release film comes into contact with a specific material under limited conditions, it is non-sticky or slightly sticky. Some existing release films do not have flame retardant properties, and have poor insulation and single functions when used in the electronics industry. Summary of the invention

[0003] In order to overcome the shortcomings and deficiencies in the prior art, the object of the present invention is to provide an insulating flame-retardant release film and a preparation method thereof.

[0004] The objective of the present invention is achieved through the following technical scheme: an insulating flame-retardant release film, comprising a silicone oil layer, an antistatic coating, a substrate layer, a flame-retardant layer, an insulating layer and a protective layer arranged in sequence from bottom to top, the flame-retardant layer is an inorganic flame retardant layer, and the insulating layer is a polyimide / montmorillonite nanocomposite film.

[0005] Preferably, the antistatic coating is a tin oxide coating with a particle size of 100-500nm. More preferably, the antistatic coating is formed by curing the antistatic coating after coating, and the antistatic coating comprises the following raw materials in parts by weight: 20-40 parts of methyl orthosilicate, 10-30 parts of phenyltrimethoxysilane, 15-25 parts of diphenyldimethoxysilane, 10-20 parts of trimethyltriethylcyclotrisiloxane, 5-15 parts of γ-methacryloxypropyltriethoxysilane, 4-8 parts of inorganic antistatic agent, 5-10 parts of methylsulfonic acid, 2-4 parts of initiator, 4-8 parts of other auxiliary agents, and 20-60 parts of isopropyl alcohol, wherein the inorganic antistatic agent is tin oxide with a particle size of 100-500nm.

[0006] The antistatic coating of the present invention adopts the above raw materials and strictly controls the weight ratio of each raw material. The prepared antistatic coating not only has excellent antistatic performance, but also has good transparency and substrate adhesion, high hardness and excellent scratch resistance.

[0007] Preferably, the initiator is a mixture of 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzophenone in a weight ratio of 1-2: 1. The present invention can initiate the polymerization reaction at a lower temperature by strictly controlling the type, compounding and ratio of the initiator, thereby increasing the reaction rate and reducing energy consumption.

[0008] Preferably, the tin oxide is a mixture of antimony-doped tin dioxide and indium-doped tin oxide in a weight ratio of 2-4: 1. By strictly controlling the type, compounding and ratio of tin oxide, the present invention has better conductivity and stability than undoped tin oxide, and can prepare a transparent coating.

[0009] Preferably, the inorganic flame retardant layer is a magnesium hydroxide coating or an aluminum hydroxide coating. More preferably, the inorganic flame retardant layer is formed by curing a flame retardant coating after coating, and the flame retardant coating comprises the following raw materials in parts by weight: 20-40 parts of aqueous non-ionic polyurethane emulsion, 10-30 parts of silicone acrylic emulsion, 15-25 parts of fluorosilicone modified acrylic acid aqueous dispersion, 10-20 parts of styrene maleic anhydride resin, 5-15 parts of amino resin, 5-10 parts of inorganic flame retardant, 1.5-2.5 parts of initiator, 1-5 parts of emulsifier, 4-8 parts of other additives, and 20-40 parts of deionized water, and the inorganic flame retardant is magnesium hydroxide or aluminum hydroxide.

[0010] The inorganic flame retardant layer of the present invention adopts the above raw materials and strictly controls the weight ratio of each raw material. The inorganic flame retardant layer has excellent flame retardant properties and does not produce toxic or harmful gases or irritating gases when burning. It also has excellent mechanical properties, thermal stability, bonding properties, water resistance and weather resistance.

[0011] Preferably, the emulsifier is a mixture of polyoxyethylene alkyl ether hydrogen sulfate, sorbitan fatty acid ester and polyoxyethylene hardened castor oil fatty acid ester in a weight ratio of 1.5-2.5: 0.5-1.5: 1. The present invention strictly controls the type, compounding and ratio of the emulsifier, has a good emulsification effect, can improve the stability of the coating, and ensure the smooth progress of emulsion polymerization.

[0012] Preferably, the initiator is a mixture of sodium persulfate and sodium bisulfite in a weight ratio of 1-2: 1. The present invention can initiate polymerization at a lower temperature by strictly controlling the type, compounding and ratio of the initiator, thereby increasing the reaction rate and reducing energy consumption.

[0013] Preferably, the other additives are at least one of a defoamer, a dispersant, an anti-settling agent, an antioxidant, an adhesion promoter, a preservative, a pH adjuster, a film-forming aid and a leveling agent. The above additives are conventional additives in the art.

[0014] A method for preparing an insulating flame-retardant release film comprises the following steps:

[0015] (1) applying a layer of antistatic coating on the front side of the substrate layer to form an antistatic coating after curing;

[0016] (2) applying a flame retardant coating on the back of the substrate layer to form a flame retardant layer after curing;

[0017] (3) compounding a layer of polyimide / montmorillonite nanocomposite film on the surface of the flame retardant layer as an insulating layer, and then compounding a protective layer;

[0018] (4) A layer of silicone oil is coated on the surface of the antistatic coating, and a silicone oil layer is formed after curing to obtain an insulating flame-retardant release film.

[0019] The beneficial effects of the present invention are as follows: the insulating flame-retardant release film of the present invention has a good flame-retardant effect by adopting an inorganic flame retardant layer, and can also reduce the amount of smoke generated when the plastic is burned, thereby playing the role of a smoke suppressant; by adopting a polyimide / montmorillonite nanocomposite film as an insulating layer, it has high electrical insulation, heat resistance, moisture resistance, and also has good mechanical strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a partial cross-sectional view of the insulating flame-retardant release film of the present invention.

[0021] The reference numerals in the drawings are: silicone oil layer 1 , antistatic coating 2 , substrate layer 3 , flame retardant layer 4 , insulating layer 5 , and protective layer 6 . DETAILED DESCRIPTION

[0022] In order to facilitate the understanding of those skilled in the art, the following embodiments and attached Figure 1 The present invention is further described, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0023] Example 1

[0024] See Figure 1 An insulating flame-retardant release film comprises a silicone oil layer 1, an antistatic coating 2, a substrate layer 3, a flame-retardant layer 4, an insulating layer 5 and a protective layer 6 which are arranged in sequence from bottom to top. The flame-retardant layer 4 is an inorganic flame retardant layer, and the insulating layer 5 is a polyimide / montmorillonite nanocomposite film.

[0025] The insulating flame-retardant release film of the present invention has a good flame-retardant effect by adopting an inorganic flame retardant layer, and can also reduce the amount of smoke generated when the plastic burns, thereby playing the role of a smoke suppressant; by adopting a polyimide / montmorillonite nanocomposite film as the insulating layer 5, it has high electrical insulation, heat resistance, moisture resistance, and also has good mechanical strength.

[0026] In this embodiment, the silicone oil layer 1 is formed by coating with solvent-free silicone oil and then curing with UV. The present invention has a better release effect and is more environmentally friendly by coating with solvent-free silicone oil.

[0027] In this embodiment, the antistatic coating 2 is a tin oxide coating with a particle size of 100-500 nm. The present invention uses a tin oxide coating, which has a good antistatic effect and can prepare a transparent coating.

[0028] In this embodiment, the substrate layer 3 is a PET film with a light transmittance greater than 95% and a haze less than 1%. The present invention adopts the above PET film, which has high transparency, high temperature resistance, excellent heat resistance, cold resistance, good chemical resistance and oil resistance.

[0029] In this embodiment, the inorganic flame retardant layer is a magnesium hydroxide coating or an aluminum hydroxide coating. The present invention has a good flame retardant effect by using a magnesium hydroxide coating or an aluminum hydroxide coating, and can also reduce the amount of smoke generated when the plastic is burned, thus playing the role of a smoke suppressant.

[0030] In this embodiment, the protective layer 6 is a PET film with a light transmittance greater than 95% and a haze less than 1%. The present invention uses the above PET film as the protective layer 6, which has high transparency, high temperature resistance, excellent heat resistance, cold resistance, good chemical resistance and oil resistance.

[0031] The antistatic coating is formed by curing the antistatic coating after coating. The antistatic coating comprises the following raw materials in parts by weight: 20 parts of methyl orthosilicate, 10 parts of phenyltrimethoxysilane, 15 parts of diphenyldimethoxysilane, 10 parts of trimethyltriethylcyclotrisiloxane, 5 parts of γ-methacryloxypropyltriethoxysilane, 4 parts of inorganic antistatic agent, 5 parts of methylsulfonic acid, 2 parts of initiator, 4 parts of other auxiliary agents, and 20 parts of isopropanol. The inorganic antistatic agent is tin oxide with a particle size of 100 nm; the initiator is a mixture of 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzophenone in a weight ratio of 1:1; and the tin oxide is a mixture of antimony-doped tin dioxide and indium-doped tin oxide in a weight ratio of 2:1.

[0032] The inorganic flame retardant layer is formed by curing the flame retardant coating after coating. The flame retardant coating includes the following raw materials in parts by weight: 20 parts of aqueous non-ionic polyurethane emulsion, 10 parts of silicone-acrylic emulsion, 15 parts of fluorosilicone-modified acrylic aqueous dispersion, 10 parts of styrene maleic anhydride resin, 5 parts of amino resin, 5 parts of inorganic flame retardant, 1.5 parts of initiator, 1 part of emulsifier, 4 parts of other additives, and 20 parts of deionized water. The inorganic flame retardant is magnesium hydroxide or aluminum hydroxide; the emulsifier is a mixture of polyoxyethylene alkyl ether hydrogen sulfate, dehydrated sorbitan fatty acid ester and polyoxyethylene hardened castor oil fatty acid ester in a weight ratio of 1.5:0.5:1; the initiator is a mixture of sodium persulfate and sodium bisulfite in a weight ratio of 1:1.

[0033] The other additives are a mixture of a defoamer, a dispersant, a leveling agent and a film-forming aid in a weight ratio of 1:1:1:1.

[0034] A method for preparing an insulating flame-retardant release film comprises the following steps:

[0035] (1) applying a layer of antistatic coating on the front side of the substrate layer to form an antistatic coating after curing;

[0036] (2) applying a flame retardant coating on the back of the substrate layer to form a flame retardant layer after curing;

[0037] (3) compounding a layer of polyimide / montmorillonite nanocomposite film on the surface of the flame retardant layer as an insulating layer, and then compounding a protective layer;

[0038] (4) A layer of silicone oil is coated on the surface of the antistatic coating, and a silicone oil layer is formed after curing to obtain an insulating flame-retardant release film.

[0039] Example 2

[0040] The difference between this embodiment and the above-mentioned embodiment 1 is that the antistatic coating is formed by curing the antistatic coating after coating, and the antistatic coating comprises the following raw materials in parts by weight: 30 parts of methyl orthosilicate, 20 parts of phenyltrimethoxysilane, 20 parts of diphenyldimethoxysilane, 15 parts of trimethyltriethylcyclotrisiloxane, 10 parts of γ-methacryloxypropyltriethoxysilane, 6 parts of inorganic antistatic agent, 8 parts of methylsulfonic acid, 3 parts of initiator, 6 parts of other auxiliary agents, and 40 parts of isopropanol, wherein the inorganic antistatic agent is tin oxide with a particle size of 100-500nm; the initiator is a mixture of 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzophenone in a weight ratio of 1.5:1; and the tin oxide is a mixture of antimony-doped tin dioxide and indium-doped tin oxide in a weight ratio of 3:1.

[0041] The inorganic flame retardant layer is formed by curing the flame retardant coating after coating. The flame retardant coating includes the following raw materials in parts by weight: 30 parts of aqueous non-ionic polyurethane emulsion, 20 parts of silicone-acrylic emulsion, 20 parts of fluorosilicone-modified acrylic aqueous dispersion, 15 parts of styrene maleic anhydride resin, 10 parts of amino resin, 8 parts of inorganic flame retardant, 2 parts of initiator, 3 parts of emulsifier, 6 parts of other additives, and 30 parts of deionized water. The inorganic flame retardant is magnesium hydroxide or aluminum hydroxide; the emulsifier is a mixture of polyoxyethylene alkyl ether hydrogen sulfate, dehydrated sorbitan fatty acid ester and polyoxyethylene hardened castor oil fatty acid ester in a weight ratio of 2:1:1; the initiator is a mixture of sodium persulfate and sodium bisulfite in a weight ratio of 1.5:1.

[0042] The other additives are a mixture of a defoamer, a dispersant, a leveling agent and a film-forming aid in a weight ratio of 1:1:1:1.

[0043] Example 3

[0044] The difference between this embodiment and the above-mentioned embodiment 1 is that the antistatic coating is formed by curing the antistatic coating after coating, and the antistatic coating comprises the following raw materials in parts by weight: 40 parts of methyl orthosilicate, 30 parts of phenyltrimethoxysilane, 25 parts of diphenyldimethoxysilane, 20 parts of trimethyltriethylcyclotrisiloxane, 15 parts of γ-methacryloxypropyltriethoxysilane, 8 parts of inorganic antistatic agent, 10 parts of methylsulfonic acid, 4 parts of initiator, 8 parts of other auxiliary agents, and 60 parts of isopropanol, wherein the inorganic antistatic agent is tin oxide with a particle size of 500 nm; the initiator is a mixture of 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzophenone in a weight ratio of 2:1; and the tin oxide is a mixture of antimony-doped tin dioxide and indium-doped tin oxide in a weight ratio of 4:1.

[0045] The inorganic flame retardant layer is formed by curing the flame retardant coating after coating. The flame retardant coating includes the following raw materials in parts by weight: 40 parts of aqueous non-ionic polyurethane emulsion, 30 parts of silicone-acrylic emulsion, 25 parts of fluorosilicone-modified acrylic aqueous dispersion, 20 parts of styrene maleic anhydride resin, 15 parts of amino resin, 10 parts of inorganic flame retardant, 2.5 parts of initiator, 5 parts of emulsifier, 8 parts of other additives, and 40 parts of deionized water. The inorganic flame retardant is magnesium hydroxide or aluminum hydroxide; the emulsifier is a mixture of polyoxyethylene alkyl ether hydrogen sulfate, dehydrated sorbitan fatty acid ester and polyoxyethylene hardened castor oil fatty acid ester in a weight ratio of 2.5:1.5:1; the initiator is a mixture of sodium persulfate and sodium bisulfite in a weight ratio of 2:1.

[0046] The other additives are a mixture of a defoamer, a dispersant, a leveling agent and a film-forming aid in a weight ratio of 1:1:1:1.

[0047] The antistatic coatings prepared in Examples 1-3 have a pencil hardness of 9H, an adhesion of 5B, a light transmittance of 92.5%-93.6%, and a surface resistance of 1.2*10 9 -4.5*10 9 Ω, not only has excellent antistatic properties, but also has good transparency and substrate adhesion, and high hardness.

[0048] The flame retardant effect of the inorganic flame retardant layer prepared in Examples 1-3 can reach V0 level, the adhesion can reach 5B level, and the light transmittance can reach 89.2%-91.8%.

[0049] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. An insulating flame-retardant release film, characterized in that: The invention comprises a silicone oil layer, an antistatic coating, a substrate layer, a flame retardant layer, an insulating layer and a protective layer arranged in sequence from bottom to top, wherein the flame retardant layer is an inorganic flame retardant layer, and the insulating layer is a polyimide / montmorillonite nanocomposite film; the antistatic coating is formed by curing the antistatic coating after coating, and the antistatic coating comprises the following raw materials in parts by weight: 20-40 parts of methyl orthosilicate, 10-30 parts of phenyltrimethoxysilane, 15-25 parts of diphenyldimethoxysilane, and trimethyltriethylsilane. 10-20 parts of cyclotrisiloxane, 5-15 parts of γ-methacryloxypropyltriethoxysilane, 4-8 parts of inorganic antistatic agent, 5-10 parts of methylsulfonic acid, 2-4 parts of initiator, 4-8 parts of other auxiliary agents, and 20-60 parts of isopropanol, wherein the inorganic antistatic agent is tin oxide with a particle size of 100-500nm; the initiator is a mixture of 2-hydroxy-2-methyl-1-phenyl-1-propanone and benzophenone in a weight ratio of 1-2:1; The tin oxide is a mixture of antimony-doped tin dioxide and indium-doped tin oxide in a weight ratio of 2-4:1; the inorganic flame retardant layer is formed by curing the flame retardant coating after coating, and the flame retardant coating includes the following raw materials in parts by weight: 20-40 parts of aqueous non-ionic polyurethane emulsion, 10-30 parts of silicone-acrylic emulsion, 15-25 parts of fluorosilicone-modified acrylic acid aqueous dispersion, 10-20 parts of styrene-maleic anhydride resin, 5-15 parts of amino resin, 5-10 parts of inorganic flame retardant, and 1 part of initiator. .5-2.5 parts, emulsifier 1-5 parts, other additives 4-8 parts, deionized water 20-40 parts, the inorganic flame retardant is magnesium hydroxide or aluminum hydroxide, the emulsifier is a mixture of polyoxyethylene alkyl ether hydrogen sulfate, dehydrated sorbitan fatty acid ester and polyoxyethylene hardened castor oil fatty acid ester in a weight ratio of 1.5-2.5:0.5-1.5:1, and the initiator is a mixture of sodium persulfate and sodium bisulfite in a weight ratio of 1-2:

1.

2. The method for preparing an insulating flame-retardant release film according to claim 1, characterized in that: The steps include: (1) applying a layer of antistatic coating on the front side of the substrate layer, and forming an antistatic coating after curing; (2) applying a layer of flame retardant coating on the back of the substrate layer, and forming a flame retardant layer after curing; (3) Compounding a layer of polyimide / montmorillonite nanocomposite film on the surface of the flame retardant layer as an insulating layer, and then compounding a protective layer; (4) A layer of silicone oil is coated on the surface of the antistatic coating, and a silicone oil layer is formed after curing to obtain an insulating flame-retardant release film.

Citation Information

Patent Citations

  • High temperature resistant antistatic coating and preparation method thereof

    CN102250545A

  • Material for insulating substrate, printed circuit board, laminate, copper foil with resin, copper-clad laminate, polymide film, film for TAB and prepreg

    CN1479768A

  • High polymer material release film

    CN213202909U

  • Waterproof wear-resistant release film