Super matte skin-feel decorative panel and preparation method thereof
Through electron beam curing technology, combined with the mixing of polyurethane acrylate and polyether acrylate and matte steel roller extrusion, the problems of difficult matting, poor skin feel, odor and low hardness of PET skin feel boards and UV skin feel boards are solved , achieving decorative panels with high hardness, low gloss and good skin feel, reducing nitrogen usage and equipment costs.
Patent Information
- Application Number
- CN202211013922.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-23
AI Technical Summary
Existing PET skin-feeling boards and UV skin-feeling boards have defects in terms of difficulty in matting, poor skin feel, odor, and low hardness. Excimer lamp curing technology requires a high-purity nitrogen environment, has high operating costs, expensive equipment investment, and is difficult to Dealing with the flatness problem of large slabs.
Using electron beam (EB) curing technology, by mixing polyurethane acrylate, polyether acrylate, multi-functional monomers and anti-fouling additives, UV curing is performed after printing UV ink, and EB is performed in matte steel roller extrusion It is cured to form a super matte skin-feeling film, which is compounded to the substrate through PUR hot melt adhesive to achieve a decorative panel with high hardness, low gloss and good skin-feeling.
There is no need to use nitrogen, the process is simple, the conditions are mild, and it is suitable for large-scale industrial production. The prepared ultra-matte skin-like decorative panels have high hardness, low gloss and good skin feel, avoiding oxygen inhibition reaction and odor problems, and reducing production costs. .
Smart Images

Figure BDA0003811928890000091 
Figure HDA0003811928900000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of decorative panels, and more specifically, to an ultra-matte skin-feel decorative panel and a preparation method thereof. Background Art
[0002] The board is generally made of wood, and the skin feeling is because the board is covered with a skin film or coated with skin paint. The so-called skin feeling board means that when we touch the wood board with our hands, it feels like baby skin. At present, the skin feeling decorative panels are mainly divided into UV skin feeling boards and PET skin feeling boards. There is no difference between the two categories, and the main differences are in flatness, color, environmental protection level and price. PET board is a popular board decoration material in the market in recent years. PET board is the abbreviation of Polyethyleneterephthalate in English, referred to as PET board or PETP board.
[0003] At present, PET skin-feel board is made by making a layer of skin-feel UV coating on PET film, and then compounding it to the board with PUR adhesive. Similar to the common UV skin-feel board, the super matte surface is achieved by adding matting powder fillers to UV coating. The matte effect is achieved due to the scattering of light by the protrusions formed by the filler in the coating. It is irregular and uneven, and has a poor hand feel. In addition, matting powder is easy to thicken and has high thixotropy. The amount added to the coating is limited, and the matting ability is poor, so it is difficult to achieve a super matte effect (gloss 0-3gu). Moreover, due to oxygen inhibition on the light-cured surface, there will be some uncured components in the UV coating, which brings odor and low hardness.
[0004] In order to improve the shortcomings of PET skin-feel boards and ordinary UV skin-feel boards, such as difficulty in matting, poor skin feel, odor, and low hardness, Germany and Japan have introduced the technology of curing UV coatings with excimer lamps, that is, UV coatings can generate free radicals after absorbing 172-nanometer ultraviolet rays. The penetration depth of 172-nanometer ultraviolet rays is only 100 to 500 nanometers, so only a very thin layer of the coating on the surface is cured. The polymerization and cross-linking of this thin layer will shrink to form a rough surface and float on the uncured lower layer of liquid. No matting powder is required to achieve an ultra-matte surface effect.
[0005] However, the excimer lamp curing technology must be carried out in an environment of high-purity nitrogen (control the oxygen concentration below 100ppm). If it is cured in the air or in the presence of oxygen, oxygen inhibition reaction will occur, and the ink or coating surface will not be completely cured. Therefore, nitrogen is used to drive away oxygen, so that the oxygen concentration in the operating environment can be lower than 100ppm; this can achieve odor-free, and can provide higher surface hardness and high coating density. Therefore, the excimer lamp solves three problems: the first is physical extinction, the lowest brightness can reach 0°; the second is the surface hardness, which can reach up to 4h, solving the problem of scratch resistance; the third is no odor, the smell of traditional skin-feel UV is a flaw.
[0006] However, excimer lamp curing has the following disadvantages: First, a large amount of high-purity nitrogen is required during operation, which has high operating costs. Second, the one-time investment cost of the equipment is high, and it can only process flat products. If the flatness of the large plate is not enough, defective products will appear. The standard working life of the excimer lamp is normally 3,000 hours, and it is also easy to be damaged due to improper maintenance. The price of an imported light source is about 80,000 yuan. Summary of the invention
[0007] In view of this, the object of the present invention is to provide an ultra-matte skin-feel decorative panel and a preparation method thereof. The preparation method provided by the present invention does not require the use of nitrogen, and the prepared ultra-matte skin-feel decorative panel has high hardness, low gloss and good skin feel.
[0008] The present invention provides a method for preparing an ultra-matte skin-feel decorative panel, comprising the following steps:
[0009] a) mixing polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling additive to obtain EB skin sensitizer;
[0010] b) after printing UV ink on the PUR double-sided pre-coated film, UV curing is performed, and then the EB skin-sensitive light oil obtained in step a) is coated, and EB curing is performed while being squeezed by a matte steel roller to obtain an EB skin-feel film;
[0011] c) Compounding the EB skin-feel film obtained in step b) onto a substrate by means of a PUR hot-melt adhesive to obtain an ultra-matte skin-feel decorative panel.
[0012] Preferably, the polyurethane acrylate in step a) is selected from one or more of allnex resin EB1290, allnex resin EB5129 and allnex resin EB9260;
[0013] The polyether acrylate is selected from allnex resin EB83 and / or allnex resin EB841;
[0014] The multifunctional monomer is trimethylolpropane triacrylate;
[0015] The anti-fouling agent is selected from BYK333 and / or Tego2700.
[0016] Preferably, the mass ratio of the polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling agent in step a) is (40-60): (15-40): (10-40): (1-2).
[0017] Preferably, the mixing temperature in step a) is 20° C. to 30° C., the rotation speed is 1500 rpm to 2500 rpm, and the time is 20 min to 40 min.
[0018] Preferably, the PUR double-sided pre-coated film in step b) is a PET film pre-coated with PUR on both sides; the thickness of the PUR is 10 μm to 20 μm; the thickness of the PUR double-sided pre-coated film is 100 μm to 300 μm.
[0019] Preferably, the thickness of the printed UV ink in step b) is 2 μm to 20 μm.
[0020] Preferably, the curing energy of the UV curing in step b) is 200 mj / cm 2 ~1000mj / cm 2 , the curing speed is 20m / min~30m / min.
[0021] Preferably, the gram weight of the EB skin light-sensitive oil obtained by coating step a) in step b) is 5 g / m 2 ~30g / m 2 .
[0022] Preferably, the pressure of the matte steel roller in step b) is 5 g / cm 2 ~20g / cm 2 ; The curing dose of the EB curing is 30kGy~100kGy, and the curing energy is 200kev~600kev.
[0023] The present invention also provides an ultra-matte skin-feel decorative panel, which is prepared by the preparation method described in the above technical solution.
[0024] The present invention provides an ultra-matte skin-feel decorative panel and a preparation method thereof; the preparation method comprises the following steps: a) mixing polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling additive to obtain EB skin-sensitive oil; b) after printing UV ink on the PUR double-sided pre-coated film, UV curing is performed, and then the EB skin-sensitive oil obtained in step a) is coated, and EB curing is performed while matte steel rollers are extruded to obtain an EB skin-feel film; c) the EB skin-feel film obtained in step b) is compounded onto a substrate through a PUR hot melt adhesive to obtain an ultra-matte skin-feel decorative panel. Compared with the prior art, the preparation method provided by the present invention adopts specific process steps to achieve better overall interaction, and by introducing electron beam (EB) curing, there is no need to use nitrogen, and the ultra-matte skin-feel decorative panel prepared at the same time has high hardness, low gloss and good skin feel.
[0025] In addition, the preparation method provided by the present invention has a simple process, mild conditions, and is easy to control. It can realize continuous and automated production of EB skin-feeling films, is suitable for large-scale industrialization, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a flow chart for producing the EB skin feel film. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The present invention provides a method for preparing an ultra-matte skin-feel decorative panel, comprising the following steps:
[0029] a) mixing polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling additive to obtain EB skin sensitizer;
[0030] b) after printing UV ink on the PUR double-sided pre-coated film, UV curing is performed, and then the EB skin-sensitive light oil obtained in step a) is coated, and EB curing is performed while being squeezed by a matte steel roller to obtain an EB skin-feel film;
[0031] c) Compounding the EB skin-feel film obtained in step b) onto a substrate by means of a PUR hot-melt adhesive to obtain an ultra-matte skin-feel decorative panel.
[0032] The present invention first mixes polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling agent to obtain EB skin light oil. In the present invention, the polyurethane acrylate has better hardness and faster curing speed, and is preferably selected from one or more of allnex resin EB1290, allnex resin EB5129 and allnex resin EB9260, and more preferably allnex resin EB1290 and / or allnex resin EB9260. The present invention has no special restrictions on the source of the polyurethane acrylate, and commercially available products known to those skilled in the art can be used.
[0033] In the present invention, the polyether acrylate has a faster curing speed, and is preferably selected from allnex resin EB83 and / or allnex resin EB841, and more preferably allnex resin EB83. The present invention has no special restrictions on the source of the polyether acrylate, and commercially available products known to those skilled in the art can be used.
[0034] In the present invention, the multifunctional monomer is preferably trimethylolpropane triacrylate; any commercially available product well known to those skilled in the art may be used.
[0035] In the present invention, the anti-fouling agent has lower surface tension and better miscibility, and is preferably selected from BYK 333 and / or Tego 2700, and more preferably BYK 333. The present invention has no particular limitation on the source of the anti-fouling agent, and commercially available products known to those skilled in the art can be used.
[0036] In the present invention, the mass ratio of the polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling agent is preferably (40-60):(15-40):(10-40):(1-2), and more preferably 50:20:30:1.
[0037] In the present invention, the mixing method is preferably high-speed stirring; the temperature of the high-speed stirring is preferably 20°C to 30°C, the rotation speed is preferably 1500rpm to 2500rpm, more preferably 2000rpm, and the time is preferably 20min to 40min, more preferably 30min.
[0038] After obtaining the EB skin-sensitive oil, the present invention prints UV ink on the PUR double-sided pre-coated film, performs UV curing, and then applies the obtained EB skin-sensitive oil, and performs EB curing while extruding with a matte steel roller to obtain an EB skin-feel film.
[0039] In the present invention, the flow chart of producing EB skin feel film is shown in Figure 1 shown.
[0040] In the present invention, the PUR double-sided pre-coated film is preferably a PET film with double-sided pre-coated PUR, wherein the thickness of the PUR is preferably 10 μm to 20 μm, more preferably 15 μm, and the thickness of the PET film (not double-sided pre-coated with PUR) is preferably 80 μm to 260 μm, more preferably 220 μm; on this basis, the thickness of the PUR double-sided pre-coated film is preferably 100 μm to 300 μm, more preferably 250 μm; if the thickness of the PUR double-sided pre-coated film is too thin, it will affect the adhesion of the coating and the strength of the matte film, and if it is too thick, it will increase the production cost. The present invention has no special restrictions on the source of the PUR double-sided pre-coated film, and commercially available products known to those skilled in the art can be used.
[0041] The present invention has no special restriction on the source of the UV ink, and commercially available products or self-made products known to those skilled in the art can be used. The UV ink is UV decorative ink. In the actual production process, each time the UV decorative ink is printed in one color, it should be UV cured once before printing the next color. The present invention has no special restriction on this, and the process of printing the UV ink is uniformly performed once here.
[0042] In the present invention, the thickness of the printed UV ink is preferably 2 μm to 20 μm, more preferably 4 μm to 6 μm.
[0043] In the present invention, the curing energy of the UV curing is preferably 200 mj / cm 2 ~1000mj / cm 2 , more preferably 600 mj / cm 2 ~800mj / cm 2 The curing speed of the UV curing is preferably 20m / min to 30m / min, more preferably 25m / min.
[0044] In the present invention, the gram weight of the EB skin-sensitive oil obtained in the coating step a) is preferably 5 g / m 2 ~30g / m 2 , more preferably 15g / m 2 ~25g / m 2 .
[0045] In the present invention, the pressure of the matte steel roller is preferably 5g / cm 2 ~20g / cm 2 , more preferably 10 g / cm 2 ~15g / cm 2; The ultra-matte skin-feel effect of the skin-sensitive varnish comes from the rubbing of the matte steel roller, and radiation curing is performed while rubbing, specifically EB curing. The curing dose of the EB curing is preferably 30kGy~100kGy, more preferably 40kGy~50kGy, and the curing energy is preferably 200kev~600kev, more preferably 400kev~500kev; the EB curing process does not require a nitrogen atmosphere.
[0046] After obtaining the EB skin-feel film, the present invention compounds the obtained EB skin-feel film to a substrate through a PUR hot melt adhesive to obtain an ultra-matte skin-feel decorative panel. The present invention has no special restrictions on the type and source of the PUR hot melt adhesive and the substrate, and the PUR hot melt adhesive and substrate for producing decorative panels that are well known to those skilled in the art can be used. The present invention mainly prints UV ink (conventional UV-curing decorative ink) on a PUR double-sided pre-coated film, and then applies a layer of EB-curing special varnish (EB skin-sensitive varnish) after ultraviolet light (UV) curing, and simultaneously performs EB curing through the extrusion of a matte steel roller, and then rolls it up to obtain an EB skin-feel film; when in use, cut the matte skin-feel film (i.e., the above-mentioned EB skin-feel film) to a suitable size and compound it to the board with PUR hot melt adhesive.
[0047] The preparation method provided by the present invention has simple process, mild conditions and is easy to control, can realize continuous and automated production of EB skin-feel film, is suitable for large-scale industrialization, and has broad application prospects.
[0048] The present invention also provides an ultra-matte skin-feel decorative panel, which is prepared by the preparation method described in the above technical solution. The preparation method provided by the present invention adopts specific process steps to achieve better overall interaction, and introduces electron beam (EB) curing without the need to use nitrogen. At the same time, the ultra-matte skin-feel decorative panel prepared has high hardness, low gloss and good skin feel.
[0049] The present invention provides an ultra-matte skin-feel decorative panel and a preparation method thereof; the preparation method comprises the following steps: a) mixing polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling additive to obtain EB skin-sensitive oil; b) after printing UV ink on the PUR double-sided pre-coated film, UV curing is performed, and then the EB skin-sensitive oil obtained in step a) is coated, and EB curing is performed while matte steel rollers are extruded to obtain an EB skin-feel film; c) the EB skin-feel film obtained in step b) is compounded onto a substrate through a PUR hot melt adhesive to obtain an ultra-matte skin-feel decorative panel. Compared with the prior art, the preparation method provided by the present invention adopts specific process steps to achieve better overall interaction, and by introducing electron beam (EB) curing, there is no need to use nitrogen, and the ultra-matte skin-feel decorative panel prepared at the same time has high hardness, low gloss and good skin feel.
[0050] In addition, the preparation method provided by the present invention has a simple process, mild conditions, and is easy to control. It can realize continuous and automated production of EB skin-feeling films, is suitable for large-scale industrialization, and has broad application prospects.
[0051] In order to further illustrate the present invention, the following examples are provided for detailed description.
[0052] Example 1
[0053] (1) Preparation of EB skin sensitizing oil:
[0054] 30 kg of polyurethane Allnex resin EB1290, 20 kg of Allnex resin EB9260, 20 kg of difunctional polyether acrylate Allnex resin EB83, 30 kg of trimethylolpropane triacrylate (TMPTA), and 1 kg of stain-resistant additive BYK333 were put into a reactor and stirred at room temperature and high speed (2000 rpm) for 30 min to obtain EB skin-sensitive oil.
[0055] (2) Making EB skin-feeling film:
[0056] UV ink was printed on a PET film pre-coated with PUR on both sides (PET film thickness was 220 μm, PUR thickness on each side was 15 μm, and the total pre-coated film thickness was 250 μm), with a printing thickness of 4 μm; UV curing (curing energy was 700 mj / cm 2 , curing speed is 25m / min) and then coated with the EB skin sensitive oil obtained in step (1), with a coating weight of 20g / m 2 , squeezed with a matte steel roller (extrusion pressure of 15g / cm 2 ) EB curing is carried out at the same time as the varnish, the curing dosage is 40kGy, the curing energy is 500kev, the gloss of the steel roller is printed on the varnish, and then rolled up to obtain the EB skin-feel film.
[0057] (3) Make super matte skin-feel decorative panels:
[0058] The EB skin-feel film obtained in step (2) is cut to the size of the substrate, and then compounded onto the substrate using brand Zhengye T-1020F and PUR hot melt adhesive to obtain an ultra-matte skin-feel decorative panel.
[0059] Example 2
[0060] (1) Preparation of EB skin sensitizing oil:
[0061] 50 kg of polyurethane Allnex resin EB1290, 20 kg of difunctional polyether acrylate Allnex resin EB83, 30 kg of trimethylolpropane triacrylate (TMPTA), and 1 kg of stain-resistant additive BYK333 were put into a reactor and stirred at room temperature and high speed (2000 rpm) for 30 min to obtain EB skin-sensitive oil.
[0062] (2) Making EB skin-feeling film:
[0063] UV ink was printed on a PET film pre-coated with PUR on both sides (PET film thickness was 220 μm, PUR thickness on each side was 15 μm, and the total pre-coated film thickness was 250 μm), with a printing thickness of 4 μm; UV curing (curing energy was 700 mj / cm 2 , curing speed is 25m / min) and then coated with the EB skin sensitive oil obtained in step (1), with a coating weight of 20g / m 2 , squeezed with a matte steel roller (extrusion pressure of 15g / cm 2 ) EB curing is carried out at the same time as the varnish, the curing dosage is 40kGy, the curing energy is 500kev, the gloss of the steel roller is printed on the varnish, and then rolled up to obtain the EB skin-feel film.
[0064] (3) Make super matte skin-feel decorative panels:
[0065] The EB skin-feel film obtained in step (2) is cut to the size of the substrate, and then compounded onto the substrate using brand Zhengye T-1020F and PUR hot melt adhesive to obtain an ultra-matte skin-feel decorative panel.
[0066] Comparative Example 1
[0067] (1) Preparation of UV varnish containing matting powder:
[0068] 50 kg of polyurethane Allnex resin EB1290, 20 kg of difunctional polyether acrylate Allnex resin EB83, 30 kg of trimethylolpropane triacrylate (TMPTA), 1 kg of stain resistance agent BYK333, 10 kg of matting powder (Tosoh E-1011), and 5 kg of photoinitiator 184 were put into a reactor and stirred at room temperature and high speed (2000 rpm) for 30 min to obtain UV varnish containing matting powder.
[0069] (2) Making UV skin-feel film:
[0070] UV ink was printed on a PET film pre-coated with PUR on both sides (PET film thickness was 220 μm, PUR thickness on each side was 15 μm, and the total pre-coated film thickness was 250 μm), with a printing thickness of 4 μm; UV curing (curing energy was 700 mj / cm 2, curing speed is 25m / min) and then coated with UV varnish containing matting powder obtained in step (1), with a coating weight of 20g / m 2 , perform secondary UV curing (curing energy is 600mj / cm 2 , curing speed is 25m / min), and then rolled up to obtain a UV skin-feel film.
[0071] (3) Make super matte skin-feel decorative panels:
[0072] The UV skin-feel film obtained in step (2) is cut to the size of the substrate, and then compounded onto the substrate using brand Zhengye T-1020F, PUR hot melt adhesive to obtain a matte skin-feel decorative panel.
[0073] Comparative Example 2
[0074] (1) Preparation of excimer skin sensitive oil:
[0075] 50 kg of polyurethane Allnex resin EB1290, 20 kg of difunctional polyether acrylate Allnex resin EB83, 30 kg of trimethylolpropane triacrylate (TMPTA), 1 kg of stain resistance additive BYK333, and 5 kg of photoinitiator 184 were put into a reactor and stirred at room temperature and high speed (2000 rpm) for 30 min to obtain an excimer skin-sensitive light oil.
[0076] (2) Make super matte skin-feel decorative panels:
[0077] Apply UV primer on the substrate for UV curing (curing energy is 700mj / cm 2 , curing speed is 25m / min), after the primer is UV cured, the excimer skin sensitive light oil obtained in step (1) is applied, and the coating weight is 20g / m 2 After pre-curing with a 172 nm excimer lamp (cured in a nitrogen atmosphere with oxygen concentration controlled below 100 ppm), the film was cured with a mercury lamp (800 mj / cm 2 , curing speed 25m / min) to completely cure and obtain an ultra-matte skin-feel decorative panel.
[0078] Various properties of the decorative panels provided in Examples 1-2 and Comparative Examples 1-2 were tested, and the results are shown in Table 1.
[0079] Table 1 Performance data of the decorative panels provided by Examples 1 to 2 and Comparative Examples 1 to 2
[0080]
[0081] As can be seen from Table 1, compared with Comparative Example 1, Example 2 has no oxygen inhibition problem because oxygen is isolated during curing, and the crosslinking density of EB curing is lower than that of UV curing. Therefore, the decorative panel prepared has higher hardness, and the gloss comes from the rubbing of the matte steel roller, so the gloss can be made very low. Because no matting powder is used, the skin feel is very good; and the surface is well cured without odor.
[0082] Compared with comparative example 2, embodiment 2 has a higher hardness of the decorative panel because the cross-linking density of EB curing is higher than that of UV curing. No nitrogen is required during the production process, which has certain economic benefits.
[0083] In summary, the preparation method of the ultra-matte skin-feel decorative panel provided by the present invention does not require the use of nitrogen, and the prepared ultra-matte skin-feel decorative panel has high hardness, low gloss and good skin feel.
[0084] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an ultra-matte skin-feel decorative panel, comprising the following steps: a) mixing polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling agent to obtain EB skin sensitive oil; the mass ratio of polyurethane acrylate, polyether acrylate, multifunctional monomer and anti-fouling agent is (40-60): (15-40): (10-40): (1-2); b) After printing UV ink on the PUR double-sided pre-coated film, UV curing is performed, and then the EB skin-sensitive oil obtained in step a) is coated, and EB curing is performed while extruding with a matte steel roller to obtain an EB skin-sensitive film; the matte steel roller extrusion pressure is 5g / cm 2 ~20g / cm 2 ; The curing dose of the EB curing is 40kGy~50kGy, and the curing energy is 400kev~500kev; c) Compounding the EB skin-feel film obtained in step b) onto a substrate by means of a PUR hot-melt adhesive to obtain an ultra-matte skin-feel decorative panel.
2. The preparation method according to claim 1, characterized in that: The multifunctional monomer in step a) is trimethylolpropane triacrylate.
3. The preparation method according to claim 1, characterized in that: The mixing temperature in step a) is 20° C. to 30° C., the rotation speed is 1500 rpm to 2500 rpm, and the time is 20 min to 40 min.
4. The preparation method according to claim 1, characterized in that: The PUR double-sided pre-coated film in step b) is a PET film pre-coated with PUR on both sides; the thickness of the PUR is 10 μm to 20 μm; the thickness of the PUR double-sided pre-coated film is 100 μm to 300 μm.
5. The preparation method according to claim 1, characterized in that: The thickness of the printed UV ink in step b) is 2 μm to 20 μm.
6. The preparation method according to claim 1, characterized in that: The curing energy of the UV curing in step b) is 200 mj / cm 2 ~1000mj / cm 2 , the curing speed is 20m / min~30m / min.
7. The preparation method according to claim 1, characterized in that: The gram weight of the EB skin-sensitive oil obtained by coating step a) in step b) is 5 g / m 2 ~30g / m 2 .
8. An ultra-matte skin-feel decorative panel, characterized in that: The method is prepared by any one of claims 1 to 7.
Citation Information
Patent Citations
Electronic beam cured paper packaging gloss oil and curing method of printed coating
CN109666381A
Matte high-temperature release paper for leather and preparation method thereof
CN113445362A
PET decorating film with scratch resistance and excellent sense of touch
CN208182911U