Halogen-free, non-perfluoroalkyl sulfonate flame-retardant PC for electronic and electrical film and preparation method thereof
Through the synergistic action of silicon-based and phosphorus-based flame retardant, a flame-retardant PC film without halogen and perfluoroalkyl sulfonate is prepared, which solves the environmental and health risks in flame retardant modification in the prior art. It achieves high flame retardant and environmentally friendly PC film materials, comply with the UL 94 V-0 level standard.
Patent Information
- Application Number
- CN202110365215.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-04-06
AI Technical Summary
The halogenated flame retardants used in flame retardant modification of existing PC films have environmental and health risks, and halogen-free flame retardants such as perfluoroalkyl sulfonates are subject to EU regulations, making it difficult to meet high flame retardancy and environmental protection. Require.
Using the synergistic effect of silicon-based and phosphorus-based flame retardant, flame retardant PC without halogen and perfluoroalkyl sulfonate is prepared by mixing PC resin, anti-dripping agent, carbon black, antioxidant and dispersant. The film is mixed and granulated by high-speed stirring and twin-screw extrusion process.
It achieves high flame retardancy, good heat resistance and insulation, and complies with environmental protection standards, is not restricted by EU regulations, and can achieve the flame retardant effect of UL 94 V-0 level under a thickness of 0.4mm.
Smart Images

Figure 158550DEST_PATH_IMAGE002
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame-retardant PC, in particular to a halogen-free, perfluorinated alkyl sulfonate-free flame-retardant PC for electronic and electrical thin films and a preparation method thereof. Background Art
[0002] Polycarbonate (PC) is an amorphous polymer with high strength, high heat resistance, high toughness and excellent electrical insulation. It is widely used in the electronic and electrical industry. Among them, PC film is widely used in electronic and electrical equipment as an electronic insulation layer. Due to safety requirements, PC film used in electronic and electrical products must have excellent flame retardant properties.
[0003] For PC that can reach UL 94 V-0 level at a thickness of 0.4 mm, the commonly used flame retardants are divided into two categories: halogen flame retardants and halogen-free flame retardants. Among them, halogen flame retardants are mainly decabromodiphenylethane, brominated triazine, brominated polycarbonate oligomers, etc. These flame retardants will decompose and release corrosive hydrogen halide gas during heating or combustion, which is extremely harmful to the environment and human body. Halogen-free flame retardants include phosphorus flame retardants, perfluoroalkyl sulfonates and silicon flame retardants. Among them, the addition of phosphorus flame retardants can effectively promote the carbonization of PC and improve the flame retardancy of PC, but at the same time it will also degrade PC, seriously reduce its toughness and heat resistance, and is not conducive to film drawing, so it is not suitable to add a large amount; Silicon flame retardants have the advantages of high thermal stability and environmental protection. In recent years, they have been gradually used in the flame retardant modification of polymers such as PC, but their flame retardant efficiency is low, and they often cannot achieve the ideal flame retardant effect when used alone; Perfluoroalkyl sulfonate is a highly efficient flame retardant for PC. Due to its small addition amount and high thermal stability, it is widely used in the flame retardant modification of PC films. Among them, perfluorobutyl sulfonate is the most used. However, on January 16, 2020, the European Chemical Agency included perfluorobutyl sulfonic acid substances in the SVHC candidate list, becoming a substance of high concern (SVHC), and its application in PC flame retardant modification will be greatly restricted. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film and a preparation method thereof, and utilizes the synergistic effect of two environmentally friendly flame retardants, silicon-based and phosphorus-based, to prepare a flame-retardant PC material with high flame retardancy, high insulation, good heat resistance and not restricted by relevant laws and regulations of countries or regions such as the European Union.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A halogen-free, non-perfluoroalkyl sulfonate flame-retardant PC for electronic and electrical film, characterized in that it is composed of the following components in percentage by mass:
[0007] PC resin: 87-92%;
[0008] Flame retardant: 6-10%;
[0009] Anti-dripping agent: 0.2~0.5%;
[0010] Carbon black: 0.5-2%;
[0011] Antioxidant: 0.3~0.5%;
[0012] Dispersant: 0.3~0.8%.
[0013] Furthermore, preferably, the PC resin is bisphenol A aromatic polycarbonate, and its relative molecular weight is 20,000-30,000.
[0014] Furthermore, preferably, the flame retardant is a compound of an organosilicon flame retardant and a phosphorus flame retardant.
[0015] Further, preferably, the phosphorus-based flame retardant is one or more of SPB-100, TPP, RDP, and PX220; the silicon-based flame retardant is one or more of SIFR-875SF, MR-01, and RM4-7081.
[0016] Furthermore, preferably, the antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant.
[0017] Furthermore, preferably, the main component of the anti-dripping agent is polytetrafluoroethylene.
[0018] Furthermore, preferably, the carbon black is carbon black powder or carbon black masterbatch.
[0019] Further, preferably, the dispersant is one or more of ethylene bisstearamide, dimethyl silicone oil, pentaerythritol stearate, and polyethylene wax.
[0020] A method for preparing halogen-free and perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, comprising the following steps:
[0021] Step (1): Add fully dried PC resin, flame retardant, carbon black, anti-dripping agent, antioxidant and dispersant into a high-speed mixer and mix for 3 to 5 minutes;
[0022] Step (2): Add the mixture obtained in step (1) into a twin-screw extruder for melt blending and extrusion granulation to obtain halogen-free and perfluoroalkyl sulfonate-free flame-retardant PC.
[0023] Furthermore, preferably, the motor power of the high-speed stirrer in step (1) is 30 kw, and the main shaft speed is 475 rpm.
[0024] Furthermore, preferably, the aspect ratio of the twin-screw extruder in step (2) is 36-52, the screw speed is 200-300 rpm, and the extrusion temperature is 240-260°C.
[0025] The beneficial effects of this technical solution are as follows:
[0026] (1) The flame retardants used in the present invention are phosphorus-based and silicon-based flame retardants, both of which are environmentally friendly flame retardants and are not restricted by relevant laws and regulations of countries or regions such as the European Union.
[0027] (2) The present invention reduces the adverse effects of using phosphorus-based flame retardants alone on the thermal and mechanical properties of PC materials by using a combination of phosphorus-based flame retardants and silicon-based flame retardants, and also improves the flame retardant efficiency of silicon-based flame retardants. The resulting flame-retardant PC material can reach UL 94 V-0 level at a thickness of 0.4 mm, and has good thermal, mechanical and insulation properties. DETAILED DESCRIPTION
[0028] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples.
[0029] Example 1
[0030] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films, which is composed of the following components in percentage by mass: PC resin (ET3113): 90; flame retardant (SPB-100): 7.5; flame retardant (SIFR-875SF): 0.5; anti-dripping agent (polytetrafluoroethylene): 0.3; carbon black powder): 0.7; antioxidant (168): 0.2; antioxidant (1010): 0.3; dimethyl silicone oil: 0.5.
[0031] The following steps are adopted: Step (1): Add fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mix for 3 minutes at a speed of 475 rpm.
[0032] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 36, the screw speed is 250 rpm, and the extrusion temperature is 240-260 °C, to obtain product A.
[0033] Example 2
[0034] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, which is composed of the following components in percentage by mass: PC resin (1250Y): 89; flame retardant (TPP): 7; flame retardant (MR-01): 2; anti-dripping agent (polytetrafluoroethylene): 0.3; carbon black powder: 0.7; antioxidant (B190): 0.4; pentaerythritol stearate: 0.6.
[0035] The following steps are adopted: Step (1): adding fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mixing for 3 minutes at a speed of 475 rpm;
[0036] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 36, the screw speed is 250 rpm, and the extrusion temperature is 240-260 °C to obtain product B.
[0037] Example 3
[0038] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, which is composed of the following components in percentage by mass: PC resin (1250Y): 87; flame retardant (PX220): 8; flame retardant (MR-01): 2; anti-dripping agent (polytetrafluoroethylene): 0.3; carbon black masterbatch: 2; antioxidant (JC-1201): 0.3; ethylene bisstearamide: 0.2; pentaerythritol stearate: 0.2.
[0039] The following steps are adopted: Step (1): adding fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mixing for 4 min at a speed of 475 rpm;
[0040] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 40, the screw speed is 200 rpm, and the extrusion temperature is 240-260 °C to obtain product C.
[0041] Example 4
[0042] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, which is composed of the following components in percentage by mass: PC resin (E-2000): 90; flame retardant (SPB-100): 6; flame retardant (SIFR-875SF): 0.5; flame retardant (RM4-7081): 1; anti-dripping agent (polytetrafluoroethylene): 0.2; carbon black masterbatch: 1.5; antioxidant (JC-1201): 0.3; pentaerythritol stearate: 0.3; dimethyl silicone oil: 0.2.
[0043] The following steps are adopted: Step (1): adding fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mixing for 3 min at a speed of 475 rpm;
[0044] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 52, the screw speed is 200 rpm, and the extrusion temperature is 240-260 °C to obtain product D.
[0045] Example 5
[0046] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, which is composed of the following components in mass percentage: PC resin (ET3113): 89; flame retardant (RDP): 7; flame retardant (SIFR-875SF): 0.5; flame retardant (RM4-7081): 1.5; anti-dripping agent (polytetrafluoroethylene): 0.3; carbon black powder: 0.7; antioxidant (168): 0.2; antioxidant (1010): 0.3; polyethylene wax: 0.3; dimethyl silicone oil: 0.2.
[0047] The following steps are adopted: Step (1): adding fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mixing for 3 minutes at a speed of 475 rpm;
[0048] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 36, the screw speed is 250 rpm, and the extrusion temperature is 240-260 °C to obtain product E.
[0049] Example 6
[0050] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, which is composed of the following components in percentage by mass: PC resin (1250Y): 95; flame retardant (MR-01): 2; anti-dripping agent (polytetrafluoroethylene): 0.3; carbon black masterbatch: 2; antioxidant (JC-1201): 0.3; ethylene bisstearamide: 0.2; pentaerythritol stearate: 0.2.
[0051] The following steps are adopted: Step (1): adding fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mixing for 3 min at a speed of 475 rpm;
[0052] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 36, the screw speed is 250 rpm, and the extrusion temperature is 240-260 °C to obtain product F.
[0053] Example 7
[0054] As a most basic implementation scheme of the present invention, this embodiment discloses a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, which is composed of the following components in mass percentage: PC resin (1250Y): 89; flame retardant (PX220): 8; anti-dripping agent (polytetrafluoroethylene): 0.3; carbon black masterbatch: 2; antioxidant (JC-1201): 0.3; ethylene bisstearamide: 0.2; pentaerythritol stearate: 0.2.
[0055] The following steps are adopted: Step (1): adding fully dried PC resin, flame retardant, carbon black, anti-dripping agent and other raw materials into a high-speed mixer and mixing for 3 min at a speed of 475 rpm;
[0056] (2) The mixture obtained in step (1) is added into a twin-screw extruder for melt blending and extrusion granulation, wherein the aspect ratio of the twin-screw extruder is 36, the screw speed is 250 rpm, and the extrusion temperature is 240-260 °C, to obtain product G.
[0057] The products A to G obtained in Examples 1 to 7 were tested, and the test items and methods were as follows: tensile strength and elongation at break were tested according to ISO 527, IZOD notched impact strength was tested according to ISO 180, heat deformation temperature was tested according to ISO 75-2, flame retardancy was tested according to UL 94 standard, volume resistivity was tested according to IEC 60093, and dielectric strength was tested according to IEC 60243. The test results are shown in Table 1:
[0058]
[0059] In summary, after reading the present invention document, ordinary technicians in this field can make various other corresponding transformation schemes based on the technical scheme and technical concept of the present invention without creative mental labor, which all fall within the scope of protection of the present invention.
Claims
1. A halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film, characterized in that: It is composed of the following components in percentage by mass: PC resin: 87-92%; Flame retardant: 6-10%, the flame retardant is a compound of an organic silicon flame retardant and a phosphorus flame retardant; the phosphorus flame retardant is one or more of SPB-100, TPP, RDP, and PX220; the organic silicon flame retardant is one or more of SIFR-875SF, MR-01, and RM4-7081; Anti-dripping agent: 0.2~0.5%; Carbon black: 0.5-2%; Antioxidant: 0.3~0.5%; Dispersant: 0.3~0.8%.
2. The halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to claim 1, characterized in that: The PC resin is bisphenol A type aromatic polycarbonate, and its relative molecular weight is 20000-30000.
3. The halogen-free and perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to claim 1, characterized in that: The antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant.
4. The halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to claim 1, characterized in that: The main component of the anti-dripping agent is polytetrafluoroethylene.
5. The halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to claim 1, characterized in that: The carbon black is carbon black powder or carbon black masterbatch.
6. The halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to claim 1, characterized in that: The dispersant is one or more of ethylene bis stearamide, dimethyl silicone oil, pentaerythritol stearate and polyethylene wax.
7. A method for preparing a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to any one of claims 1 to 6, comprising the following steps: Step (1): Add fully dried PC resin, flame retardant, carbon black, anti-dripping agent, antioxidant and dispersant into a high-speed mixer and mix for 3 to 5 minutes; Step (2): adding the mixture obtained in step (1) into a twin-screw extruder for melt blending and extrusion granulation to obtain halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical film.
8. The method for preparing a halogen-free, perfluoroalkyl sulfonate-free flame-retardant PC for electronic and electrical thin films according to claim 7, characterized in that: The twin-screw extruder in step (2) has an aspect ratio of 36-52, a screw speed of 200-300 rpm, and an extrusion temperature of 240-260°C.