A carbon nitride / carbon nanotube composite film and its preparation method and application

Through the ultrasonic dispersion and shearing technology of carbon nitride/carbon nanotube composite films, the thermoelectric properties of carbon nitride materials are improved, the problem of low thermoelectric conversion efficiency of existing carbon nitride materials is solved, and high power factor and flexibility are achieved Applications of Thermoelectric Materials.

CN115172578BActive Publication Date: 2024-10-15GUANGZHOU HABER NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210774797.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-01
Publication Date
2024-10-15
Estimated Expiration
2042-07-01

AI Technical Summary

Technical Problem

The application of existing carbon nitride materials in the field of thermoelectric materials is limited by low bulk quantum yield and high photogenerated electron-hole recombination rate, resulting in low thermoelectric conversion efficiency.

Method used

Using carbon nitride/carbon nanotube composite film, through ultrasonic dispersion and shearing composite technology of graphitic phase carbon nitride nanoparticles and single-walled carbon nanotubes, the Seebeck coefficient and electrical conductivity are improved to form a high power factor thermoelectric material.

Benefits of technology

It achieves high conductivity, improved Seebeck coefficient and power factor, has good flexibility, is suitable for flexible wearable thermoelectric devices, and has a simple preparation method, low cost and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172578B_ABST
    Figure CN115172578B_ABST
Patent Text Reader

Abstract

The present invention provides a carbon nitride / carbon nanotube composite film and a preparation method and application thereof, wherein the carbon nitride / carbon nanotube composite film is obtained by compounding carbon nitride nanoparticles and carbon nanotubes. The carbon nitride / carbon nanotube composite film provided by the present invention has the advantages of high electrical conductivity, high Seebeck coefficient, high power factor, etc., and has good flexibility and is easy to bend, and has good application prospects in the field of flexible wearable thermoelectric devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials and relates to a carbon nitride / carbon nanotube composite film and a preparation method and application thereof. Background Art

[0002] Thermoelectric materials, also known as temperature-difference electric materials, are semiconductor functional materials that use the movement of carriers inside solids to achieve the mutual conversion between thermal energy and electrical energy. They have the advantages of small size, light weight, quiet operation, and no need for conversion media and mechanical moving parts. As a new type of energy material, they have attracted widespread attention.

[0003] Thermoelectric conversion efficiency of materials ZT = S 2 σT / κ, where S, σ, T, and κ are Seebeck coefficient, electrical conductivity, absolute temperature, and thermal conductivity, respectively. The larger the ZT value, the higher the conversion efficiency. Therefore, an excellent thermoelectric material needs to have a large Seebeck coefficient, high electrical conductivity, and low thermal conductivity.

[0004] Inorganic materials have been rapidly developed in the field of thermoelectric materials due to their high Seebeck coefficient and electrical conductivity. Some materials have been widely used in the fields of thermocouple temperature control and semiconductor refrigeration. Carbon nitride is a non-metallic semiconductor with advantages such as tunable photoelectric properties, high chemical stability, wide energy gap (bandgap), and low cost and easy synthesis. It is usually used as a photocatalyst, sensor and photovoltaic material. However, the low quantum yield of bulk carbon nitride and the high recombination rate of photogenerated electrons and holes limit its practical application. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a carbon nitride / carbon nanotube composite film and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art. The composite film of the present invention has good flexibility and excellent electrochemical properties, a high power factor, and has good application prospects in the field of flexible wearable thermoelectric devices when used as a thermoelectric material.

[0006] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0007] Provided is a carbon nitride / carbon nanotube composite film, which is obtained by composite carbon nitride nanoparticles and carbon nanotubes.

[0008] According to the above scheme, the carbon nitride nanoparticles are graphite-phase carbon nitride with a particle size of 49 to 94 nm. The graphite-phase carbon nitride has a stable structure and a layered structure similar to graphite.

[0009] According to the above scheme, the preparation method of the carbon nitride nanoparticles is: melamine is placed in a ceramic crucible, nitrogen is used as a nitrogen source, and heated to 500-600°C at a rate of 2-4°C / min, and the temperature is maintained for 2-6 hours. The obtained light yellow powder is ground into carbon nitride nanoparticles.

[0010] According to the above scheme, the carbon nanotubes are one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, and double-walled carbon nanotubes, preferably single-walled carbon nanotubes.

[0011] According to the above scheme, the mass fraction of carbon nitride in the carbon nitride / carbon nanotube composite film is 2.5-40%.

[0012] According to the above scheme, the thickness of the carbon nitride / carbon nanotube composite film is 0.0008-0.0012 cm.

[0013] The present invention also includes a method for preparing the carbon nitride / carbon nanotube composite film, the specific steps of which are as follows:

[0014] 1) ultrasonically dispersing carbon nanotubes in an organic solvent to obtain a carbon nanotube dispersion;

[0015] 2) ultrasonically dispersing carbon nitride nanoparticles in an organic solvent to obtain a carbon nitride dispersion;

[0016] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed uniformly, and then fully sheared with a handheld homogenizer, and then filtered under reduced pressure and washed to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried to obtain a carbon nitride / carbon nanotube composite film.

[0017] According to the above scheme, the organic solvent in step 1) is the same as the organic solvent in step 2), and is selected from one of anhydrous ethanol, dimethyl sulfoxide, and N,N-dimethylformamide.

[0018] According to the above scheme, the concentration of the carbon nanotube dispersion in step 1) is 0.7-1 mg / mL.

[0019] According to the above scheme, the concentration of the carbon nitride dispersion in step 2) is 0.02-0.7 mg / mL.

[0020] According to the above scheme, in step 3), the mass ratio of the carbon nanotubes in the carbon nanotube dispersion to the carbon nitride in the carbon nitride dispersion is 1.4 to 40:1.

[0021] According to the above scheme, in step 3), the ultrasonic dispersion time is 25 to 35 minutes and the power is 100 to 200W.

[0022] According to the above scheme, in step 3), the shearing time is 2 to 7 minutes, the shearing speed is 3000 to 5000 rpm, and the power is 180 to 200W.

[0023] According to the above scheme, in step 3), the vacuum drying temperature is 45-80° C., the vacuum drying time is 4-24 h, and the vacuum degree is 0.09-0.1 MPa.

[0024] The present invention also includes the application of the carbon nitride / carbon nanotube composite film in thermoelectric materials.

[0025] The invention adopts a thermal polymerization method to prepare graphite phase carbon nitride, disperses it in an organic solvent by ultrasonic method, and carries out ultrasonic shear compounding with carbon nanotubes, thereby effectively improving the conductivity while improving the Seebeck coefficient, so that the power factor is significantly improved.

[0026] The beneficial effects of the present invention are: 1. The carbon nitride / carbon nanotube composite film provided by the present invention has the advantages of high electrical conductivity, high Seebeck coefficient, high power factor, etc., and has good flexibility and is easy to bend, and has good application prospects in the field of flexible wearable thermoelectric devices;

[0027] 2. The preparation method of the present invention has simple steps, low cost, is green and environmentally friendly, and has good repeatability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a FESEM image of carbon nitride nanoparticles used in an embodiment of the present invention;

[0029] Figure 2 This is the FESEM image of the carbon nitride / carbon nanotube composite film prepared in Example 1. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0031] The preparation method of the carbon nitride nanoparticles used in the embodiment of the present invention is as follows: 5 g of melamine is placed in a ceramic crucible, nitrogen is introduced as a protective atmosphere, and the mixture is heated to 550° C. at a rate of 2.41° C. / min, and the mixture is kept at 550° C. for 4 h. The obtained light yellow powder is ground into carbon nitride nanoparticles having a particle size of 49 to 94 nm. The carbon nitride has a layered structure similar to graphite, and its FESEM image is as shown in FIG. Figure 1 shown.

[0032] Comparative Example 1

[0033] The preparation method of the carbon nanotube film is as follows: 10 mg of single-walled carbon nanotubes (diameter of 1 to 3 nm, aspect ratio of 5000 to 15000) are ultrasonically dispersed in 10 mL of anhydrous ethanol for 30 minutes, and dispersed with a handheld homogenizer for 2 minutes. The product is filtered and the filter cake is washed with anhydrous ethanol. The filter cake is then vacuum dried at 60° C. for 24 hours. The vacuum degree of the oven is 0.1 MPa to obtain a carbon nanotube film with a film thickness of 0.0008 cm.

[0034] Example 1

[0035] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0036] 1) adding 7.8 mg of single-walled carbon nanotubes (diameter of 1-3 nm, aspect ratio of 5000-15000) into 10 mL of anhydrous ethanol and ultrasonically dispersing for 30 min to obtain a carbon nanotube dispersion;

[0037] 2) adding 0.2 mg of carbon nitride nanoparticles into 10 mL of anhydrous ethanol and ultrasonically dispersing for 30 min to obtain a carbon nitride dispersion;

[0038] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at a power of 100 W, and then sheared with a handheld homogenizer for 2 minutes at a shear speed of 5000 rpm and a shear power of 180 W. The mixture is then filtered under reduced pressure and the filter cake is washed with anhydrous ethanol to obtain a filter membrane. Finally, the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film having a film thickness of 0.0010 cm and a mass fraction of carbon nitride in the composite film of 2.5%.

[0039] like Figure 2 The figure shows the FESEM image of the film sample prepared in this embodiment. It can be seen from the figure that the bundles of carbon nanotubes in the composite film prepared in this embodiment are smooth and uniform, and the graphite phase carbon nitride is perfectly attached to the surface of the carbon nanotube bundles to form a uniform and stable composite structure. The composite structure is uniform and stable, which is conducive to forming a composite film with a smooth surface, thereby effectively improving the Seebeck coefficient of the composite film.

[0040] Example 2

[0041] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0042] 1) ultrasonically dispersing 9.8 mg of single-walled carbon nanotubes in 10 mL of anhydrous ethanol to obtain a carbon nanotube dispersion;

[0043] 2) ultrasonically dispersing 0.8 mg of carbon nitride nanoparticles in 10 mL of anhydrous ethanol to obtain a carbon nitride dispersion;

[0044] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at an ultrasonic power of 100 W, and then sheared with a handheld homogenizer for 2 minutes at a shear power of 180 W, and then filtered under reduced pressure and the filter cake is washed with anhydrous ethanol to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film with a film thickness of 0.0011 cm and a mass fraction of carbon nitride in the composite film of 7.5%.

[0045] Example 3

[0046] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0047] 1) ultrasonically dispersing 10 mg of single-walled carbon nanotubes in 10 mL of anhydrous ethanol to obtain a carbon nanotube dispersion;

[0048] 2) ultrasonically dispersing 1.11 mg of carbon nitride nanoparticles in 10 mL of anhydrous ethanol to obtain a carbon nitride dispersion;

[0049] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at an ultrasonic power of 100 W, and then sheared with a handheld homogenizer for 2 minutes at a shear power of 180 W, and then filtered under reduced pressure and the filter cake is washed with anhydrous ethanol to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film with a film thickness of 0.0013 cm and a mass fraction of carbon nitride in the composite film of 10%.

[0050] Example 4

[0051] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0052] 1) ultrasonically dispersing 10 mg of single-walled carbon nanotubes in 10 mL of anhydrous ethanol to obtain a carbon nanotube dispersion;

[0053] 2) ultrasonically dispersing 2.5 mg of carbon nitride nanoparticles in 10 mL of anhydrous ethanol to obtain a carbon nitride dispersion;

[0054] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at an ultrasonic power of 100 W, and then sheared with a handheld homogenizer for 2 minutes at a shear power of 180 W, and then filtered under reduced pressure and the filter cake is washed with anhydrous ethanol to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film with a film thickness of 0.00135 cm and a mass fraction of carbon nitride in the composite film of 20%.

[0055] Example 5

[0056] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0057] 1) ultrasonically dispersing 10 mg of single-walled carbon nanotubes in 10 mL of anhydrous ethanol to obtain a carbon nanotube dispersion;

[0058] 2) ultrasonically dispersing 4.29 mg of carbon nitride nanoparticles in 10 mL of anhydrous ethanol to obtain a carbon nitride dispersion;

[0059] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at an ultrasonic power of 100 W, and then sheared with a handheld homogenizer for 2 minutes at a shear power of 180 W, and then filtered under reduced pressure and the filter cake is washed with anhydrous ethanol to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film with a film thickness of 0.0018 mm and a mass fraction of carbon nitride in the composite film of 30%.

[0060] Example 6

[0061] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0062] 1) ultrasonically dispersing 10 mg of single-walled carbon nanotubes in 10 mL of anhydrous ethanol to obtain a carbon nanotube dispersion;

[0063] 2) ultrasonically dispersing 6.67 mg of carbon nitride nanoparticles in 10 mL of anhydrous ethanol to obtain a carbon nitride dispersion;

[0064] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at an ultrasonic power of 100 W, and then sheared for 2 minutes with a handheld homogenizer at a shear power of 180 W, and then filtered under reduced pressure and the filter cake is washed with anhydrous ethanol to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film with a film thickness of 0.0017 cm and a mass fraction of carbon nitride in the composite film of 40%.

[0065] Example 7

[0066] A carbon nitride-doped carbon nanotube composite film, the specific preparation method is as follows:

[0067] 1) ultrasonically dispersing 7.8 mg of single-walled carbon nanotubes in 10 mL of dimethyl sulfoxide to obtain a carbon nanotube dispersion;

[0068] 2) ultrasonically dispersing 0.2 mg of carbon nitride nanoparticles in 10 mL of dimethyl sulfoxide to obtain a carbon nitride dispersion;

[0069] 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed for 30 minutes at an ultrasonic power of 100 W, and then sheared with a handheld homogenizer for 2 minutes at a shear power of 180 W, and then filtered under reduced pressure and the filter cake is washed with dimethyl sulfoxide to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried at 60° C. for 24 hours at a vacuum degree of 0.1 MPa to obtain a carbon nitride / carbon nanotube composite film with a film thickness of 0.0015 cm and a mass fraction of carbon nitride in the composite film of 2.5%.

[0070] The thermoelectric performance parameters of the thin film samples prepared in Comparative Example 1 and Examples 1-7 are shown in Table 1.

[0071] Table 1

[0072]

[0073] It can be seen from Table 1 that, compared with Comparative Example 1, the conductivity of Examples 1 to 6 shows a trend of first increasing and then decreasing, and the conductivity reaches a maximum of 70256.5 S / m at Example 1; and the Seebeck coefficients of Examples 1 to 6 are substantially improved compared with Comparative Example 1; the power factor reaches a maximum of 163.0 μW·m at Example 1. -1 ·K -2 .

Claims

1. A carbon nitride / carbon nanotube composite film thermoelectric material, characterized in that: The carbon nitride / carbon nanotube composite film is obtained by compounding carbon nitride nanoparticles and carbon nanotubes. The carbon nitride nanoparticles are graphite phase carbon nitride with a particle size of 49 to 94 nm. The carbon nanotubes are single-walled carbon nanotubes. The mass fraction of carbon nitride in the carbon nitride / carbon nanotube composite film thermoelectric material is 2.5 to 30%.

2. A method for preparing the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 1, characterized in that: The specific steps are as follows: 1) ultrasonically dispersing carbon nanotubes in an organic solvent to obtain a carbon nanotube dispersion; 2) ultrasonically dispersing carbon nitride nanoparticles in an organic solvent to obtain a carbon nitride dispersion; 3) The carbon nanotube dispersion obtained in step 1) is mixed with the carbon nitride dispersion obtained in step 2), and ultrasonically dispersed uniformly, and then fully sheared with a handheld homogenizer, and then filtered under reduced pressure and washed to obtain a filter membrane, and finally the obtained filter membrane is vacuum dried to obtain a carbon nitride / carbon nanotube composite thin film thermoelectric material.

3. The method for preparing the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 2, characterized in that: The organic solvent in step 1) is the same as the organic solvent in step 2), and is selected from anhydrous ethanol, dimethyl sulfoxide, and N,N-dimethylformamide.

4. The method for preparing the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 2, characterized in that: Step 1) The concentration of the carbon nanotube dispersion is 0.7-1 mg / mL.

5. The method for preparing the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 2, characterized in that: Step 2) The concentration of the carbon nitride dispersion is 0.02-0.7 mg / mL.

6. The method for preparing the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 2, characterized in that: The mass ratio of carbon nanotubes in the carbon nanotube dispersion in step 3) to carbon nitride in the carbon nitride dispersion is 1.4-40:1; the ultrasonic dispersion time in step 3) is 25-35 minutes, and the power is 100-200W; the shearing time in step 3) is 2-7 minutes, the shearing speed is 3000-5000rpm, and the power is 180-200W.

7. The method for preparing the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 2, characterized in that: In step 3), the vacuum drying temperature is 45-80° C., the vacuum drying time is 4-24 h, and the vacuum degree is 0.09-0.1 MPa.

8. Application of the carbon nitride / carbon nanotube composite thin film thermoelectric material according to claim 1 in thermoelectric materials.