A room temperature DMMP sensor based on copper ion modified polypyrrole / reduced graphene oxide, preparation method and application thereof

By modifying polypyrrole/reducing graphene oxide material by copper ion, adjusting hydrogen bond strength, improving the response performance of room-temperature DMMP sensors, solving the problems of low response and poor recovery characteristics of existing sensors, and achieving high DMMP gas at room temperature Sensitivity detection, suitable for industrial mass production.

CN115184411BActive Publication Date: 2024-11-22JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210811044.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-11-22
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

Existing room-temperature DMMP sensors based on polypyrrole and reduced graphene oxide have problems with low response and poor response recovery characteristics, and it is difficult to efficiently detect dimethyl methyl phosphate (DMMP) gas at room temperature.

Method used

Modification of polypyrrole/reducing graphene oxide (Cux+-PPy-rGO) materials through copper ions, adjust the hydrogen bond strength, improve the gas-sensitive performance of the sensor, adopt the planar structure and the design of interdigital electrodes, combining hydrothermal and impregnation methods Prepare sensors to achieve high sensitivity detection of DMMP at room temperature.

Benefits of technology

It realizes high sensitivity detection of DMMP gas at room temperature, has low detection limit, excellent selectivity, good repeatability and long-term stability, and is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115184411B_ABST
    Figure CN115184411B_ABST
Patent Text Reader

Abstract

A novel method based on copper ion modified polypyrrole / reduced graphene oxide (Cu x+ The invention relates to a room temperature DMMP sensor based on a polyethylene terephthalate (PET) substrate, a metal layer structured interdigital electrode printed on the PET substrate, and a Cu 2+ electrode coated on the interdigital electrode. x+ ‑PPy‑rGO gas sensitive film. In the present invention, copper ions are Cu 2+ Ions and Cu + The ion form exists stably in the hybrid, Cu + The presence of ions means that more charge is transferred from N atoms to Cu + ions and the formation of a stable Cu-N structure can effectively regulate the electron cloud density around the N atoms and H atoms in PPy, thereby regulating the hydrogen bonding between PPy and DMMP molecules and improving the sensitivity of the sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of resistive room temperature gas sensors, and specifically relates to a copper ion modified polypyrrole / reduced graphene oxide (Cu 2+) based on the hydrogen bond interaction principle for detecting dimethyl methyl phosphate (DMMP) at room temperature. x+ -PPy-rGO) room temperature DMMP sensor, preparation method and application in DMMP detection at room temperature. Background Art

[0002] Organophosphorus compounds refer to a class of phosphate derivatives containing organic groups. They are widely used as organophosphorus pesticides, organophosphorus nerve gases, etc. After being absorbed by the human body, they can inhibit the activity of acetylcholinesterase, resulting in the inability of acetylcholinesterase to hydrolyze acetylcholine, further causing nervous system disorders, and even death in severe cases. Therefore, real-time and accurate detection of the concentration of gaseous organophosphorus compounds in the environment is of great significance. From the perspective of experimental safety, organophosphorus pesticides and chemical warfare agents are prohibited from use in conventional laboratories due to their high toxicity. Laboratories usually use dimethyl methylphosphonate (DMMP), which has a similar chemical structure to organophosphorus compounds and has low toxicity, as a simulant of organophosphorus compounds for research.

[0003] In recent years, chemiresistive gas sensors have been widely used for the detection of organophosphorus compounds due to their low cost, simple structure, and compatibility with microelectromechanical systems. Although metal oxide-based gas sensors have the advantage of high sensitivity, metal oxide sensors usually operate at high temperatures, which results in high power consumption and increases the detection cost. Compared with metal oxides, polypyrrole and reduced graphene oxide have been widely used as sensitive materials for constructing room temperature DMMP sensors due to their advantages such as excellent conductivity and low electrical noise. However, room temperature DMMP sensors based on reduced graphene oxide (rGO) and polypyrrole (PPy) sensitive materials have problems such as low response and poor response recovery characteristics. These room temperature DMMP sensors mainly utilize hydrogen bonding interactions between sensing materials and DMMP molecules to complete DMMP detection. Therefore, regulating the hydrogen bonding strength is crucial for designing room temperature DMMP sensors with enhanced gas sensing performance. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to improve the hydrogen bonding between polypyrrole / reduced graphene oxide sensitive materials and DMMP molecules by assisting with copper ions, and to provide a method based on copper ion modified polypyrrole / reduced graphene oxide (Cu x+ -PPy-rGO) room temperature DMMP sensor, preparation method and application in DMMP detection at room temperature to solve the problems existing in the background technology.

[0005] The present invention is based on copper ion modified polypyrrole / reduced graphene oxide (Cu x+ The room temperature DMMP sensor based on Cu-PPy-rGO is a planar structure, which consists of a flexible polyethylene terephthalate (PET) substrate, an interdigital electrode with a metal layer structure printed on the PET substrate, and a gas sensitive film coated on the interdigital electrode. The gas sensitive film is Cu x+ -PPy-rGO, the gas sensitive film will change its resistance before and after being exposed to the target gas to be measured. By measuring the resistance value at both ends of the sensor's interdigital electrodes, the sensor response can be calculated. The response (S) is defined as S (%) = (R g -R a ) / R a ×100%, where R g and R a The sensor’s sensitive film material is Cu x+ -PPy-rGO, the preparation steps are as follows:

[0006] (1) Add 1.0-5.0 mL of 1-5 mg / mL graphene oxide (GO) aqueous solution into 20-50 mL of water and stir at room temperature for 0.5-2 h to obtain a graphene oxide (GO) dispersion;

[0007] (2) adding 1.0-3.0 mL of pyrrole (Py) to the dispersion of graphene oxide (GO) obtained in step (1), stirring at room temperature for 6-12 h to obtain a mixed solution of GO and Py;

[0008] (3) transferring the mixed solution of GO and Py obtained in step (2) into a hydrothermal reactor and treating at 180-220°C for 12-36 hours;

[0009] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0010] (5) Add 2.0-5.0 mg of PPy-rGO powder obtained in step (4) into 20-30 mL of 50-100 mM copper chloride aqueous solution and stir at room temperature for 2-3 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+ -PPy-rGO materials.

[0011] The Cu-based x+ The preparation method of room temperature DMMP sensor of -PPy-rGO, the steps are as follows:

[0012] (1) A flexible PET substrate is used as the substrate, and the length of the PET substrate is 10-12 mm, the width is 5-7 mm, and the thickness is 150-200 mm. A sputtering etching process is used to evaporate 10-20 pairs of interdigital electrodes with a metal layer structure on the upper surface of the PET substrate. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and their thicknesses are 10-15 μm, 4-6 μm and 1-3 μm respectively. The line width of the interdigital electrodes is 100-300 μm, and the line spacing is 100-300 μm.

[0013] (2) ultrasonically cleaning the flexible PET substrate and the interdigital electrodes obtained in step (1) with ethanol and water in sequence and drying them;

[0014] (3) Cu x+ -PPy-rGO powder is dispersed in water at a concentration of 2-10 mg / mL; the solution is drop-coated on the flexible PET substrate and the surface of the interdigital electrode after drying in step (2), and then heat-treated under an infrared lamp for 6-12 hours to obtain a Cu-based x+ Room temperature DMMP sensor based on PPy-rGO, Cu x+ -PPy-rGO film thickness is 10~50 μm.

[0015] The advantages of the present invention are:

[0016] 1) Cu in the present invention x+ -PPy-rGO sensitive material was synthesized by hydrothermal method and subsequent impregnation method, which has simple operation method, low cost and is suitable for mass production.

[0017] 2) In the present invention, Cu x+ -PPy-rGO room-temperature DMMP sensor has small size, simple preparation process, good film consistency, and is suitable for industrial mass production.

[0018] 3) Cu prepared by the present invention x+ -PPy-rGO sensor has excellent gas-sensing properties for DMMP gas at room temperature, including high sensitivity, low detection limit, excellent selectivity, good repeatability and long-term stability, and has good application prospects.

[0019] 4) The copper ion in the present invention is Cu 2+ Ions and Cu + The ion form exists stably in the hybrid, Cu + The presence of ions means that more charge is transferred from N atoms to Cu +ions and the formation of a stable Cu-N structure can effectively regulate the electron cloud density around the N atoms and H atoms in PPy, thereby regulating the hydrogen bonding between PPy and DMMP molecules and improving the sensitivity of the sensor. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the structure of the DMMP sensor prepared by the present invention.

[0021] The names of the parts are as follows: a flexible PET substrate 1, an interdigital electrode 2 having a metal layer structure deposited on the surface of the PET substrate 1 by a sputtering etching process, wherein the metal layer structure is composed of copper, nickel and gold layers from the inside to the outside, and a gas sensitive film 3 (the Cu x+ -PPy-rGO), leads 4 and 5 are connected to the interdigital electrodes 2 respectively.

[0022] Figure 2 The PPy-rGO in Example 1 and the Cu in Example 1 x+ -X-ray diffraction curve of PPy-rGO.

[0023] Figure 3 is Cu in Example 1 x+ -TEM image of PPy-rGO.

[0024] Figure 4 The PPy-rGO in Example 1 and the Cu in Example 1 x+ -X-ray photoelectron spectrum of N 1s of PPy-rGO.

[0025] Figure 5 is Cu in Example 1 x+ X-ray photoelectron spectroscopy of Cu 2p of PPy-rGO.

[0026] Figure 6 The Cu-based x+ Dynamic response recovery curves of the DMMP sensor of -PPy-rGO to different concentrations of DMMP at room temperature.

[0027] Figure 7 The Cu-based x+ Repeatability curve of the DMMP sensor of -PPy-rGO to 50 ppm DMMP at room temperature.

[0028] Figure 8 The Cu-based x+ Response recovery curve of DMMP sensor of -PPy-rGO to 100 ppm DMMP at room temperature.

[0029] Fig. 9 The Cu-based x+ Response recovery curve of DMMP sensor of -PPy-rGO to 100 ppm DMMP at room temperature.

[0030] Example 1 Preparation of Cu x+ -X-ray diffraction pattern of PPy-rGO Figure 2 As shown, Cu x+ -PPy-rGO composites exhibited the same characteristic diffraction peaks as those of PPy-rGO, and no diffraction peaks related to metallic Cu or CuO were found, proving that Cu ions were successfully introduced into the PPy-rGO composites.

[0031] Example 1 Preparation of Cu x+ - TEM images of PPy-rGO Figure 3 As shown, it can be seen that Cu x+ -PPy-rGO composites have a typical thin nanosheet morphology. No obvious particles and clusters related to Cu species were observed in the images, further proving that Cu ions were dispersedly introduced into the PPy-rGO composites.

[0032] Example 1 Preparation of Cu x+ The X-ray photoelectron spectroscopy peaks of N 1s of PPy-rGO composites are as follows: Figure 4 As shown by Figure 4 It can be seen that compared with the PPy-rGO composite material, Cu x+ The N 1s spectrum in the -PPy-rGO composite material shifted by 0.15 eV toward the low binding energy direction, and a characteristic peak of the Cu-N bond (398.7 eV) appeared, confirming the coordination between Cu ions and N atoms.

[0033] Example 1 Preparation of Cu x+ The X-ray photoelectron spectroscopy peaks of Cu 2p of PPy-rGO composites are as follows Figure 5 As shown in the figure, the introduction of Cu ions is confirmed. The two characteristic peaks at 934.6 eV and 954.4 eV are attributed to Cu 2+ , while the two characteristic peaks at 932.6 eV and 952.4 eV are attributed to Cu + , Cu + The appearance of further confirmed that in Cu x+ -Formation of Cu-N coordination structure in PPy-rGO composites.

[0034] Example 1 Preparation based on Cu x+The dynamic resistance response curve of the DMMP gas sensor of the PPy-rGO composite material to 2-100 ppm DMMP at room temperature is shown in Figure 6 It can be seen that the prepared Cu x+ -PPy-rGO-based DMMP sensor can detect DMMP gas as low as 2 ppm. With the increase of DMMP concentration, the response of the sensor gradually increases. At the same time, the sensor has fast response and recovery characteristics to different concentrations of DMMP.

[0035] Example 1 Preparation based on Cu x+ The response repeatability curve of the DMMP gas sensor based on the PPy-rGO composite material to 50 ppm DMMP at room temperature is shown in Figure 7 It can be seen that based on Cu x+ The -PPy-rGO sensor showed stable and repetitive responses upon repeated exposure to 50 ppm DMMP, indicating that the sensor has excellent reproducibility.

[0036] Example 1 Preparation based on Cu x+ The response recovery transient curve of the DMMP gas sensor of the PPy-rGO composite material to 100 ppm DMMP at room temperature is shown in Figure 8 As shown, it can be seen that the sensor has fast response and recovery characteristics to DMMP.

[0037] Example 2 Preparation of Cu-based x+ The response recovery transient curve of the DMMP gas sensor of the PPy-rGO composite material to 100 ppm DMMP at room temperature is shown in Fig. 9 As shown, it can be seen that the sensor has fast response and recovery characteristics to DMMP. DETAILED DESCRIPTION

[0038] The present invention is further described below with reference to the accompanying drawings and embodiments.

[0039] Example 1

[0040] (1) Add 1.0 mL of graphene oxide (GO) aqueous solution (1 mg / mL) into 20 mL of water and stir at room temperature for 0.5 h to obtain a GO dispersion.

[0041] (2) Add 1.0 mL of pyrrole (Py) to the GO dispersion obtained in step (1) and stir at room temperature for 6 h to obtain a mixed solution of GO and Py;

[0042] (3) The mixed solution of GO and Py obtained in step (2) was transferred into a hydrothermal reactor and treated at 180°C for 12 hours;

[0043] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0044] (5) Add 20 mL of copper chloride aqueous solution (50 mM) to 2.0 mg of PPy-rGO powder obtained in step (4) and stir at room temperature for 2 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+ -PPy-rGO materials.

[0045] (6) A flexible PET substrate is used, and the length, width and thickness of the PET are 10 mm, 5 mm and 150 mm respectively. Ten pairs of interdigital electrodes with a metal layer structure are deposited on the upper surface of the PET substrate by sputtering etching process. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and the thicknesses are 10 μm, 4 μm and 1 μm respectively. The line width of the interdigital electrodes is 100 μm and the line spacing is 100 μm.

[0046] (7) ultrasonically cleaning the flexible PET interdigital electrode obtained in step (1) with ethanol and water in sequence and drying;

[0047] (8) Cu x+ -PPy-rGO powder was dispersed in water at a concentration of 2 mg / mL; the solution was drop-coated on the surface of the flexible PET interdigital electrode dried in step (2), and then heat-treated under an infrared lamp for 6 hours to obtain a Cu-based x+ -PPy-rGO room-temperature DMMP sensor with a film thickness of 10 μm.

[0048] Example 2

[0049] (1) Add 1.0 mL of graphene oxide (GO) aqueous solution (1 mg / mL) into 20 mL of water and stir at room temperature for 0.5 h to obtain a GO dispersion.

[0050] (2) Add 1.0 mL of pyrrole (Py) to the GO dispersion obtained in step (1), and stir at room temperature for 8 h to obtain a mixed solution of GO and Py;

[0051] (3) The mixed solution of GO and Py obtained in step (2) was transferred into a hydrothermal reactor and treated at 180°C for 24 hours;

[0052] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0053] (5) Add 2.0 mg of PPy-rGO powder obtained in step (4) to 20 mL of copper chloride aqueous solution (100 mM) and stir at room temperature for 2 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+ -PPy-rGO materials.

[0054] (6) A flexible PET substrate is used, and the length, width and thickness of the PET are 10 mm, 5 mm and 200 mm respectively. Ten pairs of interdigital electrodes with a metal layer structure are deposited on the upper surface of the PET substrate by sputtering etching process. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and the thicknesses are 10 μm, 4 μm and 1 μm respectively. The line width of the interdigital electrodes is 100 μm and the line spacing is 100 μm.

[0055] (7) ultrasonically cleaning the flexible PET interdigital electrode obtained in step (1) with ethanol and water in sequence and drying;

[0056] (8) Cu x+ -PPy-rGO powder was dispersed in water at a concentration of 2 mg / mL; the solution was drop-coated on the surface of the flexible PET interdigital electrode dried in step (2), and then heat-treated under an infrared lamp for 8 hours to obtain a Cu-based x+ -PPy-rGO room-temperature DMMP sensor with a film thickness of 30 μm.

[0057] Example 3

[0058] (1) Add 3 mL of graphene oxide (GO) aqueous solution (3 mg / mL) into 30 mL of water and stir at room temperature for 0.5 h to obtain a GO dispersion.

[0059] (2) Add 2 mL of pyrrole (Py) to the GO dispersion obtained in step (1) and stir at room temperature for 10 h to obtain a mixed solution of GO and Py;

[0060] (3) The mixed solution of GO and Py obtained in step (2) was transferred into a hydrothermal reactor and treated at 200°C for 24 hours;

[0061] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0062] (5) Add 3 mg of PPy-rGO powder obtained in step (4) to 25 mL of copper chloride aqueous solution (75 mM) and stir at room temperature for 3 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+-PPy-rGO materials.

[0063] (6) A flexible PET substrate is used, and the length, width and thickness of the PET are 11 mm, 7 mm and 180 mm. A sputtering etching process is used to evaporate 15 pairs of interdigital electrodes with a metal layer structure on the upper surface of the PET substrate. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and their thicknesses are 13 μm, 5 μm and 2 μm respectively. The line width of the interdigital electrodes is 200 μm and the line spacing is 100 μm.

[0064] (7) ultrasonically cleaning the flexible PET interdigital electrode obtained in step (1) with ethanol and water in sequence and drying;

[0065] (8) Cu x+ -PPy-rGO powder was dispersed in water at a concentration of 5 mg / mL; the solution was drop-coated on the surface of the flexible PET interdigital electrode dried in step (2), and then heat-treated under an infrared lamp for 10 hours to obtain a Cu-based x+ -PPy-rGO room-temperature DMMP sensor with a film thickness of 30 μm.

[0066] Example 4

[0067] (1) Add 3 mL of graphene oxide (GO) aqueous solution (3 mg / mL) into 30 mL of water and stir at room temperature for 2 h to obtain a GO dispersion.

[0068] (2) Add 2 mL of pyrrole (Py) to the GO dispersion obtained in step (1), and stir at room temperature for 12 h to obtain a mixed solution of GO and Py;

[0069] (3) The mixed solution of GO and Py obtained in step (2) was transferred into a hydrothermal reactor and treated at 200°C for 36 hours;

[0070] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0071] (5) Add 4 mg of PPy-rGO powder obtained in step (4) to 25 mL of copper chloride aqueous solution (75 mM) and stir at room temperature for 3 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+ -PPy-rGO materials.

[0072] (6) A flexible PET substrate is used, and the length, width and thickness of the PET are 11 mm, 7 mm and 200 mm. A sputtering etching process is used to evaporate 15 pairs of interdigital electrodes with a metal layer structure on the upper surface of the PET substrate. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and their thicknesses are 13 μm, 6 μm and 2 μm respectively. The line width of the interdigital electrodes is 300 μm and the line spacing is 100 μm.

[0073] (7) ultrasonically cleaning the flexible PET interdigital electrode obtained in step (1) with ethanol and water in sequence and drying;

[0074] (8) Cu x+ -PPy-rGO powder was dispersed in water at a concentration of 5 mg / mL; the solution was drop-coated on the surface of the flexible PET interdigital electrode dried in step (2), and then heat-treated under an infrared lamp for 12 hours to obtain a Cu-based x+ -PPy-rGO room-temperature DMMP sensor with a film thickness of 30 μm.

[0075] Example 5

[0076] (1) Add 5.0 mL of graphene oxide (GO) aqueous solution (5 mg / mL) into 30 mL of water and stir at room temperature for 2 h to obtain a GO dispersion.

[0077] (2) Add 3 mL of pyrrole (Py) to the GO dispersion obtained in step (1) and stir at room temperature for 12 h to obtain a mixed solution of GO and Py;

[0078] (3) The mixed solution of GO and Py obtained in step (2) was transferred into a hydrothermal reactor and treated at 200°C for 36 hours;

[0079] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0080] (5) Add 5 mg of PPy-rGO powder obtained in step (4) to 30 mL of copper chloride aqueous solution (50 mM) and stir at room temperature for 2 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+ -PPy-rGO materials.

[0081] (6) A flexible PET substrate is used, and the length, width and thickness of the PET are 12 mm, 7 mm and 200 mm. A sputtering etching process is used to evaporate 20 pairs of interdigital electrodes with a metal layer structure on the upper surface of the PET substrate. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and their thicknesses are 13 μm, 6 μm and 3 μm respectively. The line width of the interdigital electrodes is 300 μm and the line spacing is 200 μm.

[0082] (7) ultrasonically cleaning the flexible PET interdigital electrode obtained in step (1) with ethanol and water in sequence and drying;

[0083] (8) Cu x+ -PPy-rGO powder was dispersed in water at a concentration of 10 mg / mL; the solution was drop-coated on the surface of the flexible PET interdigital electrode dried in step (2), and then heat-treated under an infrared lamp for 10 hours to obtain a Cu-based x+ -PPy-rGO room-temperature DMMP sensor with a film thickness of 50 μm.

[0084] Example 6

[0085] (1) Add 5.0 mL of graphene oxide (GO) aqueous solution (5 mg / mL) into 50 mL of water and stir at room temperature for 2 h to obtain a GO dispersion.

[0086] (2) Add 1.0 mL of pyrrole (Py) to the GO dispersion obtained in step (1) and stir at room temperature for 6 h to obtain a mixed solution of GO and Py;

[0087] (3) The mixed solution of GO and Py obtained in step (2) was transferred into a hydrothermal reactor and treated at 220°C for 24 hours;

[0088] (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the obtained solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide (PPy-rGO) powder;

[0089] (5) Add 5 mg of PPy-rGO powder obtained in step (4) to 30 mL of copper chloride aqueous solution (50 mM) and stir at room temperature for 3 h; centrifuge the resulting solution, wash the separated product with ethanol, and dry it to obtain Cu x+ -PPy-rGO materials.

[0090] (6) A flexible PET substrate is used, and the length, width and thickness of the PET are 12 mm, 7 mm and 200 mm. A sputtering etching process is used to evaporate 20 pairs of interdigital electrodes with a metal layer structure on the upper surface of the PET substrate. The metal layer structure is copper, nickel and gold layers from the inside to the outside, and their thicknesses are 15 μm, 6 μm and 3 μm respectively. The line width of the interdigital electrodes is 300 μm and the line spacing is 300 μm.

[0091] (7) ultrasonically cleaning the flexible PET interdigital electrode obtained in step (1) with ethanol and water in sequence and drying;

[0092] (8) Cu x+ -PPy-rGO powder was dispersed in water at a concentration of 10 mg / mL; the solution was drop-coated on the surface of the flexible PET interdigital electrode dried in step (2), and then heat-treated under an infrared lamp for 12 hours to obtain a Cu-based x+ -PPy-rGO room-temperature DMMP sensor with a film thickness of 50 μm.

Claims

1. A room temperature DMMP sensor based on copper ion modified polypyrrole / reduced graphene oxide, which is a planar structure, and consists of a flexible polyethylene terephthalate substrate, an interdigital electrode with a metal layer structure printed on the polyethylene terephthalate substrate, and a gas sensitive film coated on the interdigital electrode; characterized in that: The gas sensitive film material is copper ion modified polypyrrole / reduced graphene oxide, and is prepared by the following steps: (1) adding 1.0-5.0 mL of a 1-5 mg / mL graphene oxide aqueous solution to 20-50 mL of water, stirring at room temperature for 0.5-2 h to obtain a graphene oxide dispersion; (2) adding 1.0 to 3.0 mL of pyrrole to the dispersion of graphene oxide obtained in step (1), stirring at room temperature for 6 to 12 hours to obtain a mixed solution of graphene oxide and pyrrole; (3) transferring the mixed solution of graphene oxide and pyrrole obtained in step (2) into a hydrothermal reactor and treating at 180 to 220° C. for 12 to 36 hours; (4) cooling the solution in the hydrothermal reactor of step (3) to room temperature, centrifuging the resulting solution, washing the separated product with ethanol and water, and drying to obtain black polypyrrole / reduced graphene oxide powder; (5) adding 2.0-5.0 mg of the polypyrrole / reduced graphene oxide powder obtained in step (4) to 20-30 mL of a 50-100 mM copper chloride aqueous solution, and stirring at room temperature for 2-3 h; centrifuging the resulting solution, washing the separated product with ethanol, and drying to obtain copper ion-modified polypyrrole / reduced graphene oxide, denoted as Cu x+ -PPy-rGO; DMMP is dimethyl methylphosphonate.

2. The method for preparing a room temperature DMMP sensor based on copper ion modified polypyrrole / reduced graphene oxide according to claim 1, wherein the steps are as follows: (1) Using a flexible polyethylene terephthalate substrate as a substrate, 10 to 20 pairs of interdigital electrodes having a metal layer structure are deposited on the upper surface of the substrate by a sputtering etching process, wherein the metal layer structure is copper, nickel and gold layers from the inside to the outside; (2) ultrasonically cleaning the substrate and interdigital electrodes obtained in step (1) with ethanol and water in sequence and drying them; (3) Cu x+ -PPy-rGO powder is dispersed in water at a concentration of 2 to 10 mg / mL; the solution is drop-coated on the substrate and the surface of the interdigital electrode after drying in step (2), and then heat-treated under an infrared lamp for 6 to 12 hours to obtain a Cu-based x+ Room temperature DMMP sensor based on PPy-rGO, Cu x+ -The thickness of PPy-rGO film is 10 to 50 μm.

3. A method for preparing a room temperature DMMP sensor based on copper ion modified polypyrrole / reduced graphene oxide as claimed in claim 2, characterized in that: The flexible polyethylene terephthalate substrate has a length of 10 to 12 mm, a width of 5 to 7 mm, and a thickness of 150 to 200 mm.

4. A method for preparing a room temperature DMMP sensor based on copper ion modified polypyrrole / reduced graphene oxide as claimed in claim 2, characterized in that: The thicknesses of the copper, nickel and gold layers are 10-15 μm, 4-6 μm and 1-3 μm respectively; the line width of the interdigital electrodes is 100-300 μm, and the line spacing is 100-300 μm.