Fiber-reinforced polyurethane composite material and preparation method and application thereof

Through fiber-reinforced polyurethane composite materials, the problems of high loss and poor durability of traditional Chinese medicines in natural wood anticorrosion treatment are solved, high strength, low water absorption and good thermal insulation performance are achieved, and energy-saving and environmentally friendly requirements are met. It is suitable for multiple A kind of application scenario.

CN115197451BActive Publication Date: 2024-11-01CHONGQING ODEON IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210804414.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-08
Publication Date
2024-11-01
Estimated Expiration
2042-07-08

AI Technical Summary

Technical Problem

The existing natural wood anticorrosion treatments have problems such as high chemical loss, poor durability and low environmental performance, which are difficult to meet the requirements of energy conservation and environmental protection.

Method used

Using fiber-reinforced polyurethane composite material, a material with a density of 501~900Kg/m3 is formed by combining rigid polyurethane foam and reinforced fibers, with low water absorption, excellent mechanical properties, good thermal insulation, acid and alkali resistance, corrosion and moisture resistance Capability and high dimensional stability.

Benefits of technology

It realizes the high strength, high density, low water absorption, good thermal insulation and durability of the material, completely replaces the performance of natural wood, and has excellent environmental protection performance and high production efficiency. It is suitable for doors, windows, decorative panels and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115197451B_ABST
    Figure CN115197451B_ABST
Patent Text Reader

Abstract

The present invention relates to a fiber-reinforced polyurethane composite material, characterized in that the composite material contains rigid polyurethane foam and reinforcing fibers, and the material density is 501-900 kg / m 3 The composite material has a water absorption rate of ≤3%, a Shore hardness of ≥80HA, a bending strength of ≥60Mpa, a shear strength of ≥15Mpa, a dimensional stability of ≤1%, no change in appearance after being soaked in acid or alkali for 30 days, a thermal conductivity of ≤0.08W / (m·K), and a linear thermal expansion coefficient (1 / ℃) of ≤1.0×10 ‑5 The composite material has high strength and density, excellent mechanical properties (shear resistance, compression resistance, etc.), as well as good thermal insulation, acid and alkali resistance, corrosion resistance, moisture resistance, and dimensional stability. The composite material can be used in doors and windows, door and window reinforcement materials, installation frames, indoor and outdoor decorative panels, and pedestrian walkways.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite materials, and in particular to a fiber-reinforced polyurethane composite material, a preparation method and application thereof. Background Art

[0002] Natural wood is widely used in various aspects such as construction, furniture, and outdoor products due to its ecological and environmental protection, suitable elasticity and hardness, and good performance. Considering the poor natural antiseptic properties of fast-growing wood, it is usually treated with antiseptic treatment before use. No matter what kind of antiseptic impregnation treatment method is used for this type of antiseptic wood, the preservative enters the wood from the outside. Therefore, the preservative loading of the outer layer of the antiseptic wood is the highest. The lower the preservative loading is, the higher the preservative loading is for wood with a high drug loading of preservatives. Therefore, the antiseptic wood impregnated with the preservative solution will be affected by frequent temperature changes, ultraviolet radiation, and atmospheric humidity as the use time increases, which will have a rapid destructive effect on the antiseptic wood. The preservative in the outer layer in contact with the environment will gradually be lost, and its durability will gradually decrease, such as water absorption deformation, cracking, mildew, insect bites, rot, etc. The duration of the durability of the antiseptic wood is difficult to meet the use requirements of actual projects. If it needs to be maintained or replaced, a large amount of wood will be consumed, which will cause long-term damage to forest resources and also require a large number of maintenance personnel.

[0003] The proposal of carbon neutrality and carbon peak has put forward higher requirements for energy conservation and environmental protection. Therefore, it has become an urgent task to find a new material that is low-cost, has mechanical properties comparable to or even higher than solid wood, has higher corrosion and moisture resistance than existing anti-corrosion wood, and is safe, non-toxic and environmentally friendly. Summary of the invention

[0004] The present invention aims to provide a fiber-reinforced polyurethane composite material with low water absorption, good mechanical properties, acid and alkali corrosion resistance and high dimensional stability.

[0005] To achieve the above object, the present invention adopts the following technical scheme: a fiber-reinforced polyurethane composite material, the composite material contains rigid polyurethane foam and reinforcing fibers, and the material density is 501-900Kg / m 3 The composite material has a water absorption rate of ≤3%, a Shore hardness of ≥80HA, a bending strength of ≥60Mpa, a shear strength of ≥15Mpa, a dimensional stability of ≤1%, no change in appearance after being soaked in acid or alkali for 30 days, a thermal conductivity of ≤0.08W / (m·K), and a linear thermal expansion coefficient (1 / ℃) of ≤1.0×10 -5 .

[0006] The advantages of this composite material are:

[0007] (1) In terms of material density, the density of the composite material is 501-900 kg / m 3 , can be processed by cutting, sawing, planing, etc.; in terms of water absorption, the water absorption rate of composite materials is ≤3%, which is lower than that of solid wood materials and has better performance;

[0008] (2) In terms of thermal insulation, the thermal conductivity of the composite material is ≤0.08W / (m·K), and the thermal conductivity is low; compared with natural dry solid wood (thermal conductivity ≥0.08W / (m·K)), it has higher thermal insulation performance and can be used in materials with high thermal insulation requirements (such as doors, windows, and car filling materials, etc.);

[0009] (3) The mechanical properties of this composite material are greatly improved compared with natural wood (or natural wood that has been treated with antiseptics, i.e., antiseptic wood). Its shear and bending resistance are higher than that of natural wood, and its hardness is also higher than that of natural solid wood. It is light and strong, and will not lose its mechanical properties even if exposed to the air for a long time. Therefore, it can completely replace natural wood (antiseptic wood) on the market in terms of performance, and is widely used in doors and windows, door and window reinforcement materials, installation of auxiliary frames, indoor and outdoor decorative panels, and pedestrian walkways.

[0010] Compared with natural wood, which requires a certain growth cycle and antiseptic wood, this composite material can be quickly produced in the factory, with higher production efficiency and more cost-effectiveness.

[0011] Moreover, during the production process of this composite material, all chemical raw materials undergo sufficient reaction, and there is no toxic residue. The environmental protection level reaches E0, while the highest antiseptic wood on the market is only E1, and its environmental protection performance is more superior.

[0012] (4) In terms of acid and alkali resistance, corrosion resistance and moisture resistance, natural wood contains cellulose, gum, etc. These plant polysaccharides are water-soluble and easily decomposed and rotted by mold and bacteria in the environment. They have excellent acid and alkali resistance, corrosion resistance and moisture resistance. In this composite material, the chemical bonds formed by the chemical reaction of rigid polyurethane foam are very stable in the environment, not easy to hydrolyze and difficult to be decomposed by bacteria and mold in the environment. There is no change in appearance after being soaked in acid or alkali for 30 days.

[0013] (5) In terms of dimensional stability, the linear thermal expansion coefficient (1 / ℃) of the composite material is ≤1.0×10 -5 , low deformation rate, can remain stable when extreme temperature changes, and has strong resistance to cracking.

[0014] In summary, this composite material has high strength and density, excellent mechanical properties (shear resistance, compression resistance, etc.), as well as good thermal insulation, acid and alkali resistance, corrosion resistance, moisture resistance, and dimensional stability.

[0015] Furthermore, the density of the rigid polyurethane foam is 300-450 Kg / m 3 , the density of the reinforcing fiber ranges from 1 to 2.7 g / cm 3 ; The mass ratio of the rigid polyurethane foam to the reinforcing fiber is 1:1 to 4:1.

[0016] When non-combustible fibers are selected as reinforcing fibers, the fiber percentage can be obtained by burning the composite material specimen and then calculating according to GB / T 2577-2005 Glass Fiber Reinforced Plastic Numerical Content Test Method.

[0017] The inventors found that due to the high density of the reinforcing fiber, if the proportion of the total mass of the composite material is less than 20%, the dimensional adsorption polyurethane mixed liquid (such as the maximum resin adsorption of each fiber is 120% of its own mass) is not enough to fill the product cavity during the foaming process, which will form gaps and holes and affect the quality of the product. However, if the proportion of the total mass of the composite material exceeds 50%, it will affect the lightweight effect of the composite material. Therefore, the proportion of reinforcing fiber in the composite material is 20% to 50%, which is a relatively ideal content, which can not only improve the quality of the finished product but also does not affect the lightweight effect of the finished product.

[0018] Furthermore, the nail holding force of the composite material is ≥800N, which is higher than that of natural wood. After the nail enters the board, the nail hole is easily fixed and is not easy to loosen and fall off. The nail hole can be reused, and vice versa.

[0019] Furthermore, the reinforcing fiber is one or a mixture of continuous glass fiber, glass fiber mat, bamboo fiber, polymer fiber, etc., and different fibers are selected: continuous glass fiber (density 2.6g / cm 3 ), continuous glass fiber mat (density 2.6g / cm 3 ), bamboo fiber (1.49g / cm 3 ), chemical fiber (common such as PP / PET spinning fiber density 1.0~1.2g / cm 3 ), according to different fiber density and design dosage, the composite material maintains high strength through formula design.

[0020] Furthermore, the raw materials of the rigid polyurethane foam include material A and material B, and the mass ratio of material A to material B is 1:0.9 to 1:1.2.

[0021] The polyurethane foam produced with this ratio has good performance in thermal insulation, acid and alkali resistance, corrosion resistance, moisture resistance, and dimensional stability.

[0022] Furthermore, the B material is isocyanate or modified isocyanate, and the A material includes the following raw materials in parts by weight:

[0023] 100 parts of combined polyether;

[0024] 0.5-1.5 parts of catalyst;

[0025] 1.0 to 3 parts of surfactant;

[0026] 0.3-0.6 parts of foaming agent.

[0027] The modified isocyanate used in material B is a product obtained through the chemical reaction of isocyanate. Through the above ratio, material A can ensure that the polyurethane rising time is ≥3min, and the density of rigid polyurethane foam after foaming is 300~450Kg / m 3 .

[0028] Furthermore, the composite polyether is prepared by propylene oxide end-capping polymerization with polyol and / or polyamine as initiator and propylene oxide as polymerization monomer, and has a hydroxyl value of 30 to 500 mg·KOH / g, an average functionality of 2 to 6 (preferably 3 to 4.5), and a number average molecular weight of 200 to 4800 (preferably 400 to 3000).

[0029] The initiator may be selected to include one or more of glycerol, triethanolamine, pentaerythritol, diethylene glycol, sorbitol and sucrose, preferably one or more of pentaerythritol, diethylene glycol, sorbitol and sucrose;

[0030] The average functionality of the combined polyether is greater than 2, which can improve the crosslinking degree, hardness and strength of the composite material, as well as the chemical dissolution / corrosion resistance. However, the greater the functionality of the polyether, the greater the viscosity and the poorer the fluidity, so it is controlled below 6.

[0031] Furthermore, the isocyanate or modified isocyanate is aliphatic, alicyclic, araliphatic, aromatic isocyanate or a combination thereof.

[0032] The aliphatic isocyanate may be an alkylene diisocyanate, in particular an alkylene diisocyanate containing 4 to 12 carbon atoms in the alkylene group, such as 1,12-dodecane diisocyanate, 2-ethyltetramethylene-1,4-diisocyanate, 2-methyl-pentamethylene-1,5-diisocyanate, 2-ethyl-2-butylpentamethylene-1,5-diisocyanate, tetramethylene-1,4-diisocyanate and hexamethylene-1,6-diisocyanate;

[0033] Alicyclic isocyanates may include cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, 1-isocyanate-3,3,5-trimethyl-5-isocyanato-methylcyclohexane (isophorone diisocyanate), 2,4-hexahydrotoluene diisocyanate, 2,6-hexahydrotoluene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 2,2'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate, etc.

[0034] Aromatic isocyanates may be selected from diphenylmethane diisocyanate (such as 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate), polymethylene polyphenyl isocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.

[0035] The aromatic aliphatic isocyanate may be xylylene diisocyanate (such as m-xylylene diisocyanate, p-xylylene diisocyanate), etc. These isocyanates may be used alone or in combination.

[0036] Furthermore, the catalyst is mainly a heat-sensitive delayed catalyst. Before the environment reaches the catalyst deblocking temperature (50°C to 60°C), its catalytic effect is weak and the polyurethane chemical reaction is relatively slow, which can ensure that the polyurethane and the reinforcing fibers are fully infiltrated before the curing reaction.

[0037] Select a thermosensitive delayed catalyst, specifically one or more of an amine catalyst, an organic bismuth / organic tin catalyst, and a trimerization catalyst with a thermosensitive group. The thermosensitive catalyst includes a class of nitrogen element compounds, organic metal compounds, etc. with thermosensitive groups such as nitrogen heterocyclic carbenes, quaternary ammonium salts, aldimines, and phenol sulfonates as trimerization catalysts for aliphatic and aromatic isocyanates. The characteristic of this type of catalyst is that under the heating conditions of the system, the active center protected by the thermosensitive group separates to form an activation center, activates the -NCO and -OH groups, and catalyzes the polyurethane gel reaction. This thermosensitive catalyst can effectively delay the reaction time of the system, ensure the sufficient infiltration time of the polyurethane raw materials and continuous fibers in the early stage (generally requiring 4 to 10 minutes), and can quickly react and cure after entering the plate chain line in the later stage (ensuring that the curing completion time is 25 to 40 minutes). For example, the formate of 2-hydroxy-N,N,N-trimethyl-1-propylamine, N,N',N"-tris(dimethylaminopropyl)-hexahydrotriazine, and 2,4,6-tris(dimethylaminomethyl)phenol are commonly used tertiary amine trimerization catalysts.

[0038] Furthermore, the foaming agent is water. The traditional use of small molecule hydrocarbons such as Freon and cyclopentane as foaming agents will produce substances such as fluorine that are highly harmful to the environment, while using water as a foaming agent is more environmentally friendly.

[0039] Furthermore, a flame retardant with a flame retardancy level of B1 or above is added to the composite material (according to the standard classification of "GB·8624-2012 Classification of Combustion Performance of Building Materials and Products"), and the mass ratio of the composite material to the flame retardant is 10:1 to 10:4. The flame retardant does not chemically react with the A material, the B material and the reinforcing fiber, and the produced material is used in places with a high flame retardancy level such as door and window filling materials, installation of auxiliary frames, indoor and outdoor decorative panels and pedestrian walkways.

[0040] Furthermore, since organic flame retardants release toxic gases when burned (for example, halogen-containing flame retardants generally release toxic and harmful gases such as HCl, HBr, etc.), the flame retardant of the present invention selects inorganic filler flame retardants, which is more environmentally friendly.

[0041] Furthermore, the inorganic filler flame retardant is one or a mixture of phosphorus-based, nitrogen-based, expanded graphite, magnesium hydroxide, and montmorillonite.

[0042] For example, the halogen-free phosphorus filler halogen includes, but is not limited to, one or more of tris(2-chloropropyl) phosphate (TCPP), tris(2-chloroethyl) phosphate (TCEP), tris(2,3-dichloropropyl) phosphate (TDCP), tetrakis(2-chloroethyl) diethylene ether diphosphate, tetrakis(2-chloroethyl) ethylene diphosphate and tetrakis(2-chloroethyl)-2,2-dichloromethyl-1,3-propylene diphosphate, and the addition amount is preferably 5 to 20 parts by mass.

[0043] The flame retardant also includes expanded graphite, preferably natural crystalline graphite that can expand into a worm-like shape instantly after special treatment and high temperature. The expanded graphite is prepared by a procedure known in the art and usually the graphite is first modified with an oxidant such as nitrate, chromate, peroxide, or the crystal layer is opened by electrolysis, and then nitrate or sulfate is inserted into the graphite; the expanded graphite can be selected from expandable graphite with an expansion ratio of 100 to 400 ml / g, a mesh size between 32 mesh and 325 mesh, a pH value of 4 to 7, and a moisture content of no more than 1wt%, preferably 80 to 250 mesh expandable graphite, and preferably added in an amount of 5 to 15 parts by mass.

[0044] The present invention also discloses a method for preparing a fiber-reinforced polyurethane composite material, comprising the steps of yarn rack arrangement, glue injection, impregnation, curing and cutting. In the impregnation step, the glue dipping tool adopts a semi-closed vibration glue dipping method. First, the polyurethane high-pressure glue injection machine evenly sprays the polyurethane raw material on the fiber surface, and then the reinforcing fiber and the polyurethane raw material are evenly impregnated by the left and right continuous vibration and extrusion of the tool.

[0045] The glass fiber is mainly distributed longitudinally parallel to the continuous traction direction of the plate chain line (similar to the longitudinal grain of a tree); in addition, due to the left and right lateral movement of the self-made impregnation tooling, the continuous fiber is partially angled or perpendicular to the continuous traction direction of the plate chain line, and partially distributed transversely. There are also a large number of disordered long fibers in the glass fiber. Under the vibration and extrusion of the impregnation tooling, some fibers are randomly distributed at angles along the traction direction (similar to the transverse grain in wood). It is this combination of mainly longitudinal grains and partially disordered angular distribution of transverse grains that creates a unique solid wood texture.

[0046] The present invention controls the yarn arrangement and impregnation steps to uniformly mix the fiber and the polyurethane raw material, and the performance of the product is uniform and consistent, thereby realizing the standardization and scale of the production of the composite material. In particular, through a semi-closed vibration impregnation method, the fiber is distributed in the polyurethane in a certain regularity, forming a shape close to the texture of natural wood.

[0047] The invention also discloses an application of a fiber-reinforced polyurethane composite material, wherein the composite material is applied to door and window filling materials, installation auxiliary frames, indoor and outdoor decorative plates and pedestrian walkways. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 is a process flow chart of the present invention;

[0049] Figure 2 for Figure 1 Structure diagram of mid-infiltration tooling;

[0050] The numbers in the accompanying drawings are: A material barrel 1, B material barrel 2, polyurethane glue injection machine 3, yarn rack 4, impregnation tooling 5, impregnation tank 51, eccentric mechanism 52, vibration frame 53, oscillator 54, laminator 6, cutting machine 7. DETAILED DESCRIPTION

[0051] The following is a further detailed description through specific implementation methods:

[0052] The ingredients and preparation method of the fiber reinforced polyurethane composite material are as follows:

[0053] 1. Raw material preparation

[0054] (1) Material A

[0055] The composition is composed of 100 parts of combined polyether, 1.5 parts of catalyst, 3 parts of surfactant and 0.5 parts of foaming agent.

[0056] (1) Combined polyether

[0057] The average hydroxyl value of the combined polyether is 328, and the average functionality is 3.85, wherein the mass proportions of polyether polyol Ⅰa: polyether polyol Ⅰb: polyether polyol Ⅰc are 25 parts, 50 parts, and 25 parts respectively.

[0058] Wherein: (1) Polyether polyol Ia: using glycerol as the initiator, propylene oxide ring-opening polymerization, propylene oxide end-capping, number average molecular weight 2000; (2) Polyether polyol Ib: using a mixture of sucrose and diethylene glycol with a molar ratio of 3.7:6.3 as the initiator, propylene oxide ring-opening polymerization, propylene oxide end-capping, number average molecular weight 550; (3) Polyether polyol Ic: using a mixture of sorbitol and toluenediamine as the initiator, propylene oxide ring-opening polymerization, functionality 4, number average molecular weight 600;

[0059] (2) Catalyst: 1 part of catalyst IVa: RM-301 produced by Guangzhou Yourun Synthetic Materials Co., Ltd. and 0.5 part of catalyst IVb: SA-1 produced by Beijing Intede Technology Co., Ltd.

[0060] (3) Surfactant: Surfactant IIa: B8870 from Evonik of Germany was selected.

[0061] (4) Foaming agent: Water is used as the foaming agent.

[0062] (II) Material B

[0063] Polymeric MDI (full name: polyphenylmethane diisocyanate and polymers thereof) is selected, and its NCO (isocyanate group) content is 32-32.5% and its average functionality is 2.5-2.8.

[0064] (III) Reinforcement Fiber

[0065] Select Tex9600 continuous glass fiber.

[0066] (IV) Flame retardant

[0067] Two flame retardants are selected and mixed: (1) flame retardant IIIa: tetrakis (2-chloroethyl) diethylene ether diphosphate; (2) flame retardant IIIb: expandable graphite 80 mesh. The mass fraction ratio of flame retardant IIIa to flame retardant IIIb is 1:1.

[0068] 2. Raw material preparation

[0069] Example 1-4: Prepare material A, material B, flame retardant and continuous glass fiber according to the formula in Table 1.

[0070] Raw material name (mass parts) Example 1 Example 2 Example 3 Example 4 Material A 100 100 100 100 B material 120 120 120 120 Continuous glass fiber 22 55 94.2 94.2 Flame retardants 44 44 44 0

[0071] 3. Material preparation

[0072] See also Figure 1 , Figure 2 As shown, in the infiltration tool 5, the upper end of the infiltration tank 51 is open, see Figure 1 The left end is wide and the right end is narrow. A vibration frame 53 is arranged across the infiltration tank 51 along the width direction of the infiltration tank 51. The vibration frame 53 is in the shape of a letter "∏". The vibration frame 53 is connected to the output end of the eccentric mechanism 52 and can perform horizontal and vertical reciprocating motions driven by the eccentric mechanism 52. An oscillator 54 is connected to the middle of the vibration frame 53 through a suspension rod, and the oscillator 54 can oscillate when started. The connection method of the overall production line is as follows: A material barrel 1 and B material barrel 2 are respectively connected to the feed port of the polyurethane glue injection machine 3, the discharge port of the polyurethane glue injection machine 3 is connected to the liquid inlet of the infiltration tooling 5, the yarn outlet end of the yarn frame 4 is opposite to the wide mouth of the infiltration tank 51 of the infiltration tooling 5, the narrow mouth of the infiltration tank 51 is connected to the feed port of the laminator 6, and the outlet of the laminator 6 is connected to the cutting machine 7

[0073] Prepare the test pieces of Example 1, Example 2, Example 3 and Example 4 according to the following steps:

[0074] 1. Yarn arrangement on creel

[0075] The required number of glass fibers is calculated according to the density of the glass fibers and the size of the composite material, and the continuous glass fibers are passed through the creel 4, evenly arranged according to the cross section of the product, and passed through the impregnation tooling 5 for continuous traction.

[0076] 2. Glue injection

[0077] Add material A and flame retardant into material barrel A 1 and mix evenly, add material B into material barrel B 2, and the raw materials in material barrel A 1 and material barrel B 2 enter into polyurethane injection machine 3 at injection pressures of 11.0-11.5MPa and 10.0-10.5MPa respectively for mixing.

[0078] The temperature of the polyurethane injection machine 3 is controlled at 20-30° C., which is not yet at the catalyst deblocking temperature of 50-60° C., so that the A material and the B material react slowly, and the flame retardant does not react chemically with the A material and the B material.

[0079] 3. Infiltration

[0080] The polyurethane glue injection machine 3 injects the mixed polyurethane raw material into the impregnation tank 51 of the impregnation tool 5, first sprays it evenly on the surface of the glass fiber in the impregnation tank 51, and then uses the left and right continuous vibration and extrusion of the vibration frame 53 (the vertical reciprocating motion of the vibration frame 53 will squeeze the glass fiber), and the oscillator 54 will also perform oscillation and knocking motion to evenly impregnate the glass fiber and the polyurethane raw material. From the injection to the impregnation link, the rise time of the polyurethane foam is ≥3min, which fully guarantees the impregnation effect.

[0081] The glass fibers are mainly distributed longitudinally parallel to the continuous traction direction (similar to the longitudinal grain of a tree); in addition, due to the left and right lateral movement of the self-made impregnation tooling 5, the continuous fibers are partially angled or perpendicular to the continuous traction direction, and partially distributed transversely. There are also a large number of disordered long fibers in the glass fibers. Under the vibration and extrusion of the impregnation tooling 5, some of the fibers are randomly distributed at angles along the traction direction (similar to the transverse grain in wood). It is this combination of mainly longitudinal grains and partially disordered angular distribution of transverse grains that creates a unique texture of solid wood.

[0082] 4. Curing and molding

[0083] The polyurethane fully impregnated with the glass fiber enters the laminator 6, and the temperature in the laminator 6 is controlled at 60°C, at which time the deblocking temperature of the catalyst is reached, and the A material and the B material are foamed and formed, and the curing time is ≤50min.

[0084] 5. Cutting

[0085] The cured polyurethane material is cut into polyurethane material specimens of equal size by a cutting machine 7. Finally, Example 1, Example 2, Example 3, and Example 4 are manufactured into Specimen 1, Specimen 2, Specimen 3, and Specimen 4, respectively.

[0086] 3. Experimental testing

[0087] Prepare pine wood blocks of the same size as the polyurethane material specimens, and conduct experimental tests on specimens 1, 2, 3, and pine wood. The results are as follows:

[0088]

[0089] From the test results, we can see that:

[0090] (1) Material density: The density of specimens 1, 2, 3 and 4 is 750 kg / m 3 , 801Kg / m 3 、855Kg / m 3 、654Kg / m 3 , both between 501 and 900 kg / m3 The density of pine wood is 410Kg / m 3 ,The density of the specimen is much higher than that of pine wood, and can be processed by cutting, sawing and planing.

[0091] (2) Bending strength, shear strength, and Shore hardness: The bending strengths of specimens 1, 2, 3, and 4 are 125 MPa, 136 MPa, 145 MPa, and 107 MPa, respectively, and the bending strength of pine wood is 55 MPa; the shear strengths of specimens 1, 2, 3, and 4 are 31 MPa, 37 MPa, 46 MPa, and 23 MPa, respectively, and the shear strength of pine wood is 7.5 MPa. The Shore hardnesses of specimens 1, 2, 3, and 4 are 88 HA, 90 HA, 92 HA, and 83 HA, respectively, and the hardness of pine wood is 60 HA.

[0092] It can be seen that the shear and bending resistance of this composite material are higher than those of natural wood, and its hardness is also higher than that of natural solid wood. It has the characteristics of high strength and will not lose its mechanical properties even if exposed to the air for a long time. Therefore, it can completely replace the natural wood (anticorrosive wood) on the market in terms of performance, and is widely used in frame materials, such as doors and windows, door and window reinforcement materials, installation of auxiliary frames, indoor and outdoor decorative panels, pedestrian walkways and other fields.

[0093] (3) Water absorption rate: The water absorption rates of specimens 1, 2, 3 and 4 were 1.9%, 1.7%, 1.5% and 2.3% respectively, while the water absorption rate of pine wood was 19.3%. The water absorption rate of composite materials is much lower than that of natural solid wood. It is not easy to absorb water and has better waterproof and moisture-proof performance.

[0094] (4) Thermal conductivity: The thermal conductivity of specimens 1, 2, 3, and 4 are 0.06 W / (m·K), 0.07 W / (m·K), 0.07 W / (m·K), and 0.09 W / (m·K), respectively. The thermal conductivity of pine wood is 0.08 W / (m·K). It can be seen that the thermal conductivity of the composite material is similar to that of pine wood (thermal insulation materials are generally 0.03 to 0.17 W / (m·K)). Its thermal insulation performance is close to that of natural solid wood.

[0095] (5) Dimensional stability and linear thermal expansion coefficient: The dimensional stability of specimens 1, 2, 3, and 4 is 0.9%, 0.8%, 0.7%, and 0.9%, respectively, and that of pine wood is 5.6%. The linear expansion coefficient of specimens 1, 2, 3, and 4 is 0.3×10 -5 (1 / ℃), 0.7×10 -5 (1 / ℃), 0.5×10 -5 (1 / ℃), 0.5×10 -5 (1 / ℃), pine wood is 7.9×10-5 (1 / ℃), it can be seen that compared with pine wood, the composite material has a lower linear expansion coefficient and higher dimensional stability, a low deformation rate, can remain stable during extreme temperature changes, and has strong crack resistance.

[0096] (2) Acid and alkali resistance: Specimens 1, 2, 3, 4, and pine were tested according to the method in the table above. The pine swelled slightly, became partially fluffy, and changed color. The appearance of the four specimens did not change. This shows that the composite material is very stable in the environment and has stronger acid and alkali resistance than natural solid wood.

[0097] (3) Nail holding strength: The nail holding strengths of specimens 1, 2, 3, and 4 are 878 N, 907 N, 955 N, and 842 N, respectively. The nail holding strength of pine wood is 498 N. The nail holding strength of composite materials is much greater than that of natural solid wood. After the nails enter the board, the nail holes are easily fixed and are not easy to loosen or fall off. The nail holes can be reused, and vice versa.

[0098] In summary, this composite material has medium density and high strength, strong mechanical properties (shear resistance, hardness, etc.), excellent thermal insulation, acid and alkali resistance, corrosion resistance and moisture resistance, as well as good dimensional stability. Compared with natural wood such as pine, it has more comprehensive performance and does not use chemical agents to enhance corrosion resistance. It is more environmentally friendly and non-toxic than antiseptic wood, and is more suitable for doors and windows, fillings, exterior decoration, etc.

[0099] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A fiber-reinforced polyurethane composite material, characterized in that: The composite material contains rigid polyurethane foam and reinforcing fibers, and the material density is 501-900 kg / m 3 , the mass ratio of the rigid polyurethane foam to the reinforcing fiber is 1:1 to 4:1; The composite material has a water absorption rate of ≤3%, a Shore hardness of ≥80HA, a bending strength of ≥60Mpa, a shear strength of ≥15Mpa, a dimensional stability of ≤1%, no change in appearance after being soaked in acid or alkali for 30 days, a thermal conductivity of ≤0.08W / (m·K), and a linear thermal expansion coefficient (1 / ℃) of ≤1.0×10 -5 , the nail holding force of the composite material is ≥800N; the reinforcing fiber is one or a mixture of continuous glass fiber, glass fiber mat, bamboo fiber, polymer fiber; the raw materials of the rigid polyurethane foam include material A and material B, and the mass ratio of material A to material B is 1:0.9 to 1:1.2; The B material is isocyanate or modified isocyanate, and the A material includes the following raw materials in parts by weight: 100 parts of combined polyether, 0.5-1.5 parts of catalyst, the catalyst is a heat-sensitive delayed catalyst, and its deblocking temperature is 50°C-60°C, 1.0-3 parts of surfactant, and 0.3-0.6 parts of foaming agent, which is water; The preparation method of the fiber-reinforced polyurethane composite material includes the steps of yarn rack arrangement, glue injection, impregnation, curing and molding, and cutting. From the glue injection to the impregnation link, the rise time of the polyurethane foam is ≥3 minutes. In the impregnation step, the glue dipping tool adopts a semi-closed vibration glue dipping method. First, the polyurethane high-pressure glue injection machine evenly sprays the polyurethane raw material on the fiber surface, and then the reinforcing fiber and the polyurethane raw material are evenly impregnated by the left and right continuous vibration and extrusion of the tool.

2. The fiber-reinforced polyurethane composite material according to claim 1, characterized in that: The density of the rigid polyurethane foam is 300-450 Kg / m 3 , the density of the reinforcing fiber ranges from 1 to 2.7 g / cm 3 .

3. The fiber-reinforced polyurethane composite material according to claim 2, characterized in that: The hydroxyl value of the composite polyether is 30-500 mg·KOH / g, and the average functionality is 2-6.

4. The fiber-reinforced polyurethane composite material according to claim 3, characterized in that: The average functionality of the combined polyether is 3 to 4.

5.

5. The fiber-reinforced polyurethane composite material according to claim 4, characterized in that: The isocyanate or modified isocyanate is aliphatic, alicyclic, araliphatic, aromatic isocyanate or a combination thereof.

6. The fiber-reinforced polyurethane composite material according to claim 5, characterized in that: A flame retardant with a flame retardancy level of B1 or above is added to the composite material, and the mass ratio of the composite material to the flame retardant is 10:1 to 10:

4.

7. The fiber-reinforced polyurethane composite material according to claim 6, characterized in that: The flame retardant is an inorganic filler flame retardant.

8. The fiber-reinforced polyurethane composite material according to claim 7, characterized in that: The inorganic filler flame retardant is one of phosphorus-based, nitrogen-based, expanded graphite-based, magnesium hydroxide, and montmorillonite, or a mixture of several of them.

9. Use of the fiber-reinforced polyurethane composite material according to any one of claims 1 to 8, characterized in that: The composite material is used in doors and windows, door and window reinforcement materials, installation auxiliary frames, indoor and outdoor decorative panels and pedestrian walkways.