A method for determining the dynamic parameters of martensitic phase transformation in gear steel layer

Through vacuum arc furnace smelting and Gleeble3500 thermal simulation experiments, the expansion curve was measured, combined with X-ray diffraction method and metallographic microscopy technology, the martensite phase transformation temperature and dynamic parameters were determined, and a finite element model was established to solve the deformation prediction of workpieces after carburization. The problem of insufficient accuracy improves the accuracy and accuracy of carburizing and quenching simulation.

CN115200492BActive Publication Date: 2024-11-12JIANGLU MACHINERY & ELECTRONICS GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210796995.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-06
Publication Date
2024-11-12
Estimated Expiration
2042-07-06

AI Technical Summary

Technical Problem

In the numerical simulation of heat treatment, the research and analysis accuracy of the workpiece seepage structure performance and overall deformation law after carburization is insufficient, especially the data lack and accuracy of the determination of the dynamic parameters of martensite phase change, which affects the accurate prediction of the quenching process. .

Method used

The gear steel samples with different carbon contents were prepared by vacuum arc furnace smelting, and the expansion curve was measured by Gleeble3500 thermal simulation experiment. Combined with X-ray diffraction method and metallographic microscopy technology, the martensite phase transformation temperature and kinetic parameters were determined, and the finite element was established. The model simulates the carburizing and quenching process to improve the accuracy of deformation prediction.

Benefits of technology

The 20Cr2Ni4A material database has been enriched, the accuracy and accuracy of carburizing and quenching simulation calculation has been improved, and the heat treatment deformation control of gear parts has been guided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115200492B_ABST
    Figure CN115200492B_ABST
Patent Text Reader

Abstract

The invention discloses a method for determining the kinetic parameters of martensitic phase transformation of a gear steel carburized layer, relates to heat treatment in the steel industry, and solves the problem of insufficient prediction accuracy and precision of steel carburized and quenched workpieces. The method comprises the following steps: smelting a sample, using a thermal simulation test machine to determine the expansion-temperature curve of the sample at different cooling rates, performing tissue content detection, determining the critical cooling rate of martensitic transformation, and drawing a CCT curve of a continuous cooling process; calculating and obtaining the austenite thermal expansion coefficient, martensite thermal expansion coefficient, phase transformation expansion coefficient, Ms point and kinetic equation coefficient α of five groups of samples with different carbon contents; fitting the change of Ms point with carbon content and cooling based on the experimental results, and obtaining the change relationship of martensitic transformation temperature with carbon content and cooling; and simulating the carburization and quenching of gear parts with the obtained phase transformation kinetic parameters; the invention improves the accuracy and precision of steel carburization and quenching simulation calculation, thereby guiding the heat treatment deformation control of gear parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment in the steel industry, and more particularly to a method for determining kinetic parameters of martensitic phase transformation of a gear steel infiltration layer. Background Art

[0002] At present, in the field of numerical simulation of heat treatment, the research and analysis accuracy of the microstructure and overall deformation law of the carburized layer of the workpiece after carburizing needs to be improved, and there are some problems of lack of data and insufficient accuracy in the material parameters that play a decisive role in the prediction accuracy and precision; the accuracy of deformation prediction in heat treatment simulation depends to a large extent on the calculation of phase transformation strain, and the calculation of phase transformation strain is related to the phase variable and phase expansion coefficient; in carburizing heat treatment, the carbon distribution of the carburized layer determines the quenching phase transformation process, so to achieve accurate prediction of the microstructure and deformation after phase transformation, it is necessary to accurately measure the martensitic phase transformation kinetic parameters of samples with different carbon contents cooled at different cooling rates; for the calculation of phase variable, The calculation is mainly defined by the KM equation. When solving the KM equation, not only the Ms point but also the phase transformation kinetic equation coefficient α is required. There are many ways to obtain Ms. The most common method is to calculate it through the JMatPro performance software. Some scholars also obtain it based on the Ms empirical formula. However, these methods have obvious reliability and data validity problems. In addition, for the carburizing and quenching process, the carbon content of the carburized layer is unevenly distributed. The cooling rate at different positions is different due to the thickness during the quenching process, which will affect the value of the Ms point. The calculation deviation of the Ms point will be amplified during the carburizing and quenching simulation. Therefore, obtaining the Ms point with different carbon content in the carburized layer is a prerequisite for improving the accuracy of deformation prediction. In addition, the calculation of the phase transformation kinetic equation coefficient α cannot be ignored. At present, most scholars take α as 0.011, which is not rigorous enough. α is not only affected by alloying elements but also related to carbon content and cooling rate. Therefore, it is of great significance to carry out experimental determination of the martensitic phase transformation kinetic parameters of these alloys by melting and carburizing representative alloys with the same composition, which is of great significance to improve the accuracy of carburizing and quenching simulation.

[0003] The two tissues have different specific volumes before and after the phase transformation, and the resulting volume change also has a great influence on the deformation calculation; the volume expansion of the martensitic transformation process is determined by the phase expansion coefficient, and the influence of temperature on the phase expansion coefficient is much greater than that of the composition; there are currently few reports and information on the phase transformation expansion coefficient, which cannot be calculated by JMatPro. At the same time, through consulting the literature, it is found that the data of the parameters used by different scholars can differ by more than one time; in most cases, the deformation caused by the volume difference of the tissues during the phase transformation process is usually ignored; for materials with specific compositions and thin-walled parts, the contribution of phase transformation to deformation is large and cannot be ignored; and at present, the experimental data of the phase transformation expansion coefficient after carburizing treatment is relatively lacking, which is one of the main reasons why the accurate prediction of the carburizing and quenching process cannot be achieved. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problem of insufficient prediction accuracy and precision of workpieces after carburizing, and to provide a method for determining the kinetic parameters of martensitic phase transformation of a carburized layer of gear steel.

[0005] The technical solution adopted by the present invention is as follows: A method for determining the kinetic parameters of martensitic phase transformation of a gear steel infiltration layer comprises the following steps:

[0006] S1. Use vacuum arc furnace to melt 5 groups of samples with the same carbon content as gear steel, 0.2%, 0.4%, 0.6%, 0.8% and 1.0% respectively. Make the melted materials into round bar samples and machine a circular groove at one end to facilitate clamping;

[0007] S2. Clamp the sample with a fixture and weld the thermocouple in the middle of the sample. Put the sample into the Gleeble3500 thermal simulation test machine, clamp the expansion instrument on the heating part in the center of the standard sample, measure the radial deformation in the uniform temperature zone, set the heating temperature and cool at different cooling rates after austenitization. The instrument will automatically record the temperature and expansion data at different cooling rates to obtain the temperature-expansion curve;

[0008] S3. Process the expansion curve into a temperature-expansion rate curve, and use the tangent method to determine the Ms point of the five groups of samples, the austenite expansion coefficient α A 、Martensite thermal expansion coefficient α M , phase expansion coefficient

[0009] S4, using X-ray diffraction to measure the martensite and austenite contents of the thermal expansion sample, and obtaining the martensite transformation kinetic coefficient α according to the KM model;

[0010] S5, measuring the Vickers hardness at the middle position of the sample in step S2, and observing the microstructure with a metallographic microscope, determining the critical cooling rate of martensite in combination with the Ms point in step S2, and drawing a CCT curve;

[0011] S6. Plot the Ms point and the martensitic transformation kinetic parameter α calculated in step S3 on the coordinate axes, with the carbon content as the abscissa and Ms and α as the ordinates, respectively, and use linear fitting to find out the relationship between the martensitic transformation temperature of the gear steel carburized layer and the carbon content and cooling rate;

[0012] S7, establishing a material model, using the martensitic transformation kinetic parameters and CCT curve obtained in step S3 as well as the Young's modulus, Poisson's ratio and density of the material as material model parameters, and establishing a gear finite element model to simulate the carbon concentration, structure and deformation distribution of the gear during carburizing and quenching;

[0013] S8. Measure gear deformation and take samples for testing, including hardness and tissue content.

[0014] The specific steps of the vacuum arc furnace melting in step S1 include: cleaning and decontaminating the molten material before vacuum melting, washing the crucible and the two electrodes and then drying them, introducing cooling water, turning on the mechanical pump for preheating and then evacuating to a low vacuum degree; opening the molecular valve, evacuating the air in multiple stages, and then introducing argon gas for 3 times for washing; during the melting process, shaking the hand wheel to control the electrode, starting the high-frequency power supply to perform arc striking operation, and using the electric arc to melt the molten material.

[0015] In step S1, 8 samples of each group with different carbon contents are prepared, for a total of 40 samples, which are heated to 50°C above Ac3 / Ac1 on a Gleeble3500 thermal simulation test machine, with a heating rate of 1°C / s and a holding time of 600s to ensure sufficient austenitization for the determination of expansion curves at different cooling rates.

[0016] In step S2, after austenitizing, cooling is performed at cooling rates of 17.2°C / s, 8.6°C / s, 4.3°C / s, 1.72°C / s, 0.86°C / s, 0.28°C / s, 0.14°C / s, and 0.06°C / s, and the radial expansion-temperature curve at the center of the sample is recorded.

[0017] The sample measured in step S2 is inlaid, ground, polished, and corroded with 4% nitric acid alcohol solution. The structure morphology is observed under a metallographic microscope, and the hardness is characterized on a Vickers hardness tester. In step S3, the intersection point Ms is determined by the double tangent method on the expansion curve; the tangent line to the upper end of the expansion curve is drawn, and the austenite thermal expansion coefficient α is obtained from the above formula. A ; Draw the tangent line at the lower end of the expansion curve, which is the thermal expansion coefficient of martensite α M At this time, the intersection of the tangent and the vertical axis can be considered as the complete transformation of martensite at 0°C, that is, the volume change rate caused by the transformation of austenite to martensite, and the intercept is the expansion coefficient of the martensite phase at 0°C

[0018] From this, we can get the expansion coefficient of austenite to martensite at any temperature T.

[0019]

[0020] In step S3, the CCT curves of the continuous cooling process of the samples with carbon contents of 0.2%C, 0.4%C, 0.6%C, 0.8%C and 1.0%C are plotted in combination with step S2.

[0021] In step S4, the method for determining the content of martensite and austenite is to cut, grind and polish 5 groups of 40 samples, identify the physical phase of the samples by XRD, extract the diffraction line intensity by Jade 9.0, and calculate the content of martensite and austenite.

[0022] The material model is established as described in step 7. The specific steps are as follows:

[0023] S71. Use finite element simulation software to establish a gear model and material model for the carburizing and quenching process, and define the Poisson's ratio, thermal expansion coefficient, phase expansion coefficient, Young's modulus, density, austenitizing temperature, Ms point and α of martensite and austenite for the established material model, and define the thermal strain, phase change strain and organization and strain behavior of the material in the phase change process with the data of the expansion curve of the cooling process obtained in step S1, and define the material as an isotropic geometric material;

[0024] S72. Use pre-processing software to mesh the gear, convert the geometric model into a finite element model, and import the mesh into the simulation software to establish boundary conditions. Lay the gear flat, use the bottom surface of the gear as the load-bearing surface, and load gravity perpendicular to the ground. Define the working conditions as 930°C carburizing and 800°C quenching.

[0025] S73. Combine the material model of S71 and the finite element model of S72 to perform simulation analysis to obtain the carbon distribution, tissue distribution, and deformation distribution cloud maps. Use measuring tools to measure the characteristic parts of the gears and calculate the deformation data of ovality, taper, and shrinkage.

[0026] The material model described in step 7 is established based on Thermal Prophet heat treatment professional software, and the thermophysical property parameters used are input as a function of temperature-carbon content-organization performance parameters.

[0027] In step S72, Hypermesh software is used for meshing, and the meshing methods include free meshing, adaptive meshing, characteristic structure offset, permeation layer mesh segmentation control, and mesh mapping.

[0028] In step 8, the gear deformation is measured using three-dimensional coordinate scanning and a digital display vernier caliper, the hardness test is performed using a Vickers hardness tester, and the tissue content is determined using XRD ray diffraction analysis combined with Jade software calculation.

[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0030] For metal materials that need to be carburized and quenched, this method can not only determine the martensitic phase transformation kinetic parameter Ms point and kinetic equation coefficient α of materials with the same composition as the carburized layer, but also obtain the austenitizing temperature, thermal expansion coefficient, austenite thermal expansion coefficient, martensite thermal expansion coefficient, and phase transformation expansion coefficient, enriching the 20Cr2Ni4A material database and improving the accuracy and precision of the carburizing and quenching simulation calculation of 20Cr2Ni4A steel, thereby guiding the heat treatment deformation control of gear parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The present invention will now be described by way of example with reference to the accompanying drawings, in which:

[0032] Figure 1 It is a structural diagram of the expansion specimen of the present invention;

[0033] Figure 2 They are the schematic diagrams of the double tangent lines and the ΔL / L0-T curves of (a) 20Cr2Ni4A, (b) 40Cr2Ni4A, (c) 60Cr2Ni4A, (d) 80Cr2Ni4A, and (e) 100Cr2Ni4A;

[0034] Figure 3 This is the CCT curve of 20Cr2Ni4A measured;

[0035] Figure 4 is the Ms fitting curve graph;

[0036] Figure 5 is the α fitting curve graph;

[0037] Figure 6 is the finite element mesh diagram of the gear;

[0038] Figure 7 It is the deformation cloud diagram of gear carburizing and quenching. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0040] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] like Figure 1-7 As shown, this embodiment provides a method for determining the kinetic parameters of martensitic phase transformation of a gear steel infiltration layer, and the specific steps are as follows:

[0043] S1. Smelt gear steel and carbon together into samples with different carbon contents, and process them into standard samples for thermal expansion testing. The specific steps are as follows:

[0044] S11, prepare the melt, clean and dry it, check each system before opening the furnace, clean the crucible and two electrodes after the inspection, open the main gate after drying, and pass cooling water;

[0045] S12, turn on the mechanical pump, preheat for 30 minutes, ensure the equipment is stable, and start vacuuming after preheating;

[0046] S13, when the vacuum reaches 5×10-1Pa, close the valve of the mechanical pump and open the molecular pump to perform multiple multi-stage vacuuming;

[0047] S14, after evacuating to vacuum, introduce argon gas, perform 2-3 times of gas washing, evacuate to vacuum again, and fill with argon gas;

[0048] S15, placing the melt on the crucible, turning the hand wheel to move the electrode and align it with the crucible electrode, turning on the high-frequency power supply, turning the hand wheel to make the electrodes contact and strike an arc, and separating the electrodes after the arc is struck, keeping a proper distance;

[0049] S16. Turn the hand wheel to melt the molten material with electric arc, and move the arc several times to prevent overburning; use the mechanical arm to turn the sample during melting to ensure uniform melting;

[0050] S17. After the smelting is completed and the sample is cooled, the DF-100 photoelectric direct reading spectrometer is used to detect the smelted sample material. The composition is as follows:

[0051] Table 1 Element composition of XXCr2Ni4A steel (wt%)

[0052] C Si Mn Cr Ni Mo Nb Al V 20Cr 0.1753 0.31291 0.51996 1.45815 3.30683 0.00177 0.00225 0.02156 0.05256 40Cr 0.3767 0.33724 0.50817 1.38136 3.4362 0.00114 0.0023 0.02514 0.01117 60Cr 0.56785 0.34571 0.51489 1.37053 3.4306 0.00133 0.00285 0.0266 0.00937 80Cr 0.76558 0.3633 0.51361 1.34669 3.42124 0.00161 0.0035 0.02555 0.00653 100Cr 1.01801 0.36287 0.52142 1.34395 3.40101 0.00139 0.00336 0.03236 0.00536

[0053] S2. Place 8 samples of each of the 5 groups of carbon content samples into the Gleeble 3500 thermal simulator for thermal expansion test. The specific steps are as follows:

[0054] S21. Prepare 5 groups of samples with 0.2%C, 0.4%C, 0.6%C, 0.8%C and 1.0%C into φ3mm×10mm cylindrical specimens, spot weld the thermocouple in the middle of the specimen, clamp the two ends of the specimen with copper fixtures, put it into the specimen machine, and fix the copper fixture with the clamp and the slide;

[0055] S22. Clamp the radial expansion instrument on the cross section where the thermocouple is located to measure the radial deformation of the sample in the uniform temperature zone; pass current through the sample to be measured to heat it with the resistance of the sample itself; heat it to 880°C on a Gleeble thermal simulator and keep it warm for 600s. After keeping warm, cool it to room temperature at different cooling rates (17.2°C / s, 8.6°C / s, 4.3°C / s, 1.72°C / s, 0.86°C / s, 0.28°C / s, 0.14°C / s, 0.06°C / s), and use an automatic recorder to record the change of the sample expansion with temperature (Δd-T) during the cooling process;

[0056] S3. Obtain the martensitic phase transformation temperature Ms, the austenite thermal expansion coefficient, the martensite thermal expansion coefficient, and the martensitic phase expansion coefficient according to the thermal expansion curve, and draw a CCT curve. The specific steps are as follows:

[0057] The physical meaning of the thermal expansion coefficient is the change in unit length of the sample when the temperature increases or decreases by 1K, which can be calculated by the following formula:

[0058]

[0059] Where α is the thermal expansion coefficient, d is the diameter after heat treatment, d0 is the diameter before heat treatment, △T is the temperature increment, and △d is the diameter increment.

[0060] S31. Divide the expansion curve by the original diameter to obtain the expansion rate (Δd / d0-T) curve. Use the double tangent method to make an intersection on the expansion rate curve to determine the phase change Ms. Make a tangent to the upper end of the expansion rate curve. From the above formula, we know that the thermal expansion coefficient of austenite is α. A ; Draw the tangent line at the lower end of the expansion rate curve, which is the thermal expansion coefficient of martensite α M At this time, the intersection of the tangent and the vertical axis can be considered as the complete transformation of martensite at 0°C, that is, the volume change rate caused by the transformation of austenite to martensite, and the intercept is the expansion coefficient of the martensite phase at 0°C

[0061] From this, we can get the expansion coefficient of austenite to martensite at any temperature T.

[0062]

[0063] S32. By making a double tangent of the expansion rate curve, the following phase change parameters can be obtained:

[0064] Table 2 Calculation results of XXCr2Ni4A expansion experiment

[0065]

[0066] S33, the samples with different cooling processes were inlaid, ground, polished, and corroded with 4% nitric acid alcohol solution, and the microstructure was observed by metallographic microscope and scanning electron microscope, and the critical cooling rate of martensitic transformation was determined; the CCT curves of the continuous cooling process of 0.2%C, 0.4%C, 0.6%C, 0.8%C, and 1.0%C were drawn in combination with the expansion rate curve;

[0067] S4. Plot the Ms and phase change kinetic parameter α calculated in step S3 on the coordinate axes, with temperature as the abscissa and Ms and α as the ordinates, and use linear fitting to obtain the relationship between Ms and α and carbon content as follows:

[0068] Ms=419-360C

[0069] α=0.02841-0.00613C

[0070] S5. The steps of establishing the finite element model and numerical calculation of the carburizing and quenching process are as follows:

[0071] S51. Use finite element simulation software to establish a gear model and material model for the carburizing and quenching process, and define the Poisson's ratio, thermal expansion coefficient, phase expansion coefficient, Young's modulus, density, austenitizing temperature, phase transformation Ms and phase transformation kinetic equation coefficient of martensite and austenite for the established material model, and define the material thermal strain, phase transformation strain and the organization and strain behavior of the phase transformation process with the data of the expansion curve of the cooling process obtained in step S1, and define the isotropic geometric material of the material;

[0072] S52. Use pre-processing software to mesh the gears. The meshing methods include free meshing, adaptive meshing, characteristic structure offset, permeation layer mesh segmentation control, and mesh mapping. To improve the accuracy of simulation calculations, the mesh type is a full hexahedron. At the same time, the calculation convergence is ensured, and the mesh quality is checked according to GB / T33582-2017 "General Rules for Finite Element Analysis of Mechanical Product Structures";

[0073] Import the mesh into the simulation software to establish boundary conditions, place the gear flat, use the bottom surface of the gear as the force-bearing surface, and load gravity perpendicular to the ground. At the same time, define the working conditions as 930℃ carburizing and 880℃ quenching.

[0074] S53, combining the material model of S51 and the finite element model of S52 to perform simulation analysis, obtain the carbon distribution, organization distribution, and deformation distribution cloud map, use the measuring tool to measure the characteristic parts of the gear teeth, and calculate the technical requirement indicators such as ovality and shrinkage;

[0075] The material model is established based on Thermal Prophet heat treatment professional software, and the data definition adopts the function form of temperature-carbon content-organization performance parameters;

[0076] The above finite element model is analyzed to obtain the organization and deformation distribution cloud map, as shown in the figure. The path curve (pathplotting) and distance measurement tool (distance) are used to extract the data of gear tooth organization and deformation. The calculation results are shown in Table 3.

[0077] The deformation of the gear after carburizing and quenching was measured, and the gear ovality and shrinkage were measured by three-dimensional scanning; the gear was sampled, inlaid, ground, polished, and corroded for metallographic microscopic observation, and the sample was prepared for phase identification using XRD, and the diffraction line intensity was extracted by Jade9.0 to calculate the martensite and austenite content. The test results are shown in Table 3:

[0078] Table 3 Gear test results

[0079]

[0080] The experimental results are highly consistent with the simulation values, which proves the accuracy of the determination of the kinetic parameters of martensitic transformation in the gear steel layer.

Claims

1. A method for determining the kinetic parameters of martensitic transformation of a gear steel layer, characterized in that: The following steps are involved: S1. Use vacuum arc furnace to melt 5 groups of samples with the same carbon content as gear steel, 0.2%, 0.4%, 0.6%, 0.8% and 1.0% respectively. Make the melted materials into round bar samples and machine a circular groove at one end to facilitate clamping; S2. Clamp the sample with a fixture and weld the thermocouple in the middle of the sample. Put the sample into the Gleeble 3500 thermal simulation test machine, clamp the expansion instrument on the heating part in the center of the standard sample, measure the radial deformation in the uniform temperature zone, set the heating temperature and cool at different cooling rates after austenitization. The instrument will automatically record the temperature and expansion data at different cooling rates to obtain the temperature-expansion curve. S3. Process the expansion curve into a temperature-expansion rate curve, and use the tangent method to determine the Ms point of the five groups of samples, the austenite expansion coefficient α A 、Martensite thermal expansion coefficient α M , phase expansion coefficient ; S4, using X-ray diffraction to measure the martensite and austenite contents of the thermal expansion sample, and obtaining the martensite transformation kinetic coefficient α according to the KM model; S5, measuring the Vickers hardness at the middle position of the sample in step S2, and observing the microstructure with a metallographic microscope, determining the critical cooling rate of martensite in combination with the Ms point in step S2, and drawing a CCT curve; S6. Plot the Ms point and the martensitic transformation kinetic parameter α calculated in step S3 on the coordinate axes, with the carbon content as the abscissa and Ms and α as the ordinates, respectively, and use linear fitting to find out the relationship between the martensitic transformation temperature of the gear steel carburized layer and the carbon content and cooling rate; S7, establishing a material model, using the martensitic transformation kinetic parameters and CCT curve obtained in step S3 as well as the Young's modulus, Poisson's ratio and density parameters of the material as material model parameters, and establishing a gear finite element model to simulate the carbon concentration, structure and deformation distribution of the gear during carburizing and quenching; S8. Measure gear deformation and take samples for testing, including hardness and tissue content.

2. The method for determining the kinetic parameters of martensitic transformation of gear steel layer according to claim 1, characterized in that: The specific steps of the vacuum arc furnace melting in step S1 include: cleaning and decontaminating the molten material before vacuum melting, washing the crucible and the two electrodes and then drying them, introducing cooling water, turning on the mechanical pump for preheating and then evacuating to a low vacuum degree; opening the molecular valve, evacuating the air in multiple stages, and then introducing argon gas for 3 times for washing; during the melting process, shaking the hand wheel to control the electrode, starting the high-frequency power supply to perform arc striking operation, and using the electric arc to melt the molten material.

3. The method for determining the kinetic parameters of martensitic transformation of gear steel layer according to claim 1, characterized in that: In step S1, 8 samples of each group with different carbon contents are prepared, and they are heated to 50°C above Ac3 / Ac1 on a Gleeble3500 thermal simulation test machine, with a heating rate of 1°C / s and a holding time of 600s to ensure full austenitization.

4. The method for determining the kinetic parameters of martensitic transformation of a gear steel layer according to claim 1, characterized in that: In step S2, after austenitizing, cooling is performed at 17.2°C / s, 8.6°C / s, 4.3°C / s, 1.72°C / s, 0.86°C / s, 0.28°C / s, 0.14°C / s, and 0.06°C / s, and the radial expansion-temperature curve at the center of the sample is recorded.

5. The method for determining the kinetic parameters of martensitic transformation of gear steel infiltration layer according to claim 1, characterized in that: The sample measured in step S2 is inlaid, ground, polished, and corroded with 4% nitric acid alcohol solution. The structure morphology is observed under a metallographic microscope, and the hardness is characterized on a Vickers hardness tester. In step S3, the intersection point Ms is determined by the double tangent method on the expansion curve; the tangent line to the upper end of the expansion curve is drawn, and the austenite thermal expansion coefficient α is obtained from the above formula. A ; Draw the tangent line at the lower end of the expansion curve, which is the thermal expansion coefficient of martensite α M At this time, the intersection of the tangent and the vertical axis can be considered as the complete transformation of martensite at 0°C, that is, the volume change rate caused by the transformation of austenite to martensite, and the intercept is the expansion coefficient of the martensite phase at 0°C From this, the expansion coefficient of austenite to martensite at any temperature T is obtained In step S3, the CCT curves of the continuous cooling process of the samples with carbon contents of 0.2%C, 0.4%C, 0.6%C, 0.8%C and 1.0%C are plotted in combination with step S2.

6. The method for determining the kinetic parameters of martensitic transformation of gear steel infiltration layer according to claim 1, characterized in that: In step S4, the method for determining the content of martensite and austenite is to cut, grind and polish 5 groups of 40 samples, identify the physical phase of the samples by XRD, extract the diffraction line intensity by Jade 9.0, and calculate the content of martensite and austenite.

7. The method for determining the kinetic parameters of martensitic transformation of gear steel layer according to claim 1, characterized in that: The material model is established as described in step 7. The specific steps are as follows: S71. Use finite element simulation software to establish a gear model and material model for the carburizing and quenching process, and define the Poisson's ratio, thermal expansion coefficient, phase expansion coefficient, Young's modulus, density, austenitizing temperature, Ms point and α of martensite and austenite for the established material model, and define the thermal strain, phase change strain and organization and strain behavior of the material in the phase change process with the data of the expansion curve of the cooling process obtained in step S1, and define the material as an isotropic geometric material; S72. Use pre-processing software to mesh the gear, convert the geometric model into a finite element model, and import the mesh into the simulation software to establish boundary conditions. Lay the gear flat, use the bottom surface of the gear as the load-bearing surface, and load gravity perpendicular to the ground. Define the working conditions as 930°C carburizing and 800°C quenching. S73. Combine the material model of S71 and the finite element model of S72 to perform simulation analysis to obtain the carbon content, tissue distribution, and deformation distribution cloud map. Use measuring tools to measure the characteristic parts of the gear and calculate the deformation data of ovality, taper, and shrinkage.

8. The method for determining the kinetic parameters of martensitic transformation of gear steel layer according to claim 1, characterized in that: In step 8, the gear deformation is measured using three-dimensional coordinate scanning and a digital display vernier caliper, the hardness test is performed using a Vickers hardness tester, and the tissue content is determined using XRD ray diffraction analysis combined with Jade software calculation.

9. The method for determining the kinetic parameters of martensitic transformation of a gear steel layer according to claim 1, characterized in that: The material model described in step 7 is established based on Thermal Prophet heat treatment professional software, and the thermophysical property parameters used are input as a function of temperature-carbon content-organization performance parameters.

10. The method for determining the kinetic parameters of martensitic transformation of a gear steel layer according to claim 7, characterized in that: In step S72, Hypermesh software is used for meshing, and the meshing methods include free meshing, adaptive meshing, characteristic structure offset, permeation layer mesh segmentation control, and mesh mapping.