Resin sheet and circuit board material using the same
By using a resin sheet composed of a cyclic polyolefin resin copolymer with a temperature lower than 100°C and a hydrogenated block unit, the problem of transmission loss in the high-frequency region is solved, low dielectric properties are achieved, and the transmission efficiency of communication signals is improved. reliability.
Patent Information
- Application Number
- CN202180017158.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-02-19
AI Technical Summary
Existing circuit substrate materials have increased transmission losses in high-frequency regions, resulting in attenuation and reduced reliability of communication signals. Materials with low dielectric properties need to be developed to suppress transmission losses.
A resin sheet containing a specific cyclic polyolefin resin copolymer is used, and the resin layer of the resin sheet contains a cyclic polyolefin resin copolymer with a crystal melting peak temperature of less than 100°C, and is produced by hydrogenating an aromatic vinyl polymer and hydrogenating a copolymer. A combination of conjugated diene polymer block units to optimize its dielectric loss tangent.
The dielectric loss tangent is less than 0.005 at 12GHz, which reduces the dielectric loss and improves the transmission efficiency and communication reliability of electrical signals.
Smart Images

Figure GDA0003817174100000071 
Figure GDA0003817174100000301 
Figure GDA0003817174100000341
Abstract
Description
Technical Field
[0001] The present invention relates to a resin sheet having excellent low dielectric properties and a circuit board material using the same. Background Art
[0002] Generally, as circuit board materials used in electrical and electronic equipment, what is mainly used is a copper-clad laminate (CCL), which is obtained by applying copper foil to the surface of an insulating plate obtained by overlapping sheets (prepreg) impregnated with resin on a substrate such as paper or glass and subjecting them to a pressurized heat treatment; and what is called a flexible printed circuit (FPC), which is obtained by forming an insulating adhesive layer on a base film and pasting a conductor foil such as copper thereon.
[0003] In recent years, due to the increase in the amount and speed of information transmission in electrical / electronic equipment, the frequency of communication has been increasing. Among them, the increase in transmission loss (α) has become a major issue. The lower the value of this transmission loss (α), the less the attenuation of the information signal, which means that high reliability of communication can be ensured.
[0004] Transmission loss (α) is proportional to frequency (f), so α becomes larger in communication in high frequency regions, resulting in reduced reliability. As a method of suppressing transmission loss (α), a method of reducing the dielectric loss tangent (tanδ) proportional to α in the same way as frequency (f) can be cited. In order to transmit communication signals at high speed, materials with low dielectric loss tangent (tanδ), that is, materials with low dielectric properties, are required.
[0005] As materials having low dielectric properties, for example, Patent Document 1 describes a low dielectric resin composition, a laminate, and a metal-clad laminate containing a polyimide having a specific structure and a bisimide compound having a specific structure.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2001-006437 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] An object of the present invention is to provide a resin sheet having low dielectric properties and a circuit board material using the same.
[0011] Solutions for solving problems
[0012] The present inventors have conducted intensive studies to solve the above problems and have found that a resin sheet containing a specific cyclic polyolefin resin copolymer can solve the above problems.
[0013] That is, the present invention has the following features.
[0014] [1] A resin sheet comprising at least a resin layer (A) and having a dielectric loss tangent of less than 0.005 at 12 GHz, wherein the resin layer (A) contains a cyclic polyolefin resin copolymer having a crystal melting peak temperature of less than 100°C.
[0015] [2] The resin sheet according to [1], wherein the cyclic polyolefin resin copolymer has cyclohexane in a side chain of the polyolefin.
[0016] [3] The resin sheet according to [1] or [2], wherein the cyclic polyolefin resin copolymer is: a resin copolymer comprising at least one hydrogenated aromatic vinyl polymer block unit and at least one hydrogenated conjugated diene polymer block unit; or a modified product of the resin copolymer obtained using an unsaturated carboxylic acid and / or anhydride thereof.
[0017] [4] The resin sheet according to [3], wherein the hydrogenation level of the hydrogenated aromatic vinyl polymer block unit is 90% or more.
[0018] [5] The resin sheet according to [3] or [4], wherein the hydrogenation level of the hydrogenated conjugated diene polymer block unit is 95% or more.
[0019] [6] The resin sheet according to any one of [1] to [5], wherein the resin layer (A) contains a thermoplastic resin (b), and the thermoplastic resin (b) is at least one selected from the group consisting of ethylene polymers, olefin thermoplastic elastomers and styrene thermoplastic elastomers.
[0020] [7] The resin sheet according to [6], wherein the storage modulus at 24° C. is less than 2000 MPa.
[0021] [8] The resin sheet according to any one of [1] to [5], wherein the resin layer (A) is a composite containing a glass cloth (C).
[0022] [9] The resin sheet according to any one of [1] to [5], wherein the resin sheet is a laminate comprising the resin layer (A) and a glass cloth (C).
[0023]
[10] The resin sheet according to [8] or [9], wherein the dielectric loss tangent of the glass cloth (C) is less than 0.005 at 10 GHz.
[0024]
[11] A resin sheet according to any one of [1] to [5], wherein the resin sheet is a laminate comprising the resin layer (A) and a resin layer (D), wherein the resin layer (D) contains an amorphous resin (d) having a glass transition point of 100°C or higher and a dielectric loss tangent of less than 0.02 at 12 GHz.
[0025]
[12] The resin sheet according to
[11] , wherein the amorphous resin (d) is at least one resin selected from the group consisting of alicyclic olefin polymers, polycarbonates, polyarylates, polysulfones, and copolymers thereof.
[0026]
[13] The resin sheet according to
[11] or
[12] , wherein at least one outermost layer is a resin layer (A).
[0027]
[14] The resin sheet according to any one of [1] to
[13] , which is used for a circuit board.
[0028]
[15] A circuit board material comprising a laminate of the resin sheet according to any one of [1] to
[13] and a conductor.
[0029] Effects of the Invention
[0030] According to the present invention, a resin sheet having low dielectric properties and a circuit board material using the same can be obtained. DETAILED DESCRIPTION
[0031] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the following description unless it exceeds the gist of the invention.
[0032] When the expression "to" is used below, it is used as an expression including the numerical values or physical property values before and after it.
[0033] The resin sheet of the present invention comprises at least a resin layer (A) containing a cyclic polyolefin resin copolymer having a crystal melting peak temperature of lower than 100°C.
[0034] <<Resin layer (A)>>
[0035] The resin layer (A) of the present invention contains a cyclic polyolefin resin copolymer having a crystal melting peak temperature of less than 100° C. The cyclic polyolefin resin copolymer is preferably the main component resin of the resin layer (A) from the viewpoint of low dielectric properties, and its content is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 70% by mass or more, and further preferably 80% by mass or more in the resin component constituting the resin layer (A). There is no particular upper limit on the content, and the resin component of the resin layer (A) may be only the cyclic polyolefin resin copolymer (100% by mass).
[0036] <Cyclic polyolefin resin copolymer>
[0037] The "cyclic" in the cyclic polyolefin resin copolymer of the present invention refers to the alicyclic structure possessed by the cyclic polyolefin resin copolymer, specifically, the alicyclic structure possessed by the side chain of the polyolefin. Suitable examples of the alicyclic structure include cycloalkanes, bicycloalkanes, polycyclic compounds, etc., among which cycloalkanes are preferred, and cyclohexane is more preferred.
[0038] In addition, the alicyclic structure is more preferably an alicyclic structure produced by hydrogenation of an aromatic ring in a hydrogenated aromatic vinyl polymer block unit described below.
[0039] (Physical properties of cyclic polyolefin resin copolymer)
[0040] The cyclic polyolefin resin copolymer of the present invention has a crystal melting peak temperature of less than 100°C.
[0041] The crystal melting peak temperature of the cyclic polyolefin resin copolymer is preferably 50° C. or higher, more preferably 60° C. or higher, and further preferably 65° C. or higher. The crystal melting peak temperature is preferably 90° C. or lower, and more preferably 85° C. or lower.
[0042] The crystal melting peak temperature in the present invention is the temperature at which a crystal melting peak is detected in differential scanning calorimetry (DSC) measured at a heating rate of 10°C / min. The cyclic polyolefin resin copolymer of the present invention only needs to have a crystal melting peak below 100°C, and for example, it also includes the case where the crystal melting peak exists at two points, below 100°C and at 100°C or above.
[0043] It should be noted that, as well-known cyclic polyolefins, hydrogenated products of ring-opening polymers having repeating units derived from monocyclic or polycyclic norbornene-based monomers (for example, International Publication No. 2012 / 046443, International Publication No. 2012 / 033076, etc.) can be cited, and the cyclic polyolefin has an alicyclic structure in the main chain of the polymer, and does not exist at a crystalline melting peak temperature below 100° C. or is amorphous.
[0044] On the other hand, the cyclic polyolefin resin copolymer of the present invention has an alicyclic structure in the side chain of the polyolefin, and therefore has a crystal melting peak temperature lower than 100°C.
[0045] The dielectric loss tangent of the cyclic polyolefin resin copolymer of the present invention is preferably less than 0.005 at 12 GHz, and more preferably less than 0.001. The smaller the dielectric loss tangent, the smaller the dielectric loss, so when used as a circuit substrate material, the transmission efficiency and high speed of the electrical signal can be obtained, which is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is 0 or more.
[0046] The melt flow rate (MFR) of the cyclic polyolefin resin copolymer of the present invention is not particularly limited, and is usually 0.1 g / 10 minutes or more, and is preferably 0.5 g / 10 minutes or more from the viewpoint of the molding method and the appearance of the molded body. In addition, it is usually 20.0 g / 10 minutes or less, and is preferably 10.0 g / 10 minutes or less, and more preferably 5.0 g / 10 minutes or less from the viewpoint of material strength. By setting the MFR within the above range, the compatibility with the thermoplastic resin described later is good.
[0047] The MFR is determined by measuring the temperature at 230° C. and the load at 2.16 kg in accordance with ISO R1133.
[0048] <Cyclic polyolefin (a)>
[0049] The cyclic polyolefin resin copolymer of the present invention is preferably a cyclic polyolefin comprising at least one hydrogenated aromatic vinyl polymer block unit and at least one hydrogenated conjugated diene polymer block unit (hereinafter also referred to as "cyclic polyolefin (a)"), or a modified product of the cyclic polyolefin (a) obtained using an unsaturated carboxylic acid and / or anhydride thereof (hereinafter also referred to as "modified cyclic olefin (a')") from the viewpoint of low dielectric properties.
[0050] In the present invention, "block" refers to a polymer segment of a copolymer that is microphase-separated from polymer segments having different structures or compositions from the copolymer. Microphase separation occurs because polymer segments are not mixed together in a block copolymer.
[0051] It should be noted that microphase separation and block copolymers are extensively discussed in "Block Copolymers-Designer Soft Materials" in the February 1999 issue of PHYSICS TODAY, pages 32-38.
[0052] Examples of the cyclic polyolefin (a) include a diblock copolymer composed of a hydrogenated aromatic vinyl polymer block unit (hereinafter also referred to as "block A") and a hydrogenated conjugated diene polymer block unit (hereinafter also referred to as "block B"), a triblock copolymer containing two or more blocks A and at least one of blocks B, a tetrablock copolymer, a pentablock copolymer, and the like.
[0053] The cyclic polyolefin (a) preferably contains at least two blocks A, and suitable examples thereof include ABA type, ABAB type, ABABA type and the like.
[0054] In addition, the cyclic polyolefin (a) preferably comprises a segment formed by an aromatic vinyl polymer at each end. Therefore, the cyclic polyolefin (a) of the present invention preferably has at least 2 hydrogenated aromatic vinyl polymer block units (block A) and at least 1 hydrogenated conjugated diene polymer block unit (block B) between the 2 hydrogenated aromatic vinyl polymer block units (block A). From the above viewpoint, the cyclic polyolefin (a) is more preferably ABA type or ABABA type.
[0055] The content of the hydrogenated aromatic vinyl polymer block unit (block A) in the cyclic polyolefin (a) is preferably 30 to 99 mol%, more preferably 40 to 90 mol%, and more preferably 50 mol% or more, and even more preferably 60 mol% or more.
[0056] When the ratio of the hydrogenated aromatic vinyl polymer block unit (block A) is at least the above lower limit, the rigidity does not decrease and the heat resistance and linear thermal expansion coefficient are good. On the other hand, when it is at most the above upper limit, the flexibility is good.
[0057] The content of the hydrogenated conjugated diene polymer block unit (block B) in the cyclic polyolefin (a) is preferably 1 to 70 mol%, more preferably 10 to 60 mol%, and more preferably 50 mol% or less, and even more preferably 40 mol% or less.
[0058] When the ratio of the hydrogenated conjugated diene polymer block unit (block B) is not less than the above lower limit, the flexibility is good. On the other hand, when it is not more than the above upper limit, the rigidity does not decrease, and the heat resistance and linear thermal expansion coefficient are also good.
[0059] The hydrogenated aromatic vinyl polymer block unit and the hydrogenated conjugated diene polymer block unit constituting the cyclic polyolefin (a) can be obtained by hydrogenating a polymer block composed of an aromatic vinyl monomer and a conjugated diene monomer such as 1,3-butadiene, which will be described in detail later.
[0060] In addition, the cyclic polyolefin (a) is preferably a block copolymer having no functional group. “Having no functional group” means that no functional group, that is, no group containing atoms other than carbon atoms and hydrogen atoms, exists in the block copolymer.
[0061] Hereinafter, the monomers for forming the aromatic vinyl polymer block units and the conjugated diene polymer block units before hydrogenation will be described.
[0062] (Aromatic vinyl monomer)
[0063] The aromatic vinyl monomer as a raw material of the aromatic vinyl polymer block unit before hydrogenation is a monomer represented by the general formula (1).
[0064]
[0065] In the above general formula (1), R is hydrogen or an alkyl group, and Ar is phenyl, halogenated phenyl, alkylphenyl, alkylhalogenated phenyl, naphthyl, pyridyl or anthracenyl.
[0066] When the aforementioned R is an alkyl group, the carbon number is preferably 1 to 6, and the alkyl group may be monosubstituted or polysubstituted with a functional group such as a halogen group, a nitro group, an amino group, a hydroxyl group, a cyano group, a carbonyl group, or a carboxyl group.
[0067] In addition, the aforementioned Ar is preferably a phenyl group or an alkylphenyl group, and more preferably a phenyl group.
[0068] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, vinyltoluene (including all isomers, particularly preferably p-vinyltoluene), ethylstyrene, propylstyrene, butylstyrene, vinylbiphenyl, vinylnaphthalene, vinylanthracene (including all isomers), and mixtures thereof. Among them, styrene is preferred.
[0069] (Conjugated diene monomer)
[0070] The conjugated diene monomer as a raw material of the conjugated diene polymer block unit before hydrogenation is not particularly limited as long as it is a monomer having two conjugated double bonds.
[0071] Examples of the conjugated diene monomer include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2-methyl-1,3-pentadiene, and analogous compounds thereof, and mixtures thereof. Among them, 1,3-butadiene is preferred.
[0072] It should be noted that when 1,3-butadiene is used as a conjugated diene monomer, the polybutadiene as its polymer has 1,4-bond units ([-CH2-CH=CH-CH2-]) and 1,2-bond units ([-CH2-CH(CH=CH2)-]), so through hydrogenation, the former provides the same structure as the repeating unit of polyethylene (ethylene structure), and the latter provides the same structure as the repeating unit when 1-butene is polymerized (1-butene structure). Therefore, the hydrogenated conjugated diene polymer block of the present invention preferably contains at least one of the ethylene structure and the 1-butene structure.
[0073] In addition, when isoprene is used as a conjugated diene monomer, the polyisoprene as its polymer contains 1,4-bond units ([-CH2-C(CH3)=CH-CH2-]), 3,4-bond units ([-CH2-CH(C(CH3)=CH2)-]) and 1,2-bond units ([-CH2-C(CH3)(CH=CH2)-]), and contains at least any one of the three repeating units obtained by hydrogenation.
[0074] (Block structure)
[0075] Cyclic polyolefin (a) is preferably produced by hydrogenation of multi-block copolymers such as triblock copolymers, tetrablock copolymers, and pentablock copolymers such as SBS, SBSB, SBSBS, SBSBSB, SIS, SISIS, and SISBS (herein, S refers to polystyrene, B refers to polybutadiene, and I refers to polyisoprene.) Blocks can be linear blocks or can be branched. The polymer chain in the case of branching can be bonded to any position along the backbone of the copolymer. In addition, blocks can be tapered blocks or star blocks in addition to linear blocks.
[0076] The block copolymer before hydrogenation constituting the cyclic polyolefin (a) may contain one or more additional block units other than the aromatic vinyl polymer block units and the conjugated diene polymer block units. For example, in the case of a triblock copolymer, these additional block units may be bonded to any position of the triblock polymer backbone.
[0077] Preferred examples of the hydrogenated aromatic vinyl polymer block unit include hydrogenated polystyrene, and preferred examples of the hydrogenated conjugated diene polymer block unit include hydrogenated polybutadiene or hydrogenated polyisoprene, with hydrogenated polybutadiene being more preferred.
[0078] Furthermore, as a preferred embodiment of the cyclic polyolefin (a), a hydrogenated triblock or hydrogenated pentablock copolymer of styrene and butadiene can be mentioned, and it is preferred that no other functional group or structural modifier is included.
[0079] (Hydrogenation Level)
[0080] The cyclic polyolefin (a) is substantially completely hydrogenated, in addition to the double bonds derived from the conjugated diene such as butadiene being hydrogenated, and the aromatic rings derived from styrene and the like being hydrogenated. Specifically, it means a cyclic polyolefin having the hydrogenation levels shown below.
[0081] The hydrogenation level of the hydrogenated aromatic vinyl polymer block unit is preferably 90% or more, more preferably 95% or more, further preferably 98% or more, and particularly preferably 99.5% or more.
[0082] The hydrogenation level of the hydrogenated conjugated diene polymer block unit is preferably 95% or more, more preferably 99% or more, and even more preferably 99.5% or more.
[0083] By carrying out such a high level of hydrogenation, the dielectric loss can be reduced, and the rigidity and heat resistance are also good.
[0084] The hydrogenation level of the hydrogenated aromatic vinyl polymer block units indicates the proportion of the aromatic vinyl polymer block units saturated by hydrogenation, and the hydrogenation level of the hydrogenated conjugated diene polymer block units indicates the proportion of the conjugated diene polymer block units saturated by hydrogenation.
[0085] In addition, the hydrogenation level of each block unit was determined using proton NMR.
[0086] The cyclic polyolefin (a) may be used alone or in combination of two or more.
[0087] As the cyclic polyolefin (a) of the present invention, commercially available products can be used, and specific examples thereof include TEFABLOC (registered trademark) manufactured by Mitsubishi Chemical Corporation.
[0088] <Modified Cyclic Polyolefin (a')>
[0089] As the cyclic polyolefin resin copolymer of the present invention, a modified cyclic polyolefin (a') can be used. The modified cyclic polyolefin (a') is a modified product of the above-mentioned cyclic polyolefin (a) with an unsaturated carboxylic acid and / or anhydride thereof.
[0090] By modifying the cyclic polyolefin (a), the polarity of the polymer increases, and thus it can be expected that the adhesiveness with a metal layer such as copper foil will be improved.
[0091] (Modification operation of cyclic polyolefin (a))
[0092] The modification operation of the cyclic polyolefin (a) will be described below. The modification operation is preferably performed by adding an unsaturated carboxylic acid and / or anhydride thereof as a modifying agent to the cyclic polyolefin (a) to allow the mixture to react.
[0093] [Modifier]
[0094] Examples of the unsaturated carboxylic acid and / or its anhydride as the above-mentioned modifier include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, α-ethylacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid, and their anhydrides.
[0095] Moreover, as an acid anhydride, maleic anhydride, citraconic anhydride, and nadic anhydride are mentioned specifically,.
[0096] Examples of the nadic acids or their anhydrides include endo-cis-bicyclo[2.2.1]hept-2,3-dicarboxylic acid (nadic acid), methyl-endo-cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid (methyl nadic acid), and their anhydrides.
[0097] Among these unsaturated carboxylic acids and / or their anhydrides, acrylic acid, maleic acid, nadic acid, maleic anhydride, and nadic anhydride are preferred.
[0098] The unsaturated carboxylic acid and / or its anhydride may be used alone or in combination of two or more.
[0099] [Modification method]
[0100] By modifying the cyclic polyolefin (a) with the unsaturated carboxylic acid and / or its anhydride, a modified cyclic polyolefin (a') can be obtained. As the modification method, solution modification, melt modification, solid phase modification based on electron beam or ionizing radiation irradiation, modification in a supercritical fluid, etc. can be appropriately used.
[0101] Among these, melt modification is preferred due to its excellent equipment and cost competitiveness, and melt kneading modification using an extruder due to its excellent continuous productivity is more preferred.
[0102] As the apparatus used at this time, for example, a single screw extruder, a twin screw extruder, a Banbury mixer, and a roll mixer are mentioned. Among them, a single screw extruder and a twin screw extruder are preferred because they are excellent in continuous productivity.
[0103] Generally, modification of the cyclic polyolefin (a) with an unsaturated carboxylic acid and / or anhydride thereof is performed by a grafting reaction in which a carbon-hydrogen bond of a hydrogenated conjugated diene polymer block unit, which is one of the block units constituting the cyclic polyolefin (a), is cleaved to generate a carbon radical and an unsaturated functional group is added thereto.
[0104] As a source of carbon radical generation, in addition to the above-mentioned electron beam and ionizing radiation, a high temperature method, an organic peroxide, an inorganic peroxide, an azo compound and other free radical generators can also be used. As a free radical generator, an organic peroxide is preferably used from the viewpoint of cost and operability.
[0105] Examples of the azo compound include azobisisobutyronitrile, azobisdimethylvaleronitrile, azobis(2-methylbutyronitrile), and diazonitrophenol.
[0106] Examples of the inorganic peroxide include hydrogen peroxide, potassium peroxide, sodium peroxide, calcium peroxide, magnesium peroxide, and barium peroxide.
[0107] Examples of the organic peroxide include those included in the group consisting of hydroperoxide, dialkyl peroxide, diacyl peroxide, peroxyester, and ketone peroxide.
[0108] Specifically, there can be mentioned hydrogen peroxides such as cumene hydroperoxide and tert-butyl hydroperoxide; dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; diacyl peroxides such as lauryl peroxide and benzoyl peroxide; peroxyesters such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate and tert-butyl peroxyisopropyl carbonate; and ketone peroxides such as cyclohexanone peroxide.
[0109] These radical generators may be used alone or in combination of two or more.
[0110] [Melt-mixing modification]
[0111] In the commonly used melt kneading modification operation, a cyclic polyolefin (a), an unsaturated carboxylic acid and / or its anhydride, and an organic peroxide are mixed and put into a kneader or an extruder, and extruded while being heated and melt kneaded. The molten resin coming out of the front die is cooled in a water tank or the like to obtain a modified cyclic polyolefin (a').
[0112] The blending ratio of the cyclic polyolefin (a) and the unsaturated carboxylic acid and / or its anhydride is 0.2 to 5 parts by mass of the unsaturated carboxylic acid and / or its anhydride relative to 100 parts by mass of the cyclic polyolefin (a).
[0113] When the blending ratio of the unsaturated carboxylic acid and / or its anhydride to the cyclic polyolefin (a) is above the above lower limit, the required modification ratio for exerting the effect of the present invention can be obtained. In addition, when it is below the above upper limit, unreacted unsaturated carboxylic acid and / or its anhydride does not remain, which is also preferred as a dielectric property.
[0114] The blending ratio of the unsaturated carboxylic acid and / or its anhydride and the organic peroxide is 20 to 100 parts by mass of the organic peroxide relative to 100 parts by mass of the unsaturated carboxylic acid and / or its anhydride.
[0115] When the mixing ratio of the organic peroxide to the unsaturated carboxylic acid and / or its anhydride is above the lower limit, the required modification ratio for exerting the effect of the present invention can be obtained. In addition, when it is below the upper limit, the cyclic polyolefin (a) does not deteriorate and the hue does not deteriorate.
[0116] In addition, as melt-kneading and modification conditions, for example, extrusion is preferably performed at a temperature of 150 to 300° C. in a single-screw extruder or a twin-screw extruder.
[0117] [Modification rate]
[0118] The modification ratio of the modified cyclic polyolefin (a') with the unsaturated carboxylic acid and / or its anhydride is preferably 0.1 to 2% by mass.
[0119] When the modification rate is above the above lower limit, the polarity of the polymer becomes larger, and the adhesion to metal layers such as copper foil is improved, so it is preferred. In addition, when it is below the above upper limit, the deterioration of the dielectric loss of the cyclic polyolefin (a) can be prevented. In addition, the generation of odor and the deterioration of color can also be prevented.
[0120] The modification rate of the modified cyclic polyolefin (a') can be measured by proton NMR after subjecting the modified cyclic polyolefin (a') to methyl esterification.
[0121] <Other ingredients>
[0122] The resin layer (A) of the present invention may optionally contain components other than the above-mentioned cyclic polyolefin resin copolymer for the purpose of further improving functionality, specifically, UV blockers, antistatic agents, antioxidants, coupling agents, plasticizers, flame retardants, colorants, dispersants, emulsifiers, low elasticity agents, diluents, defoamers, ion capture agents, inorganic fillers, organic fillers, etc.
[0123] <<Resin Sheet Characteristics>>
[0124] The dielectric loss tangent of the resin sheet in the present invention is preferably less than 0.005 at 12 GHz, more preferably less than 0.002, and further preferably less than 0.001. The smaller the dielectric loss tangent, the smaller the dielectric loss, so when used as a circuit substrate material, the transmission efficiency and high speed of the electrical signal can be obtained, which is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is 0 or more.
[0125] The haze of the resin sheet in the present invention is preferably 10% or less, more preferably 5% or less, and further preferably 3% or less. By making the haze of the resin sheet below the above range, transparency can be ensured. The lower limit of the haze is not particularly limited as long as it is 0 or more.
[0126] The thickness of the resin sheet is preferably 10 μm or more and 200 μm or less. When the thickness is within the above range, a circuit board material can be obtained that appropriately maintains strength and can cope with miniaturization of electric and electronic equipment.
[0127] <Method for producing resin sheet>
[0128] Hereinafter, a method for producing the resin sheet of the present invention will be described. However, the following description is an example of a method for producing the resin sheet of the present invention, and the resin sheet of the present invention is not limited to a resin sheet produced by the production method described below.
[0129] The resin sheet of the present invention can be produced, for example, by melt-mixing the cyclic polyolefin resin copolymer and, if necessary, the other components described above using a single-screw or twin-screw extruder, co-extruding them using a T-die, and rapidly cooling and solidifying them using a cast roll.
[0130] When the resin sheet of the present invention is produced by kneading using an extruder or the like, it is preferred that the melt kneading be performed in a state of being heated to usually 180 to 300°C, preferably 220 to 280°C.
[0131] <<Application of resin sheet>>
[0132] Examples of uses of the resin sheet of the present invention include, but are not limited to, copper foil laminates, flexible printed circuit boards, multilayer printed circuit boards, circuit board materials for electrical / electronic devices such as capacitors, underfill materials, inter-chip fills for 3D-LSI, insulating sheets, and heat dissipation substrates.
[0133] <<First Embodiment>>
[0134] When the bending resistance of the resin sheet of the present invention is to be improved, the resin layer (A) preferably contains at least one thermoplastic resin (b) selected from the group consisting of ethylene polymers, olefin thermoplastic elastomers, and styrene thermoplastic elastomers.
[0135] That is, the first embodiment of the present invention is a resin sheet containing a cyclic polyolefin resin copolymer having a crystalline melting peak temperature of less than 100°C and at least one thermoplastic resin (b) selected from the group consisting of ethylene polymers, olefin thermoplastic elastomers and styrene thermoplastic elastomers, and having a dielectric loss tangent of less than 0.005 at 12 GHz.
[0136] Since these thermoplastic resins (b) have good compatibility with the above-mentioned cyclic polyolefin resin copolymer, the transparency of the obtained resin sheet is also good.
[0137] If the bending resistance of the resin sheet is good, it is not easy to break even if the sheet is bent, so it can be appropriately used for purposes such as flexible printed circuit boards (FPCs). In addition, it is also possible to prevent the breakage and cracking of the sheet in the process of winding into a roll and storing and conveying the sheet in a roll state when the sheet is made into a film.
[0138] Examples of the ethylene-based polymer include homopolymers of ethylene and copolymers of ethylene and other monomers.
[0139] The copolymer of ethylene and other monomers described above preferably contains ethylene as a main component. Here, "containing ethylene as a main component" means that the copolymer contains 50 mol% or more, preferably 60 mol% or more of ethylene structural units.
[0140] In addition, other monomers copolymerizable with ethylene are not particularly limited as long as they are monomers copolymerizable with ethylene.
[0141] Preferred examples of the ethylene polymer include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyethylene obtained by polymerization using a metallocene catalyst, etc. Among them, linear low-density polyethylene (LLDPE) is preferably used because of its high flexibility.
[0142] The olefin-based thermoplastic elastomer contains a polyolefin as a hard segment and a rubber component as a soft segment.
[0143] The olefin-based thermoplastic elastomer may be a mixture (polymer blend) of the polyolefin and the rubber component, a crosslinked product obtained by crosslinking the polyolefin and the rubber component, or a polymer obtained by polymerizing the polyolefin and the rubber component.
[0144] Examples of the polyolefin include polypropylene and polyethylene.
[0145] Examples of the rubber component include diene rubbers such as isoprene rubber, butadiene rubber, butyl rubber, propylene-butadiene rubber, acrylonitrile-butadiene rubber, and acrylonitrile-isoprene rubber, ethylene-propylene non-conjugated diene rubber, and ethylene-butadiene copolymer rubber.
[0146] Examples of the styrene-based thermoplastic elastomer include styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, and hydrogenated styrene-butadiene-styrene block copolymers and hydrogenated styrene-isoprene-styrene block copolymers obtained by hydrogenating these.
[0147] Among the thermoplastic resins (b), from the viewpoint of bending resistance, styrene-based thermoplastic elastomers are preferred, and hydrogenated styrene-butadiene-styrene block copolymers are more preferred.
[0148] The storage modulus of the thermoplastic resin (b) at 24°C is preferably 0.1 MPa or more, more preferably 1 MPa or more. In addition, it is preferably less than 500 MPa, more preferably less than 300 MPa, and further preferably less than 50 MPa. By making the storage modulus less than the above-mentioned upper limit, it is possible to impart appropriate flexibility and improve bending resistance when blended with the cyclic polyolefin resin copolymer. In addition, by setting the storage modulus to be above the above-mentioned lower limit, it is possible to prevent the adhesion of the thermoplastic resin (b) and the attachment of the sheet, and it is possible to produce efficiently.
[0149] The density of the thermoplastic resin (b) is preferably 930 mg / cm 3 Below, more preferably 920 mg / cm 3 Below, more preferably 910 mg / cm 3 By setting the density to be less than the above value, the storage modulus of the thermoplastic resin (b) can be easily reduced, and appropriate flexibility can be imparted when blended with the cyclic polyolefin resin copolymer, thereby improving the bending resistance.
[0150] The dielectric loss tangent of the thermoplastic resin (b) is preferably less than 0.005 at 12 GHz, and more preferably less than 0.001. The smaller the dielectric loss tangent, the smaller the dielectric loss, so when used as a circuit substrate material, the transmission efficiency and high speed of the electrical signal can be obtained, so it is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is 0 or more.
[0151] The content of the thermoplastic resin (b) in the resin layer (A) is preferably more than 5% by mass, more preferably more than 10% by mass in the resin component constituting the resin layer (A). In addition, preferably less than 50% by mass, more preferably less than 30% by mass. By making the content ratio of the thermoplastic resin (b) more than the above-mentioned lower limit, it is possible to impart flexibility and improve bending resistance to the cyclic polyolefin resin copolymer. On the other hand, by making the content ratio of the thermoplastic resin (b) less than the above-mentioned upper limit, it is possible to maintain the characteristics such as low dielectric properties and heat resistance possessed by the cyclic polyolefin resin copolymer.
[0152] Furthermore, one kind of the resins listed above as the thermoplastic resin (b) may be used alone, or two or more kinds may be used in combination.
[0153] When the resin layer (A) contains the above-mentioned thermoplastic resin (b), the storage modulus of the resin layer (A) at 24°C is preferably 50 MPa or more, more preferably 100 MPa or more, and further preferably 200 MPa or more. In addition, it is preferably less than 2000 MPa, more preferably less than 1800 MPa, and further preferably less than 1700 MPa. By making the storage modulus of the resin layer (A) above the above-mentioned lower limit, the rigidity of the sheet can be guaranteed, and undesirable conditions such as loosening or wrinkling during film making or processing can be prevented. On the other hand, by making the storage modulus of the resin layer (A) less than the above-mentioned upper limit, flexibility can be imparted to the resin sheet, and the bending resistance of the resin sheet can be improved, thereby preventing rupture when winding on a roller during film making or punching during substrate processing.
[0154] <<Second Embodiment>>
[0155] When the linear thermal expansion coefficient of the resin sheet of the present invention is to be suppressed, it is preferred that the resin sheet contain glass cloth (C).
[0156] The resin layer (A) and the glass cloth (C) may be integrated or may be separate entities.
[0157] For example, the glass cloth (C) may be impregnated with the cyclic polyolefin resin copolymer to prepare a composite body in which the cyclic polyolefin resin copolymer and the glass cloth (C) are composited and integrated to constitute the resin layer (A).
[0158] In addition, the resin layer (A) and the glass cloth (C) may be laminated as independent entities. In the case of a laminate of the resin layer (A) and the glass cloth (C), the resin layer (A) formed of a cyclic polyolefin resin copolymer may be laminated on one or both surfaces of the glass cloth (C).
[0159] Among them, from the viewpoint of low dielectric properties and low linear thermal expansion coefficient, a resin composite in which the cyclic polyolefin resin copolymer is impregnated into the glass cloth (C) and the cyclic polyolefin resin copolymer and the glass cloth (C) are integrated is preferred.
[0160] That is, an example of the second embodiment of the present invention is a resin composite containing a cyclic polyolefin resin copolymer having a crystalline melting peak temperature of less than 100° C. and a glass cloth (C).
[0161] Moreover, another example of the second embodiment of the present invention is a resin laminate including a resin layer (A) containing a cyclic polyolefin resin copolymer having a crystalline melting peak temperature of less than 100° C. and a glass cloth (C).
[0162] If the linear thermal expansion coefficient of the resin sheet can be suppressed, when the resin sheet and a conductor such as a metal layer are laminated to produce a circuit board material, the difference in linear thermal expansion coefficient between the resin sheet and the conductor can be reduced, and curling and warping after lamination can be reduced.
[0163] It should be noted that as a method for suppressing the linear thermal expansion coefficient of the resin sheet, a method of filling an inorganic filler with a low linear thermal expansion coefficient is generally used. However, if a large amount of inorganic fillers are not filled, the effect cannot be expected, and in the case of thermoplastic resins, if a large amount of inorganic fillers are filled, melt mixing and extrusion molding become difficult. In addition, as a method for suppressing the linear thermal expansion coefficient of the resin sheet, there is a method of impregnating glass fibers, but there is a problem of easily generating anisotropy.
[0164] In this embodiment, by using the glass cloth (C), an effect of isotropically suppressing the linear thermal expansion coefficient can be expected. In addition, an advantage that the content of the glass cloth (C) can be easily adjusted can also be expected.
[0165] The content of the glass cloth (C) is preferably 1% by volume or more, more preferably 3% by volume or more, and further preferably 4% by volume or more in 100% by volume of the resin layer (A). In addition, it is preferably 60% by volume or less, more preferably 40% by volume or less, and further preferably 20% by volume or less. By making the content of the glass cloth (C) above the prescribed lower limit, it is expected that the linear thermal expansion coefficient of the resin sheet can be reduced, and by making it below the prescribed upper limit, the lightness and flexibility of the resin sheet can be maintained.
[0166] The dielectric loss tangent of the glass cloth (C) is preferably less than 0.005 at 10 GHz, and more preferably less than 0.0005. The smaller the dielectric loss tangent, the smaller the dielectric loss, so when used as a circuit board material, the transmission efficiency and speed of the electrical signal can be obtained, which is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is 0 or more.
[0167] The average linear thermal expansion coefficient of the glass cloth (C) is preferably less than 5 ppm / °C, more preferably less than 3 ppm / °C in the temperature range of 0°C to 100°C. When the linear thermal expansion coefficient of the glass cloth (C) is less than the above upper limit, the linear thermal expansion coefficient of the resin sheet can be reduced.
[0168] The thickness of the glass cloth (C) is preferably 10 μm or more and 200 μm or less. By making the thickness within the above range, the glass cloth (C) has flexibility that allows it to be easily bent, so it can be expected that the linear thermal expansion coefficient can be suppressed while maintaining the flexibility of the resin. Furthermore, it is suitable for circuit board materials that can cope with miniaturization of electrical / electronic equipment.
[0169] The surface of the glass cloth (C) may be treated with a silane compound such as vinyltriethoxysilane, 2-aminopropyltriethoxysilane, 2-glycidoxypropyltrimethoxysilane, etc., in order to improve affinity with the resin and prevent peeling.
[0170] Specific examples of the glass cloth (C) include NE glass manufactured by Nitto Bosho Co., Ltd. and quartz glass "SQX series" manufactured by Shin-Etsu Chemical Co., Ltd.
[0171] The average linear thermal expansion coefficient of the resin sheet in this embodiment is preferably less than 80 ppm / °C, more preferably less than 65 ppm / °C in the temperature range of 0°C to 100°C. By setting the linear thermal expansion coefficient of the resin sheet to be less than the above upper limit, the difference in linear thermal expansion coefficient with the metal layer such as copper foil can be reduced, so that curling and warping when the resin sheet and the metal layer are laminated can be suppressed.
[0172] In the resin sheet of the present embodiment, as other components, in addition to the other components of the aforementioned resin layer (A), heat-resistant stabilizers, weathering stabilizers, slip agents, anti-blocking agents, anti-fogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, organic fillers, inorganic fillers, thermoplastic resins and thermosetting resins other than cyclic polyolefin resin copolymers may be blended as needed to the extent that the purpose of the present invention is not impaired, and the blending ratio is an appropriate amount. Specific examples of the stabilizer to be blended as an optional component include phenolic antioxidants such as tetrakis[methylene-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate alkyl ester, and 2,2'-oxalamidobis[ethyl-3(3,5-di-tert-butyl-4-hydroxyphenyl)]propionate; fatty acid metal salts such as zinc stearate, calcium stearate, and calcium 12-hydroxystearate; polyhydric alcohol fatty acid esters such as glyceryl monostearate, glyceryl monolaurate, glyceryl distearate, and pentaerythritol tristearate. These may be blended alone or in combination, and for example, a combination of tetrakis[methylene-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, zinc stearate, and glyceryl monostearate may be exemplified.
[0173] <Method for Manufacturing Resin Sheet of Second Embodiment>
[0174] The resin sheet of the present embodiment is preferably produced by the following <first production method> or <second production method>.
[0175] [First Manufacturing Method]
[0176] The first manufacturing method includes the following steps (1) and (2).
[0177] (1) A film-forming step of obtaining a sheet-like product from a cyclic polyolefin resin copolymer.
[0178] (2) A laminating step of laminating the sheet-like object and glass cloth.
[0179] (1. Film Forming Process)
[0180] In this film forming step, the cyclic polyolefin resin copolymer is formed into a sheet shape.
[0181] The film forming method is not particularly limited and may be a known method. For example, there may be mentioned a method in which a cyclic polyolefin resin copolymer is melt-extruded from a T-die and then cast using a casting roll (such as a cooling roll or a casting drum).
[0182] It should be noted that, when various additives other than the cyclic polyolefin resin copolymer are used, the cyclic polyolefin resin copolymer and the various additives can be kneaded in a kneading device before film forming. The kneading method and the kneading device used are not particularly limited, and for example, known extruders such as single-screw extruders, twin-screw extruders, and multi-screw extruders can be used.
[0183] (2. Lamination process)
[0184] In the laminating step, the sheet-like object obtained in the above-mentioned film forming step and the glass cloth (C) are laminated.
[0185] The lamination method is not particularly limited and may be a known method. For example, there may be mentioned a method of bonding the sheet-like object and the glass cloth (C) with an adhesive.
[0186] After the sheet is overlapped with the glass cloth (C), a pressure impregnation step of impregnating the glass cloth (C) with the cyclic polyolefin resin copolymer by pressurization can be performed. The cyclic polyolefin resin copolymer and the glass cloth (C) are integrally composited by the pressure impregnation step.
[0187] When hot pressing is performed, the pressing method and pressing temperature are not particularly limited. For example, the following method can be mentioned: the sheet-like object and the glass cloth (C) are overlapped and clamped between two flat plates, and hot pressing is performed at a temperature higher than the flow start temperature of the resin for 0.5 to 10 minutes and a pressure of 0.1 to 1 MPa, and the pressure is released after cooling to room temperature to obtain a resin composite. In this case, the sheet-like object may be overlapped on one side of the glass cloth, or on both sides of the glass cloth.
[0188] [Second Manufacturing Method]
[0189] The second production method includes a direct coating step of directly coating the glass cloth (C) with the cyclic polyolefin resin copolymer. By the direct coating, the cyclic polyolefin resin copolymer is impregnated into the glass cloth (C), and the cyclic polyolefin resin copolymer and the glass cloth (C) can be integrally composited.
[0190] The coating method of the cyclic polyolefin resin copolymer is not particularly limited, and examples thereof include comma coating, reverse coating, knife coating, dip coating, dip-nip, kiss coating, air knife coating, spin coating, roll coating, printing, dipping, slide coating, curtain coating, die coating, casting, extrusion coating, and the like.
[0191] <<Third Embodiment>>
[0192] When the linear thermal expansion coefficient of the resin sheet of the present invention is to be suppressed, it is preferable to use a laminate comprising the above-mentioned resin layer (A) and a resin layer (D) containing an amorphous resin (d) having a glass transition point of 100° C. or higher and a dielectric loss tangent of less than 0.02 at 12 GHz.
[0193] That is, the third embodiment of the present invention is a resin laminate, which comprises: a resin layer (A) containing a cyclic polyolefin resin copolymer having a crystalline melting peak temperature of less than 100°C, and a resin layer (D) containing an amorphous resin (d) having a glass transition point of more than 100°C and a dielectric loss tangent of less than 0.02 at 12 GHz.
[0194] Hereinafter, the resin sheet of the present embodiment may be referred to as a "resin laminate".
[0195] <Resin Layer (A)>
[0196] The resin layer (A) in this embodiment is the same as the resin layer (A) described in the above <<Resin layer (A)>>.
[0197] <Resin Layer (D)>
[0198] The resin layer (D) in this embodiment contains an amorphous resin (d) having a glass transition point of 100°C or higher and a dielectric loss tangent of less than 0.02 at 12 GHz. By using an amorphous resin, it is easy to laminate appropriately without peeling from the resin layer (A) containing a cyclic polyolefin resin copolymer having a large amount of amorphous components.
[0199] (Amorphous resin (d))
[0200] The glass transition point of the amorphous resin (d) is 100°C or more, preferably 120°C or more, and more preferably 130°C or more. In addition, it is preferably lower than 200°C, more preferably lower than 170°C, and more preferably lower than 150°C. By making the glass transition point of the amorphous resin (d) higher than the above lower limit, the heat resistance is improved, and the linear thermal expansion during heating and the dimensional change caused by the contraction during cooling can be suppressed. On the other hand, by making the glass transition point lower than the above upper limit, it is possible to laminate well without peeling from the resin layer (A) containing the cyclic polyolefin resin copolymer or lamination unevenness.
[0201] The glass transition point is measured at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC) in accordance with JIS K 7121 (2012).
[0202] The dielectric loss tangent of the amorphous resin (d) at 12 GHz in the resin layer (D) is preferably less than 0.02, more preferably less than 0.01. The smaller the dielectric loss tangent, the smaller the dielectric loss, so when a circuit substrate is made, the transmission efficiency and speed of the electrical signal can be obtained, which is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is 0 or more.
[0203] The non-crystalline resin (d) in the resin layer (D) is preferably at least one resin selected from the group consisting of alicyclic olefin polymers, polycarbonates, polyarylates, polysulfones, and copolymers thereof. Among them, alicyclic olefin polymers are more preferred from the viewpoint of low dielectric properties.
[0204] The aforementioned alicyclic olefin polymer is a polymer having a structural unit derived from an alicyclic olefin, and specifically refers to a polymer obtained by hydrogenating a ring-opening (co)polymer of an alicyclic olefin as needed, an addition (co)polymer of an alicyclic olefin, a random copolymer of an alicyclic olefin and an α-olefin such as ethylene and propylene, or a grafted modified product obtained by modifying the above (co)polymer with an unsaturated carboxylic acid, a derivative thereof, etc. Among these, a cyclic olefin copolymer (COC) obtained by addition polymerization of norbornene and ethylene units, and a cyclic olefin polymer (COP) obtained by ring-opening polymerization of norbornene or dicyclopentadiene and stabilization by hydrogenation can be appropriately used.
[0205] The aforementioned polycarbonate is a linear polymer containing a carbonate bond in the main chain, and is a polymer that can be obtained by reacting various dihydroxy diaryls by transesterification. Specifically, polycarbonate produced from 2,2-bis(4-hydroxyphenyl)propane (bisphenol A) and phosgene or diphenyl carbonate can be cited, but it is not limited thereto.
[0206] The aforementioned polyarylate is a condensation product of a dicarboxylic acid component and a dihydric phenol component. The glass transition point of the polyarylate can be adjusted by appropriately selecting the aforementioned dicarboxylic acid component and the dihydric phenol component. Specifically, polyarylate formed from terephthalic acid, isophthalic acid and bisphenol A can be cited, but it is not limited thereto.
[0207] The aforementioned polysulfone is a polymer characterized by having a sulfonyl group. Examples of the production method include copolymerization of olefins and sulfoxides, oxidation of polysulfide, and the like, but the method is not limited thereto.
[0208] The content ratio of the amorphous resin (d) in the resin layer (D) of the present embodiment is preferably 30% by mass or more, more preferably 50% by mass or more, and further preferably 70% by mass or more. The resin layer (D) can be formed only by the amorphous resin (d) (100% by mass). By making the content ratio of the amorphous resin (d) above the above range, it is expected that the heat resistance and the linear thermal expansion coefficient will be appropriately improved when stacked with the resin layer (A).
[0209] Furthermore, one kind of the resins listed above as the non-crystalline resin (d) may be used alone, or two or more kinds may be used in combination.
[0210] For the purpose of imparting functionality, in the resin layer (D) of the present embodiment, in addition to the aforementioned amorphous resin (d), other components may be appropriately mixed. Specifically, in order to improve the adhesion with the resin layer (A), a cyclic polyolefin resin copolymer identical to the resin layer (A) may be mixed, or in order to improve the bending resistance of the resin laminate of the present invention, a thermoplastic elastomer may be mixed. Furthermore, an ultraviolet light blocking agent, an antioxidant, a coupling agent, a plasticizer, a flame retardant, a colorant, a dispersant, an emulsifier, a low elasticity agent, a diluent, a defoaming agent, an ion capture agent, an inorganic filler, an organic filler, etc. may be optionally mixed.
[0211] <Structure of resin laminate>
[0212] The resin laminate of the present embodiment includes at least one resin layer (A) and at least one resin layer (D).
[0213] Therefore, it can be a two-layer structure of a resin layer (A) and a resin layer (D), or it can be a three-layer structure in which a resin layer (A) is configured on both sides of a resin layer (D), or a resin layer (D) is configured on both sides of a resin layer (A). It can also be a multilayer structure in which a resin layer (A) and a resin layer (D) are overlapped multiple times. In addition, a resin layer other than a resin layer (A) and (D) can be provided on a single side of a resin layer (A) and / or a resin layer (D). Specifically, an adhesive layer for improving the adhesion between resin layers, a colored resin layer for imparting visual recognition of a resin laminate, etc. can be provided.
[0214] Among the above, from the viewpoint of suppressing the warping of the resin laminate, it is preferred that the two outermost layers of the resin laminate are the resin layer (A), or the two outermost layers of the resin laminate are the resin layer (D). That is, it is preferred that the three-layer structure is configured with the resin layer (A) on both sides of the resin layer (D), the three-layer structure is configured with the resin layer (D) on both sides of the resin layer (A), the multi-layer structure is configured with the resin layer (A) and the resin layer (D) overlapping multiple times and the two outermost layers of the resin laminate are the resin layer (A), or the multi-layer structure is configured with the resin layer (A) and the resin layer (D) overlapping multiple times and the two outermost layers of the resin laminate are the resin layer (D).
[0215] When the resin layer (A) contains the modified cyclic polyolefin (a'), from the viewpoint of adhesion to the metal layer, preferably at least one outermost layer of the resin laminate is the resin layer (A), and more preferably both outermost layers of the resin laminate are the resin layer (A).
[0216] The thickness of the resin laminate of the present embodiment is not particularly limited, but is preferably about 10 to 200 μm in consideration of processability and practicality.
[0217] In addition, the thickness of the resin layer (A) of the resin laminate of the present embodiment is preferably 10% to 60% of the entire resin laminate, and the thickness of the resin layer (D) is preferably 40% to 90% of the entire resin laminate. By making the thickness of each resin layer within the above range, the heat resistance of the resin layer (D) is improved, and the effect of suppressing the linear thermal expansion coefficient can be appropriately demonstrated. It should be noted that, when the resin laminate has a plurality of the above-mentioned resin layers (A) and resin layers (D), it is preferable that the total value of the thickness of each layer is within the above range.
[0218] <Characteristics of Resin Laminate>
[0219] The dielectric loss tangent of the resin laminate of this embodiment at 12 GHz is preferably less than 0.005, more preferably less than 0.002. The lower the dielectric loss tangent, the smaller the dielectric loss, so when it is made into a circuit substrate, the transmission efficiency and speed of the electrical signal can be obtained, which is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is 0 or more.
[0220] In addition, the average linear thermal expansion coefficient of the resin laminate of the present embodiment is preferably 15 ppm / °C or more, more preferably 20 ppm / °C or more in the temperature range of 0°C to 100°C. In addition, it is preferably 115 ppm / °C or less, more preferably 100 ppm / °C or less. By making the linear thermal expansion coefficient of the resin laminate within the above range, the shrinkage of the molded product using the resin laminate can be suppressed, or when the resin laminate is used in the circuit substrate material application for electrical / electronic equipment, the unfavorable situation that the laminate curls or warps after lamination due to the difference in shrinkage rate with the metal layer such as copper foil can be improved.
[0221] <Method for producing resin laminate>
[0222] Hereinafter, a method for producing the resin laminate of the present embodiment will be described. However, the following description is an example of a method for producing the resin laminate of the present invention, and the resin laminate of the present invention is not limited to a resin laminate produced by the production method described below.
[0223] The resin laminate of the present embodiment can be produced, for example, by melt-mixing the cyclic polyolefin resin copolymer and other additives as the raw materials of the resin layer (A) using a single-screw or twin-screw extruder, and similarly melt-mixing the amorphous resin (d) and other additives as the raw materials of the resin layer (D), co-extruding them using a T-die, and rapidly cooling and solidifying them using a casting roll.
[0224] As a method for laminating the resin layer (A) and the resin layer (D), the lamination can be performed by coextrusion as described above, or the resin layer (A) and the resin layer (D) formed by each film and other layers can be laminated by lamination or heat pressing. In addition, during lamination, an adhesive layer can be provided in order to improve the adhesion between the resin layers.
[0225] <Application of resin laminate>
[0226] The resin laminate of this embodiment can be used as a copper foil laminate, a flexible printed substrate, a multilayer printed circuit substrate, a laminate for electrical / electronic circuits such as capacitors, a bottom filling material, a chip inter-fill for 3D-LSI, an insulating sheet, a heat dissipation substrate, etc., and a material for a circuit substrate, but is not limited to these.
[0227] <<Circuit board materials>>
[0228] The resin sheets according to the first to third embodiments of the present invention can be made into circuit board materials by laminating them with conductors.
[0229] As the conductor, a metal foil formed of a conductive metal such as copper or aluminum, an alloy containing these metals, or a metal layer formed by plating or sputtering can be used.
[0230] When used as a circuit board material for electric or electronic equipment, the thickness of the resin sheet is preferably 10 μm or more and 200 μm or less. In addition, the thickness of the conductor is preferably 0.2 μm or more and 70 μm or less.
[0231] The circuit board material of the present invention is characterized in that the dielectric loss tangent is sufficiently low.
[0232] The dielectric loss tangent of the circuit substrate material is preferably less than 0.01 at 12 GHz, and more preferably less than 0.008. The lower the dielectric loss tangent, the more efficient and high-speed transmission of electrical signals can be obtained when the circuit substrate is made, so it is preferred. The lower limit of the dielectric loss tangent is not particularly limited, as long as it is greater than 0.
[0233] <Method for producing circuit board material>
[0234] The circuit board material in the present invention can be produced, for example, by the following method.
[0235] After the conductors are stacked on the resin sheets of the first to third embodiments of the present invention, a circuit is formed using a photoresist or the like, and a required number of such layers are stacked.
[0236] The stacking of the resin sheet and the conductor can be a method of directly overlapping the conductive metal foil on the resin sheet, or a method of bonding the resin sheet and the conductive metal foil using an adhesive. In addition, it can be a method of forming a conductive metal layer by plating or sputtering, or these methods can be used in combination.
[0237] Example
[0238] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited in any way by these examples. The values of various manufacturing conditions and evaluation results in the following examples have the meaning of preferred values as the upper or lower limits in the embodiments of the present invention, and the preferred range can be the range limited by the combination of the values of the aforementioned upper or lower limits and the values of the following examples or the values of the examples.
[0239] In addition, in the following description, "part" means "part by mass".
[0240] <<Test Example 1: Physical properties and evaluation of cyclic polyolefin resin copolymer>>
[0241] In Test Example 1, physical properties of the following materials a-1 and a-2, which are examples of the cyclic polyolefin resin copolymer of the present invention, and the following material a-101 were measured and evaluated.
[0242] <Physical Property Measurement and Evaluation>
[0243] (1) Molecular weight (Mw)
[0244] ·Device: GPC HLC-832GPC / HT manufactured by Tosoh Corporation
[0245] Detector: MIRAN 1A infrared spectrophotometer (measurement wavelength, 3.42 μm)
[0246] Column: 3 AD806M / S manufactured by Showa Denko K.K. (For calibration of the column, monodisperse polystyrene manufactured by Tosoh Corporation (A500, A2500, F1, F2, F4, F10, F20, F40, F288, each 0.5 mg / ml solution) was measured, and the logarithmic values of the elution volume and the molecular weight were approximated by a cubic equation).
[0247] ·Measurement temperature: 135℃
[0248] Concentration: 20mg / 10mL
[0249] Injection volume: 0.2ml
[0250] Solvent: o-dichlorobenzene
[0251] Flow rate: 1.0ml / min
[0252] (2) Ratio of polymer blocks
[0253] [Measurement based on carbon NMR]
[0254] · Equipment: Bruker "AVANCE400 spectrometer"
[0255] Solvent: o-dichlorobenzene-h4 / p-dichlorobenzene-d4 mixed solvent
[0256] Concentration: 0.3g / 2.5mL
[0257] Determination: 13 C-NMR
[0258] Resonance frequency: 400MHz
[0259] Cumulative times: 3600
[0260] Flip angle: 45 degrees
[0261] Data acquisition time: 1.5 seconds
[0262] Pulse repetition time: 15 seconds
[0263] ·Measurement temperature: 100℃
[0264] · 1 H irradiation: fully decoupled
[0265] (3) Hydrogenation Levels of Hydrogenated Aromatic Vinyl Polymer Block Units and Hydrogenated Conjugated Diene Polymer Block Units
[0266] [Measurement by proton NMR]
[0267] · Equipment: Bruker "AVANCE400 spectrometer"
[0268] Solvent: Tetrachloroethane
[0269] Concentration: 0.045g / 1.0mL
[0270] Determination: 1 H-NMR
[0271] Resonance frequency: 400MHz
[0272] Flip angle: 45 degrees
[0273] Data acquisition time: 4 seconds
[0274] Pulse repetition time: 10 seconds
[0275] Cumulative times: 64
[0276] ·Measurement temperature: 80℃
[0277] · Hydrogenation level of hydrogenated aromatic vinyl polymer block unit: reduction rate of integrated value from 6.8 to 7.5 ppm
[0278] · Hydrogenation level of hydrogenated conjugated diene polymer block unit: reduction rate of integrated value from 5.7 to 6.4 ppm
[0279] (4) Modification rate of modified cyclic polyolefin
[0280] [Measurement by proton NMR]
[0281] · Device: AVANCE400 spectrometer manufactured by BRUKER
[0282] Solvent: Deuterated o-dichlorobenzene
[0283] Concentration: 20mg / 0.62mL
[0284] Determination: 1 H-NMR
[0285] Resonance frequency: 400MHz
[0286] Flip angle: 45 degrees
[0287] Data acquisition time: 4 seconds
[0288] Pulse repetition time: 10 seconds
[0289] Cumulative times: 64
[0290] ·Measurement temperature: 120℃
[0291] Modification rate of acid-modified cyclic polyolefin: reduction rate of integrated value from 3.42 to 3.94 ppm
[0292] (5) Transparency
[0293] A 2 mm thick, 4 cm x 8 cm flat plate was injection molded using SE-18D injection molding machine manufactured by Sumitomo Heavy Industries, Ltd. at a molding temperature of 220° C. and a mold temperature of 40° C. The haze of the plate was measured according to the method described in JIS K7105 (1981).
[0294] The measured HAZE value was used as an evaluation of transparency. The evaluation results are shown in Table 1. It should be noted that the lower the HAZE value, the better the transparency.
[0295] (6) Heat resistance
[0296] Three sheets obtained in (5) above were stacked, and the Vicat softening temperature was measured by the method described in JIS K 7206 (1999). The heat resistance was evaluated using the measured Vicat softening temperature. The evaluation results are shown in Table 1. It should be noted that the higher the Vicat softening temperature, the higher the heat resistance.
[0297] <Raw Materials>
[0298] a-1: As the cyclic polyolefin (a), "TEFABLOC (registered trademark) CPMC930" manufactured by Mitsubishi Chemical Corporation was used to prepare a cyclic polyolefin resin copolymer a-1.
[0299] Crystal melting peak temperature: 75℃
[0300] Dielectric loss tangent: 0.0003 (12GHz)
[0301] Density (ASTM D792): 0.94 g / cm 3
[0302] MFR (230°C, 2.16kg): 1g / 10min
[0303] ·Hydrogenated aromatic vinyl polymer block unit: Hydrogenated polystyrene with a content of 65 mol% and a hydrogenation level of 99.5% or more
[0304] ·Hydrogenated conjugated diene polymer block unit: Hydrogenated polybutadiene with a content of 35 mol% and a hydrogenation level of 99.5% or more
[0305] Block structure: Pentablock structure, total hydrogenation level: more than 99.5%
[0306] a-2: As the modified cyclic polyolefin (a'), "TEFABLOC (registered trademark) CP MC940AP" manufactured by Mitsubishi Chemical Corporation was used to prepare a cyclic polyolefin resin copolymer a-2.
[0307] Crystal melting peak temperature: 75℃
[0308] Dielectric loss tangent: 0.0009 (12GHz)
[0309] Density (ASTM D792): 0.94 g / cm 3
[0310] MFR (230°C, 2.16kg): 3g / 10min
[0311] ·Hydrogenated aromatic vinyl polymer block unit: Hydrogenated polystyrene with a content of 67 mol% and a hydrogenation level of 99.5% or more
[0312] ·Hydrogenated conjugated diene polymer block unit: Hydrogenated polybutadiene with a content of 33 mol% and a hydrogenation level of 99.5% or more
[0313] Block structure: Pentablock structure, total hydrogenation level: more than 99.5%
[0314] Maleic acid modification rate: 1.2% by mass
[0315] Mw: 68000
[0316] a-101: Tuftec M1943 manufactured by Asahi Kasei Corporation was used as a modified product of maleic acid of a hydrogenated styrene-butadiene block copolymer.
[0317] a-101 is a maleic acid-modified polyolefin. The aromatic vinyl polymer block unit of the polyolefin as a raw material is not hydrogenated and therefore does not have a crystal melting peak temperature.
[0318] [Table 1]
[0319]
[0320] <<Test Example 2>>
[0321] In Test Example 2, dielectric loss tangent, storage modulus, flex resistance, and haze were evaluated for the case where the resin sheet contained a thermoplastic resin and the case where the resin sheet did not contain a thermoplastic resin.
[0322] <Measurement method>
[0323] (1) Dielectric properties
[0324] The dielectric loss tangent in the in-plane direction of the resin sheet was measured using a cavity resonator method and evaluated according to the following criteria. The measurement frequency was set to 12 GHz.
[0325] [Evaluation criteria]
[0326] A (good): Dielectric loss tangent less than 0.005
[0327] B (bad): Dielectric loss tangent is 0.005 or more
[0328] (2) Storage modulus
[0329] The dynamic viscoelasticity of the resin sheet was measured under the following conditions using a viscoelasticity spectrometer DVA-200 (manufactured by IT Instruments & Controls Co., Ltd.) Based on the measurement results, the value of the storage modulus at 24° C. was defined as the storage modulus of each resin, and evaluation was performed according to the following criteria.
[0330] [Measurement conditions]
[0331] Vibration frequency: 10Hz
[0332] Strain: 0.1%
[0333] Heating rate: 3℃ / min
[0334] Measuring temperature: -50℃~200℃
[0335] [Evaluation criteria]
[0336] A (good): Storage modulus less than 2000 MPa
[0337] B (poor): Storage modulus is 2000 MPa or more
[0338] (3) Bending resistance
[0339] The folding strength of the resin sheet was measured using an MIT folding tester in accordance with JIS P8115 to evaluate the bending resistance.
[0340] [Measurement conditions]
[0341] Bending speed: 175 times / minute
[0342] Bending angle: left and right 135 degrees
[0343] Load: 9.8N
[0344] Test direction: film length direction (MD), width direction (TD)
[0345] [Evaluation criteria]
[0346] A (very good): Broken after bending more than 300 times
[0347] B (good): Broken after bending more than 10 times but less than 300 times
[0348] C (poor): Broken after less than 10 bends
[0349] (4) Haze
[0350] The total light transmittance and diffuse transmittance of the resin sheet were measured using a haze meter in accordance with JIS K 7105. The haze was calculated from the obtained total light transmittance and diffuse transmittance by the following formula, and evaluated based on the following criteria.
[0351] [Haze] (%) = [Diffuse transmittance] / [Total transmittance] × 100
[0352] [Evaluation criteria]
[0353] A (very good): haze is less than 5%
[0354] B (good): Haze is more than 5% and less than 10%
[0355] C (poor): Haze exceeds 10%
[0356] <Raw Materials>
[0357] [Cyclic polyolefin resin copolymer]
[0358] The cyclic polyolefin resin copolymers a-1 and a-2 described in <<Test Example 1>> were used.
[0359] [Thermoplastic resin]
[0360] b-1: hydrogenated styrene-butadiene-styrene block copolymer (SEBS), dielectric loss tangent (12 GHz) = 0.0004, storage modulus (24°C) = 6.2 MPa, density = 890 mg / cm 3
[0361] b-2: Linear low-density polyethylene (L-LDPE), dielectric loss tangent (12 GHz) = 0.0003, storage modulus (24°C) = 290 MPa, density = 920 mg / cm 3
[0362] b-3: Linear low-density polyethylene (L-LDPE), dielectric loss tangent (12 GHz) = 0.0003, storage modulus (24°C) = 190 MPa, density = 908 mg / cm 3
[0363] <Example 1>
[0364] A-1 as a cyclic polyolefin resin copolymer and b-1 as a thermoplastic resin were melt-kneaded using a single screw extruder, extruded using a T-die, cooled and solidified using a casting roll, and thus formed into a resin sheet A1-1 having a thickness of 100 μm. The storage modulus, dielectric properties, bending resistance, and haze of the obtained resin sheet A1-1 were evaluated. The results are shown in Table 2.
[0365] <Examples 2 to 4>
[0366] Resin sheets A1-2 to A1-4 were formed by the same method as in Example 1 except that the cyclic polyolefin resin copolymer and the thermoplastic resin were melt-kneaded according to the formulation described in Table 2. The storage modulus, dielectric properties, bending resistance, and haze of the obtained resin sheets A1-2 to A1-4 were evaluated. The results are shown in Table 2.
[0367] <Reference Example 1>
[0368] The cyclic polyolefin resin copolymer a-1 monomer was melt-kneaded using a single screw extruder, extruded using a T die, cooled and solidified using a casting roll, and thus formed into a resin sheet A101 having a thickness of 100 μm. The storage modulus, dielectric properties, bending resistance, and haze of the obtained sheet were evaluated. The results are shown in Table 2.
[0369] [Table 2]
[0370]
[0371] From Examples 1 to 4 and Reference Example 1 in Table 2 above, it can be confirmed that the resin sheet containing the cyclic polyolefin resin copolymer of the present invention has low dielectric properties.
[0372] In addition, Examples 1 to 4 show that by mixing a specific thermoplastic resin into the cyclic polyolefin resin copolymer, low dielectric properties can be maintained and bending resistance can be improved. When such a resin sheet is bent, it can prevent breakage and cracking, so it is easy to roll it up, punch it, etc., and it can also be expected to be used as a material for a flexible substrate (FPC).
[0373] <<Test Example 3>>
[0374] In Test Example 3, the dielectric loss tangent and the linear thermal expansion coefficient were evaluated in the case where the resin sheet and the glass cloth were composited and in the case where they were not composited.
[0375] <Measurement method>
[0376] (1) Dielectric properties
[0377] The dielectric loss tangent in the in-plane direction of the resin sheet was measured using a cavity resonator method and evaluated according to the following criteria. The measurement frequency was set to 12 GHz.
[0378] [Evaluation criteria]
[0379] A (good): Dielectric loss tangent less than 0.005
[0380] B (bad): Dielectric loss tangent is 0.005 or more
[0381] (2) Linear thermal expansion coefficient
[0382] A test piece having a width of 3 mm and a length of 10 mm was cut out from the resin sheet, and the linear thermal expansion coefficient of the test piece was measured in accordance with JIS K 7197 using TMA / SS7100 manufactured by Hitachi High-Tech Science Corporation, and evaluated according to the following criteria.
[0383] [evaluate]
[0384] A (good): The average linear thermal expansion coefficient at 0℃ to 100℃ is less than 65ppm / ℃
[0385] B (bad): The average linear thermal expansion coefficient at 0°C to 100°C is 65 ppm / °C or more
[0386] <Raw Materials>
[0387] [Cyclic polyolefin resin copolymer]
[0388] The cyclic polyolefin resin copolymer a-2 described in <<Test Example 1>> was used.
[0389] [Glass cloth]
[0390] c-1: quartz glass (manufactured by Shin-Etsu Chemical Co., Ltd., thickness: 50 μm, dielectric loss tangent: 0.0001 (10 GHz), linear thermal expansion coefficient: 0.5 ppm / °C)
[0391] <Example 5>
[0392] The cyclic polyolefin resin copolymer a-2 was melt-kneaded using an extruder to form a resin sheet A2 having a thickness of 100 μm. The resin sheet A2 and the glass cloth c-1 were cut into 10 cm squares, and two resin sheets A2 were stacked on both sides of the glass cloth c-1 in a manner to form the volume ratio in Table 3. The laminate was clamped between two smooth metal plates and hot-pressed at 200°C, 60 seconds, and a pressure of 20 MPa to obtain a resin composite A2-1. The dielectric properties and linear thermal expansion coefficient of the obtained resin composite A2-1 were evaluated. The results are shown in Table 3.
[0393] <Examples 6 to 7>
[0394] Resin composites A2-2 and A2-3 were prepared by the same method as in Example 5 except that the volume ratio of the cyclic polyolefin resin copolymer a-2 and the glass cloth c-1 was adjusted as shown in Table 3. Dielectric properties and linear thermal expansion coefficients of the obtained resin composites A2-2 and A2-3 were evaluated. The results are shown in Table 3.
[0395] <Reference Example 2>
[0396] The dielectric properties and linear thermal expansion coefficient of the resin sheet A2 were evaluated.
[0397] [Table 3]
[0398]
[0399] According to Examples 5 to 7 in Table 3 above, it can be confirmed that the composite of the cyclic polyolefin resin copolymer and glass cloth of the present invention can maintain low dielectric properties and reduce the linear thermal expansion coefficient. When such a resin composite is used as a circuit board material, for example, it can reduce dielectric loss and suppress curling and warping of the board caused by the difference in thermal expansion coefficient with the metal layer.
[0400] <<Test Example 4>>
[0401] In Test Example 4, the dielectric loss tangent and the linear thermal expansion coefficient were evaluated when the resin layer (A) containing the cyclic polyolefin resin copolymer and the resin layer (D) containing the amorphous resin (d) were laminated and when they were not laminated.
[0402] <Measurement method>
[0403] (1) Dielectric properties
[0404] The dielectric loss tangent of the resin laminate in the in-plane direction at 12 GHz was measured using a cavity resonator method and evaluated based on the following criteria.
[0405] [Evaluation criteria]
[0406] A (good): Dielectric loss tangent less than 0.005
[0407] B (bad): Dielectric loss tangent is 0.005 or more
[0408] (2) Linear thermal expansion coefficient
[0409] A test piece having a width of 3 mm and a length of 10 mm was cut out from the resin laminate, and the linear thermal expansion coefficient of the test piece was measured in accordance with JIS K 7197 using TMA / SS7100 manufactured by Hitachi High-Tech Science Corporation, and evaluated according to the following criteria.
[0410] [Evaluation criteria]
[0411] A (good): The average linear thermal expansion coefficient at 0℃ to 100℃ is less than 115ppm / ℃
[0412] B (bad): The average linear thermal expansion coefficient at 0°C to 100°C is 115 ppm / °C or more
[0413] <Raw Materials>
[0414] [Cyclic polyolefin resin copolymer]
[0415] The cyclic polyolefin resin copolymer a-2 described in <<Test Example 1>> was used.
[0416] [Amorphous resin]
[0417] d-1: alicyclic olefin copolymer (COC) obtained by polymerizing norbornene-ethylene, dielectric loss tangent = 0.0002 (12 GHz), Tg = 138°C
[0418] d-2: Polycarbonate, dielectric loss tangent = 0.0059 (12GHz), Tg = 145°C
[0419] d-3: Hydrogenated alicyclic olefin polymer (COP) obtained by ring-opening polymerization of cyclopentadiene, dielectric loss tangent = 0.0002 (12 GHz), Tg = 102°C
[0420] d-4: Low Tg alicyclic olefin copolymer (COC) obtained by polymerizing norbornene-ethylene, dielectric loss tangent = 0.0002 (12 GHz), Tg = 69°C
[0421] <Example 8>
[0422] Use single screw extruder to melt mix the cyclic polyolefin resin copolymer a-2 as resin layer (A) and the amorphous resin d-1 as resin layer (D) respectively, coextrude with T die so that front layer and back layer are resin layer (A), middle layer is resin layer (D), cool and solidify with cast roll, thus film-formed into the resin laminated body of thickness 100 μm. For the thickness of each layer, the discharge of each extruder is adjusted in the way that resin layer (A) / resin layer (D) / resin layer (A) becomes 1 / 8 / 1. Dielectric properties and linear thermal expansion coefficient are evaluated to the obtained resin laminated body. The results are shown in Table 4.
[0423] <Examples 9, 10, Reference Example 4>
[0424] A resin laminate was formed into a film by the same method as in Example 8 except that the resin layer (A) and the resin layer (D) were coextruded with the formulation and lamination ratio described in Table 4. The dielectric properties and linear thermal expansion coefficient of the obtained resin laminate were evaluated. The results are shown in Table 4.
[0425] <Reference Example 3>
[0426] The dielectric properties and the linear thermal expansion coefficient were evaluated for a sheet having a thickness of 100 μm obtained by melt-kneading the cyclic polyolefin resin copolymer a-2 using a single-screw extruder.
[0427] [Table 4]
[0428]
[0429] As shown in Examples 8 to 10 of Table 4 above, it is shown that by laminating the resin layer (D) containing a resin exhibiting a predetermined dielectric loss tangent and glass transition point as the amorphous resin (d) on the resin layer (A), the linear thermal expansion coefficient can be reduced while maintaining the dielectric properties of the cyclic polyolefin resin copolymer a-2. By using the resin laminate as, for example, an electrical and electronic circuit substrate material, the dielectric loss can be reduced, and the curling and warping of the substrate caused by the difference in thermal expansion coefficient with the metal layer can be suppressed.
Claims
1. A conductor bonding resin sheet, comprising at least a resin layer (A) and having a dielectric loss tangent of less than 0.002 at 12 GHz, wherein the resin layer (A) contains a cyclic polyolefin resin copolymer having a crystal melting peak temperature of less than 100° C. The content of the cyclic polyolefin resin copolymer in the resin component constituting the resin layer (A) is 50% by mass or more, The cyclic polyolefin resin copolymer is a cyclic polyolefin (a) comprising at least one hydrogenated aromatic vinyl polymer block unit and at least one hydrogenated conjugated diene polymer block unit, or a modified product of the cyclic polyolefin (a) obtained by using an unsaturated carboxylic acid and / or anhydride thereof. The content of the hydrogenated aromatic vinyl polymer block unit in the cyclic polyolefin (a) is 30 to 99 mol %, and the content of the hydrogenated conjugated diene polymer block unit is 1 to 70 mol %.
2. The conductor bonding resin sheet according to claim 1, in, The cyclic polyolefin resin copolymer has cyclohexane in a side chain of polyolefin.
3. The conductor bonding resin sheet according to claim 1 or 2, in, The hydrogenation level of the hydrogenated aromatic vinyl polymer block unit is 90% or more.
4. The conductor bonding resin sheet according to claim 1 or 2, in, The hydrogenation level of the hydrogenated conjugated diene polymer block unit is 95% or more.
5. The conductor bonding resin sheet according to claim 1 or 2, in, The resin layer (A) contains a thermoplastic resin (b), and the thermoplastic resin (b) is at least one selected from the group consisting of ethylene-based polymers, olefin-based thermoplastic elastomers, and styrene-based thermoplastic elastomers. 6 . The conductor bonding resin sheet according to claim 5 , which has a storage elastic modulus at 24° C. of less than 2000 MPa.
7. The conductor bonding resin sheet according to claim 1 or 2, in, The resin layer (A) is a composite containing a glass cloth (C).
8. The conductor bonding resin sheet according to claim 1 or 2, in, The resin sheet is a laminate including the resin layer (A) and the glass cloth (C).
9. The conductor bonding resin sheet according to claim 7, in, The dielectric loss tangent of the glass cloth (C) is less than 0.005 at 10 GHz.
10. The conductor bonding resin sheet according to claim 8, in, The dielectric loss tangent of the glass cloth (C) is less than 0.005 at 10 GHz.
11. The conductor bonding resin sheet according to claim 1 or 2, in, The resin sheet is a laminate including the resin layer (A) and a resin layer (D), wherein the resin layer (D) contains an amorphous resin (d) having a glass transition point of 100° C. or higher and a dielectric loss tangent of less than 0.02 at 12 GHz.
12. The conductor bonding resin sheet according to claim 11, in, The non-crystalline resin (d) is at least one resin selected from the group consisting of alicyclic olefin polymers, polycarbonates, polyarylates, polysulfones, and copolymers thereof.
13. The conductor bonding resin sheet according to claim 11, in, At least one outermost layer is a resin layer (A).
14. The conductor bonding resin sheet according to claim 1 or 2, which is used for a circuit board. 15 . A circuit board material comprising laminating the resin sheet according to claim 1 and a conductor.
Citation Information
Patent Citations
Low dielectric resin composition and circuit laminated board
JP2001006437A
Resin composition and object molded therefrom
WO2012033076A1
Cyclic olefin copolymer and cross-linked product thereof
WO2012046443A1
Terminal-modified vinyl alicyclic hydrocarbon polymer and manufacturing method of the same
JP2005239851A
Insulating material for electronic component
JP2011001473A