A radiation-resistant EPDM rubber composite material and preparation method thereof

By using carbon black, white carbon black, lead oxide and barium sulfate as reinforcement fillers, and two-dimensional graphene and boron nitride as radiation-resistant agents in ethylene propylene rubber, an excellent radiation-resistant and mechanical properties are prepared. Rubber composite materials solve the problem of difficult to take into account both radiation resistance and mechanical properties in the prior art, and achieve high performance maintenance in high radiation environments.

CN115232408BActive Publication Date: 2024-11-26NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210919111.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-02
Publication Date
2024-11-26
Estimated Expiration
2042-08-02

AI Technical Summary

Technical Problem

The existing EPDM radiation-resistant rubber has poor radiation resistance after increasing radiation-resistant fillers in high-energy radiation environments, and poor aging resistance after reduction, resulting in a decrease in mechanical properties, making it difficult to ensure excellent radiation and mechanical properties at the same time.

Method used

Carbon black, white carbon black, lead oxide and barium sulfate as reinforced fillers, two-dimensional graphene and boron nitride as radiation anti-radiant agents, and ethylene propylene ternary rubber composite material made by high-temperature vulcanization, combining additives and vulcanizing agents The preparation was carried out to form a rubber composite material with excellent radiation resistance.

Benefits of technology

It has achieved the maintenance of tensile strength, elongation and rebound performance in a high radiation environment, the retention rate of radiation resistance and mechanical properties reaching more than 90%, and has excellent anti-irradiation aging and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003776877900000061
    Figure BDA0003776877900000061
  • Figure BDA0003776877900000071
    Figure BDA0003776877900000071
Patent Text Reader

Abstract

The present invention belongs to the technical field of rubber composite materials, and specifically relates to a radiation-resistant EPDM rubber composite material and a preparation method thereof. The rubber composite material is made of EPDM rubber, reinforcing filler, anti-radiation agent, auxiliary agent and vulcanizing agent by high temperature vulcanization; wherein the reinforcing filler is composed of carbon black, white carbon black, lead oxide and barium sulfate according to a weight ratio of 3:1:1:0.6; the anti-radiation agent is composed of boron nitride and graphene according to a weight ratio of 10:3; based on 100 parts by weight of EPDM rubber, the amount of reinforcing filler is 30 to 40 parts by weight, the amount of anti-radiation agent is 13 to 20 parts by weight, the amount of auxiliary agent is 15 to 25 parts by weight, and the amount of vulcanizing agent is 2.5 to 4 parts by weight. The EPDM rubber composite material prepared by the present invention has excellent mechanical properties while taking into account anti-radiation properties. After irradiation, the retention rate of its tensile strength and rebound rate performance is ≥90%, and it has excellent anti-radiation aging performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radiation-resistant rubber composite materials, and in particular relates to a radiation-resistant ethylene propylene diene monomer rubber composite material and a preparation method thereof. Background Art

[0002] Radiation-resistant rubber is a special rubber that can maintain its original physical properties under γ and β ray radiation. It can not only play a sealing role, but also resist the erosion of high-energy rays. It has broad application prospects in high-energy radiation environments such as nuclear reactors, nuclear power systems, aerospace vehicles, chemical industry, and medical treatment.

[0003] With the rapid development of nuclear power plants and space technology in my country, more and more rubber products are used in nuclear reactor devices, aerospace devices, medical radiation protection products and protective clothing. Due to the interaction between high-energy radiation particles and polymer materials, rubber materials are ionized and activated, resulting in changes in the mechanical properties of rubber materials, which will cause the performance of rubber products to be damaged to varying degrees. Therefore, higher requirements are placed on the radiation resistance of rubber products. The existing EPDM radiation-resistant rubber has poor radiation-resistant performance as the amount of radiation-resistant filler increases, and the tensile strength and resilience of the rubber deteriorate after radiation degradation. When the amount of radiation-resistant filler is reduced, the radiation resistance and aging resistance are poor, and the stability decreases. Therefore, it is of great significance to effectively ensure the mechanical properties while having excellent radiation resistance. Summary of the invention

[0004] In order to solve the above problems, the present invention proposes a radiation-resistant EPDM rubber composite material and a preparation method thereof, taking EPDM rubber as a material matrix, selecting carbon black, white carbon black, lead oxide and barium sulfate as reinforcing fillers, and two-dimensional graphene and boron nitride as radiation-resistant agents, to produce an EPDM rubber composite material with excellent radiation-resistant performance.

[0005] One of the purposes of the present invention is to provide a radiation-resistant EPDM rubber composite material, wherein the rubber composite material is made of EPDM rubber, a reinforcing filler, an anti-radiation agent, an additive and a vulcanizing agent through high-temperature vulcanization; wherein the reinforcing filler is composed of carbon black, white carbon black, lead oxide and barium sulfate in a weight ratio of 3:1:1:0.6; the anti-radiation agent is composed of boron nitride and graphene in a weight ratio of 10:3;

[0006] Based on 100 parts by weight of EPDM rubber, the amount of the reinforcing filler is 30 to 40 parts by weight, the amount of the anti-radiation agent is 13 to 20 parts by weight, the amount of the auxiliary agent is 15 to 25 parts by weight, and the amount of the vulcanizing agent is 2.5 to 4 parts by weight.

[0007] Preferably, the EPDM rubber is a polymer of ethylene and propylene, and the ethylene content of the EPDM rubber is 60% and the propylene content is 40%.

[0008] Preferably, the carbon black is N550 carbon black with a particle size of 25 to 30 μm; the white carbon black is fumed white carbon black with a particle size of 10 to 50 nm and a specific surface area of ​​200 to 300 m 2 / g.

[0009] Preferably, the auxiliary agents are an activator, an antioxidant and a softener, the activator is zinc oxide and stearic acid, the antioxidant is antioxidant DPPD and CTU, and the softener is paraffin oil 2280.

[0010] Preferably, the vulcanizing agent is dicumyl peroxide and a co-vulcanizing agent, and the co-vulcanizing agent is tetramethylthiuram disulfide.

[0011] Preferably, based on 100 parts by weight of rubber, the amount of zinc oxide is 5 to 8 parts by weight, the amount of stearic acid is 1 to 3 parts by weight, the amount of antioxidant DPPD is 0.5 to 1 part by weight, the amount of antioxidant CTU is 0.5 to 1 part by weight, the amount of paraffin oil 2280 is 2 to 3 parts by weight, the amount of diisopropylbenzene peroxide is 2 to 3 parts by weight, and the amount of tetramethylthiuram disulfide is 0.5 to 1 part by weight.

[0012] The second object of the present invention is to provide a method for preparing the above-mentioned radiation EPDM rubber composite material, comprising the following steps:

[0013] Step 1, weigh each raw material component according to proportion;

[0014] Step 2, plasticating and mixing: adding the EPDM raw rubber into an internal mixer for plasticating for 2 to 3 minutes, adding the auxiliary agent, reinforcing filler and anti-radiation agent in sequence and mixing for 10 to 15 minutes to obtain a mixed rubber;

[0015] Step 3, the rubber mix obtained in step 2 is placed in an open mill for 1 to 2 minutes, and then the accelerator and the vulcanizing agent are added. After the accelerator and the vulcanizing agent are completely mixed into the rubber material, thin pass for 2 to 3 minutes. According to the requirements of the sample, the rubber mix is ​​pressed into the required thickness, and the sheet is placed in a flat vulcanizer for vulcanization. After the vulcanization is completed, the mold is opened to take out the cut piece.

[0016] Preferably, in step 3, the vulcanization pressure is 10-15 MPa, the temperature is 168-175° C., and the time is 400 s.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention uses carbon black, white carbon black, lead oxide and barium sulfate as reinforcing fillers, and two-dimensional graphene and boron nitride as anti-radiation agents, to develop an EPDM rubber composite material with excellent mechanical properties and radiation resistance. The radiation-resistant EPDM rubber performance indicators meet the following requirements: tensile strength ≥13MPa, elongation ≥600%, brittle temperature ≤-50°C without cracking, and Shore A hardness 55±3. After irradiation, the final performance indicators meet the following requirements: the retention rates of tensile strength, elongation and rebound performance are all ≥65%, and the retention rates of tensile strength and rebound performance are ≥90%. The material has excellent radiation aging resistance and mechanical properties. DETAILED DESCRIPTION

[0019] The present invention is described in detail below in conjunction with specific embodiments, but it should be understood that the scope of protection of the present invention is not limited by the specific embodiments. The experimental methods in the following examples where specific conditions are not specified are usually operated under conventional conditions, and the sources of the unspecified experimental materials are all commercially available. Since they do not involve the invention, the steps are not described in detail.

[0020] Example 1

[0021] A radiation-resistant EPDM rubber composite material, wherein the rubber composite material is made of EPDM rubber, a reinforcing filler, an anti-radiation agent, an antioxidant, a softener and an additive through high-temperature vulcanization; wherein the reinforcing filler is composed of carbon black, white carbon black, lead oxide and barium sulfate in a weight ratio of 3:1:1:0.6; and the anti-radiation agent is composed of boron nitride and graphene in a weight ratio of 10:3;

[0022] Formulation of radiation resistant EPDM composites:

[0023] 600g EPDM rubber, reinforcing filler: 90g N550 carbon black, 30g fumed silica, 30g barium sulfate, 18g lead oxide, anti-radiation agent: 60g boron nitride, 18g graphene, antioxidant: antioxidant DPPD 3.0g, antioxidant CTU 3.0g, activator: zinc oxide 30g, stearic acid 6g, softener: paraffin oil 2280: 60g, vulcanizing agent: diisopropyl peroxide DCP: 6.0g, accelerator: tetramethylthiuram disulfide TMTD: 3g.

[0024] The method for preparing the radiation-resistant EPDM rubber composite material comprises the following steps:

[0025] Step 1, weigh each raw material component according to the proportion, and dry each raw material component in an oven at 120°C for 2h;

[0026] Step 2, plasticating and mixing: adding the EPDM raw rubber into an internal mixer for plasticating for 2 to 3 minutes, and sequentially adding an activator, an antioxidant, a reinforcing filler, an anti-radiation agent and a softener for internal mixing for 10 to 15 minutes to obtain a mixed rubber;

[0027] Step 3, the rubber mix obtained in step 2 is placed in an open mill for 1 to 2 minutes, and then the accelerator and the vulcanizing agent are added. After the accelerator and the vulcanizing agent are completely mixed into the rubber material, thin pass for 2 to 3 minutes. According to the sample requirements, the rubber mix is ​​pressed into the required thickness, and the sheet is placed in a flat vulcanizer for vulcanization. The vulcanization pressure is 13MPa, the temperature is 172°C, and the time is 400s. After the vulcanization is completed, the mold is opened to take out the cut piece.

[0028] Example 2

[0029] Basically the same as Example 1, except that:

[0030] Formulation of radiation resistant EPDM composites:

[0031] 600g EPDM rubber, reinforcing filler: 108g N550 carbon black, 36g fumed silica, 36g barium sulfate, 21.6g lead oxide, anti-radiation agent: 60g boron nitride, 18g graphene, antioxidant: 4.5g DPPD, 4.5g CTU, activator: 30g zinc oxide, 6g stearic acid, softener: paraffin oil 2280: 90g, vulcanizing agent: DCP: 6.0g, accelerator: tetramethylthiuram disulfide TMTD: 3g.

[0032] The vulcanization pressure is 15 MPa, the temperature is 168° C., and the time is 400 s.

[0033] Example 3

[0034] Basically the same as Example 1, except that:

[0035] Formulation of radiation resistant EPDM composites:

[0036] 600g EPDM rubber, reinforcing filler: 90g N550 carbon black, 30g fumed silica, 30g barium sulfate, 18g lead oxide, anti-radiation agent: 90g boron nitride, 27g graphene, antioxidant: 4.5g DPPD, 4.5g CTU, activator: 30g zinc oxide, 6g stearic acid, softener: paraffin oil 2280: 120g, vulcanizing agent: DCP: 6.0g, accelerator: tetramethylthiuram disulfide TMTD: 3g.

[0037] The vulcanization pressure is 10 MPa, the temperature is 175° C., and the time is 400 s.

[0038] Example 4

[0039] Basically the same as Example 1, except that:

[0040] Formulation of radiation resistant EPDM composites:

[0041] 600g EPDM rubber, reinforcing filler: 108g N550 carbon black, 36g fumed silica, 36g barium sulfate, 21.6g lead oxide, anti-radiation agent: 90g boron nitride, 27g graphene, antioxidant: 4.5g DPPD, 4.5g CTU, activator: 30g zinc oxide, 12g stearic acid, softener: paraffin oil 2280: 90g, vulcanizing agent: DCP: 9.0g, accelerator: tetramethylthiuram disulfide TMTD: 6.0g.

[0042] Comparative Example 1

[0043] The method is basically the same as Example 1, except that the reinforcing filler in the formula of the radiation-resistant EPDM rubber composite material is 90 g of N550 carbon black, 30 g of barium sulfate, and 18 g of lead oxide.

[0044] Comparative Example 2

[0045] The method is basically the same as Example 1, except that the reinforcing filler in the formula of the radiation-resistant EPDM rubber composite material is 90g of N550 carbon black and 30g of fumed silica.

[0046] Comparative Example 3

[0047] The method is basically the same as Example 1, except that the reinforcing filler in the formula of the radiation-resistant EPDM rubber composite material is 90 g of N550 carbon black.

[0048] Comparative Example 4

[0049] The method is basically the same as Example 1, except that the radiation-resistant agent in the formula of the radiation-resistant EPDM rubber composite material is only 60g of boron nitride.

[0050] Comparative Example 5

[0051] The method is basically the same as Example 1, except that the radiation-resistant agent in the formula of the radiation-resistant EPDM rubber composite material is only 18g of graphene.

[0052] The test method is as follows:

[0053] The EPDM rubber composite materials prepared in Example 1 and Comparative Examples 1 to 4 were cut into samples by a dumbbell cutter, and performance tests were performed according to GB / T528-2009. Each group of samples had at least 5 samples, and the average value was taken. The performance after the test was as follows:

[0054] Table 1 Rubber composite material properties of Example 1 and Comparative Examples 1 to 4

[0055]

[0056]

[0057] As can be seen from Table 1, the tensile strength, elongation at break and rebound performance of the fluorosilicone rubber composite material prepared by the present invention are significantly better than those of Comparative Examples 1 to 3. The performance indicators of Example 1 and Comparative Example 5 meet the requirements of tensile strength ≥13MPa, elongation ≥600%, brittle temperature ≤-50°C without cracking, and Shore A hardness of 55±3. The tensile strength, elongation at break and rebound of Comparative Example 4 using the anti-radiation agent alone are worse than those of Example 1 and Comparative Example 5. This is because graphene, as an anti-radiation agent, also has a certain reinforcing effect on the fluorosilicone rubber composite material.

[0058] The EPDM rubber composite materials prepared in Example 1 and Comparative Examples 4-5 were irradiated with a cumulative dose of 4×10 7 After rad irradiation aging, its performance is shown in Table 2.

[0059] Table 2 Comparison of radiation resistance performance between Example 1 and Comparative Examples 4 to 5

[0060] Tensile strength(MPa) Elongation at break (%) Rebound rate (%) Example 1 15 467 57 Comparative Example 4 6 345 30 Comparative Example 5 8 390 36

[0061] It can be seen from Table 1 and Table 2 that after irradiation, the tensile strength of Example 1 increases. This may be because after irradiation, the degree of crosslinking of the EPDM rubber composite material of Example 1 becomes larger, thereby increasing the tensile strength and reducing the elongation at break and the rebound rate. When a single boron nitride anti-radiation agent is added, such as in Comparative Example 4, the tensile strength decreases, and the elongation at break and the rebound rate are both less than 65%. When a single graphene anti-radiation agent is added, such as in Comparative Example 5, the tensile strength is greater than 65%, and the elongation at break and the rebound rate are both less than 65%. This is because graphene, as an anti-radiation agent, also has a certain reinforcing effect on the fluorosilicone rubber composite material. Only when boron nitride and graphene anti-radiation agents are added at the same time, the final performance indicators meet the retention rates of tensile strength, elongation, and rebound performance of ≥65%, and the retention rates of tensile strength and rebound performance are ≥90%.

[0062] From the above, it can be seen that the radiation-resistant EPDM rubber composite material prepared by the present invention selects EPDM with excellent electrical insulation, ozone aging resistance, heat aging resistance, weathering aging resistance and cold resistance as the material matrix, uses carbon black, white carbon black, lead oxide and barium sulfate as reinforcing fillers, and two-dimensional graphene and boron nitride as radiation-resistant agents to develop a fluorosilicone composite material with excellent radiation-resistant performance, thereby significantly improving the various properties of fluorosilicone rubber, and its tensile strength is ≥13MPa, elongation is ≥600%, brittle temperature is ≤-50℃ without cracking, and Shao A hardness is 55±3. When boron nitride and graphene radiation-resistant agents are added at the same time, after irradiation, the final performance indicators meet the retention rate of tensile strength, elongation and rebound performance of ≥65%, and the retention rate of tensile strength and rebound performance is ≥90%. It has excellent mechanical properties while taking into account radiation aging resistance. This new radiation-resistant fluorosilicone rubber composite material has broad application prospects in high radiation environments.

[0063] It should be noted that, when the present invention involves a numerical range, any numerical value within the numerical range is feasible. In order to avoid redundancy, the present invention only describes the preferred embodiments, but those skilled in the art may make other changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0064] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A radiation-resistant EPDM rubber composite material, It is characterized in that The rubber composite material is made of EPDM rubber, reinforcing filler, anti-radiation agent, additive and vulcanizing agent through high temperature vulcanization; wherein the reinforcing filler is composed of carbon black, white carbon black, lead oxide and barium sulfate in a weight ratio of 3:1:1:0.6; the anti-radiation agent is composed of boron nitride and graphene in a weight ratio of 10:3; Based on 100 parts by weight of rubber, the amount of N550 carbon black is 15 parts, the amount of fumed silica is 5 parts, the amount of barium sulfate is 5 parts, the amount of lead oxide is 3 parts, the amount of boron nitride is 10 parts, the amount of graphene is 3 parts, the amount of zinc oxide is 5 parts by weight, the amount of stearic acid is 1 part by weight, the amount of antioxidant DPPD is 0.5 parts by weight, the amount of antioxidant CTU is 0.5 parts by weight, the amount of paraffin oil 2280 is 10 parts by weight, the amount of diisopropylbenzene peroxide is 1 part by weight, and the amount of tetramethylthiuram disulfide is 0.5 parts by weight; The method for preparing the radiation-resistant EPDM rubber composite material comprises the following steps: Step 1, weigh each raw material component according to proportion; Step 2, plasticating and mixing: adding the EPDM raw rubber into an internal mixer for plasticating for 2 to 3 minutes, adding the auxiliary agent, reinforcing filler and anti-radiation agent in sequence and mixing for 10 to 15 minutes to obtain a mixed rubber; Step 3, placing the rubber mix obtained in step 2 in an open mill for 1 to 2 minutes, then adding the accelerator and the vulcanizing agent, and after the accelerator and the vulcanizing agent are completely mixed into the rubber material, thinning for 2 to 3 minutes, and pressing the rubber mix to the required thickness according to the sample requirements. After the sheet is removed, it is placed in a flat vulcanizer for vulcanization. After the vulcanization is completed, the mold is opened to take out the cut piece; the vulcanization pressure is 13MPa, the temperature is 172°C, and the time is 400s.

2. The radiation-resistant EPDM rubber composite material according to claim 1, It is characterized in that The EPDM rubber is a polymer of ethylene and propylene, and the ethylene content of the EPDM rubber is 60% and the propylene content is 40%.

3. The radiation-resistant EPDM rubber composite material according to claim 1, It is characterized in that The particle size of N550 carbon black is 25-30 μm; the particle size of fumed silica is 10-50 nm, and the specific surface area is 200-300 m 2 / g.