Moisture-curable network silicone polymer and its use

Through the combination of vinyl-terminated and hydride-terminated polyorganosiloxane and the C-C-C bond structure, the problem of poor oil resistance of silicone polymers at high temperatures is solved, and efficient moisture curing and thermal stability are achieved, which is suitable for automobiles. Sealing and Adhesives.

CN115244108BActive Publication Date: 2024-10-29HENKEL KGAA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202080064255.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-16
Publication Date
2024-10-29
Estimated Expiration
2040-12-16

AI Technical Summary

Technical Problem

Existing moisture-curable silicone polymers have poor oil resistance at high temperatures and are prone to 'end group tail bite' or 'depolymerization' reactions, leading to degradation and viscosity changes. They cannot effectively resist acidic environments, and their curing rates are slow and difficult to Meet the needs of industrial applications.

Method used

Using a combination of vinyl-terminated and hydride-terminated polyorganosiloxane, through a C-C-C bond structure and a hydrosilylation catalyst, an organosilicon polymer with a network structure is prepared to improve its thermal stability and curing rate, and in wet conditions The cross-linking reaction is carried out in the presence of a curing catalyst.

Benefits of technology

Significantly improves the oil resistance and thermal stability of silicone polymers at 150°C, provides excellent initial wet strength and rapid curing characteristics, can maintain performance at high temperatures and in oil, and is suitable for automotive sealing and adhesive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115244108B_ABST
    Figure CN115244108B_ABST
Patent Text Reader

Abstract

The present invention provides a moisture-curable network silicone polymer and a composition thereof, which has improved resistance to automotive oil at high temperature. The network silicone polymer contains terminal moisture-curable functional groups and a partially cross-linked structure, wherein the partially cross-linked structure contains C-C-C bonds, which separate the siloxane main chain from the moisture-curable functional groups and prevent thermal decomposition of the siloxane main chain.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to moisture curable network silicone polymers and compositions thereof. The curable network silicone polymers and compositions provide resistance to petroleum oil and heat at elevated temperatures and are particularly suitable as silicone room temperature vulcanizing sealants and adhesives for automotive gaskets. Background Art

[0002] Curable organosilicon polymers and compositions can be used as adhesives, sealants, release coatings, conformal coatings, potting compounds, encapsulants, etc. in a wide range of applications, including automotive, construction, highway, electronic devices and packaging components, appliance assembly and consumer uses. Typically, curable organosilicon polymers and compositions for these applications have been specially prepared to provide strength, toughness, cure speed, modulus, elongation, high temperature resistance and high humidity resistance. For example, curable organosilicon polymers and compositions can be formed into gaskets, which are widely used in the automotive industry. In use, the organosilicon composition is subjected to various conditions and must continue to function without compromising integrity. One such condition includes exposure to engine oil at elevated temperatures.

[0003] Oil resistant silicone compositions as room temperature vulcanizing (RTV) sealants are described in U.S. Patent Nos. 4,514,529, 4,673,750, 4,735,979 and 4,847,396 and International Publication No. WO9319130. One disadvantage of RTV silicone compositions is their slow cure rate, which is commercially unacceptable for certain applications, such as sealing electronic modules, where mass production may depend on the cure rate. Therefore, silicone compositions with improved cure rates are desired. In addition, specific grades of metal oxides and / or fiberized blast furnace slag fibers are added to silicone compositions to impart oil resistance to elastomeric products, as described in European Patent Publication No. EP0572148 and U.S. Patent Nos. 5,082,886 and 4,052,357. Such additions increase the complexity of the process and increase costs.

[0004] While many technologies in the art provide solutions for silicone polymers and compositions, moisture-curable silicone polymers have poor petroleum resistance at elevated temperatures due to a phenomenon known in the art as "end group backbiting," "backbiting," or "unzipping" reactions. Little work has been done to improve oil resistance by modifying the "end group structure" of silicone polymers. Therefore, there is a need in the art for silicone polymers that undergo efficient moisture curing without the formation of corrosive acid byproducts; while providing oil resistance at elevated temperatures, avoiding the use of waste fillers, and preventing degradation of the intrinsic silicone backbone due to backbiting reactions. The present invention meets this need. Summary of the invention

[0005] The present invention provides moisture-curable reticulated silicone polymers and compositions thereof for sealing and adhering flanges in automotive powertrains and heating, ventilation and air conditioning (HVAC). In use, the cured silicone compositions of the present invention can be exposed to various conditions, including high temperatures, automotive oils, acids, and continue to function without compromising integrity. One such condition includes exposure to engine oil at elevated temperatures.

[0006] One aspect of the present invention relates to an organosilicon polymer prepared as follows:

[0007] (i) from about 10 to about 98% of a vinyl terminated polyorganosiloxane having a weight average molecular weight greater than about 1,000 g / mol, preferably greater than about 10,000 g / mol;

[0008] (iii) from about 1 to about 20% of a hydride terminated polyorganosiloxane having a weight average molecular weight of less than about 100,000 g / mol, preferably less than about 10,000 g / mol;

[0009] (ii) from about 0.001 to about 20% of a vinyl or hydride (SiH) multifunctional organic compound, and (iv) from about 0.00001 to about 5% of a hydrosilylation catalyst,

[0010] wherein the molar ratio of vinyl functional groups to hydride functional groups is from about 0.1 to 0.8; and

[0011] The weight average molecular weight of the organosilicon polymer is about 10,000 to 3,000,000 g / mol, preferably about 100,000 to 500,000 g / mol.

[0012] Other aspects of the present invention relate to a moisture-curable silicone polymer, which is composed of (A) the silicone polymer having excess hydride functional groups and (B) a capped vinyl functional silane CH2=CH-SiYn R 3-n The reaction product is prepared by

[0013] wherein Y is alkoxy, aryloxy, acetoxy, oxime, alkenyloxy, amino, α-hydroxycarboxylic acid amide (—OCR'2CONR"2), α-hydroxycarboxylic acid ester (—OCR'2COOR"), H, OH, halogen, or a combination thereof; n=1, 2, or 3; and R, R', and R" are each independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl, or a combination thereof; and

[0014] wherein the ratio of vinyl functional groups in the (B) capped vinyl functional silane to hydride functional groups in the (A) organosilicon polymer is about 1 to 1.5.

[0015] Another aspect of the present invention relates to a moisture curing composition comprising

[0016] (1) from about 10 to about 90% of the above-mentioned moisture-curable silicone polymer;

[0017] (2) from about 0.00001 to about 5% of a moisture cure catalyst; and

[0018] (3) Optionally, from about 5 to about 90% of a finely divided inorganic filler or mixture of fillers. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The viscosity curves of Example 2 (C) (triangular points) and Example 6 (square points) are shown.

[0020] Figure 2 These are the GPC chromatograms of Example 2 (C) (straight line) and Example 6 (dashed line). DETAILED DESCRIPTION

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those of ordinary skill in the art. In the event of conflict, this document (including definitions) shall prevail. Although those similar or equivalent to the methods and materials described herein can be used in the practice or testing of the present disclosure, preferred methods and materials are described below. All publications, patent applications, patents and other references mentioned herein are incorporated herein by reference in their entirety. The materials, methods and examples disclosed herein are illustrative only and are not intended to be restrictive.

[0022] As used herein, the term "comprising" may include the embodiments "consisting of" and "consisting essentially of." As used herein, the terms "comprising," "including," "having," "has," "may," "containing," and variations thereof are intended to be open-ended transitional phrases, terms, or words that require the presence of the named ingredients / steps and allow for the presence of other ingredients / steps. However, such descriptions should be interpreted as also describing a composition or method as "consisting of" and "consisting essentially of the listed ingredients / steps," which only allow for the presence of the recited ingredients / steps and any impurities that may result therefrom, and exclude other ingredients / steps.

[0023] The numerical values ​​herein, particularly as they relate to polymers or polymer compositions, reflect average values ​​for a composition that may contain individual polymers of varying characteristics. Furthermore, unless otherwise indicated, numerical values ​​should be understood to include values ​​that are the same when reduced to the same number of significant figures and values ​​that differ from the stated value by less than the experimental error of routine measurement techniques of the type described in this application for determining the value.

[0024] All ranges disclosed herein include the listed endpoints and can be independently combined (for example, the range of "2 to 10" includes the endpoints 2 and 10 and all intermediate values). The endpoints and any values ​​of the ranges disclosed herein are not limited to the exact ranges or values; they are imprecise enough to include values ​​approximating these ranges and / or values. As used herein, approximate language can be applied to modify any quantitative representation that can vary and does not result in a change in the basic function associated with it. Therefore, in some cases, the value modified by one or more terms (such as "about") may not be limited to the exact value specified. In at least some cases, the approximate language may correspond to the precision of the instrument used to measure the value. The modifier "about" should also be considered to disclose the range defined by the absolute values ​​of the two endpoints. For example, the expression "about 2 to about 4" also discloses the range "2 to 4". The term "about" can refer to plus or minus 10% of the indicated number. For example, "about 10%" can indicate a range of 9% to 11%, and "about 1" can mean 0.9-1.1. Other meanings of "about" may be apparent from the context, such as rounding, so that, for example, "about 1" may also mean 0.5 to 1.4.

[0025] As used herein, a polymer or oligomer is a macromolecule composed of monomer units equal to or greater than about one monomer unit.Polymer and oligomer, or polymeric and oligomeric are used interchangeably in the present invention.

[0026] As used herein, the term "alkyl" refers to a monovalent linear, cyclic or branched moiety containing C1 to C24 carbons and containing only single bonds between carbon atoms in the moiety, and includes, for example, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, heptyl, 2,4,4-trimethylpentyl, 2-ethylhexyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-hexadecyl and n-octadecyl.

[0027] As used herein, the term "aryl" refers to a monovalent unsaturated aromatic carbocyclic group of 6 to 24 carbon atoms having a single ring (e.g., phenyl) or multiple condensed (fused) rings, wherein at least one ring is aromatic (e.g., naphthyl, dihydrophenanthryl, fluorenyl or anthracenyl). Preferred examples include phenyl, methylphenyl, ethylphenyl, methylnaphthyl, ethylnaphthyl, etc.

[0028] As used herein, the term "alkoxy" refers to the group -OR, wherein R is alkyl as defined above.

[0029] As used herein, the above groups may be further substituted or unsubstituted. When substituted, the hydrogen atoms on the group are replaced by one or more substituents, and the one or more substituents are one or more groups independently selected from the following: alkyl, alkenyl, alkynyl, cycloalkyl, cycloalkenyl, cycloalkynyl, aryl, heteroaryl, heteroalicyclic, aralkyl, heteroaralkyl, (heteroalicyclic) alkyl, hydroxy, protected hydroxy, alkoxy, aryloxy, acyl, ester, sulfhydryl, alkylthio, arylthio, cyano, halogen, carbonyl, thiocarbonyl, O-carbamoyl, N-carbamoyl The invention also includes aryl, cycloalkyl, cycloalkyl, cycloalkenyl, cycloalkynyl, and heterocyclic groups.

[0030] The term "moisture cure" herein refers to the hardening or vulcanization of the curable portion of a material or polymer by condensation crosslinking of terminal functional groups of polymer chains induced by water or moisture in the air in the presence of a moisture curing catalyst.

[0031] The term "organosilicon polymer" herein refers to a siloxane polymer, a polyorganosiloxane, or a polydiorganosiloxane, such as polydimethylsiloxane (PDMS).

[0032] The present invention provides the art with a class of novel network silicone polymers containing CCC bonds in the backbone and at branching sites or crosslinking points in the backbone. The network silicone polymers containing CCC bonds provide improved protection against tail biting and depolymerization reactions. The network silicone polymers can be terminated with functional groups that can undergo further moisture curing.

[0033] Silicone polymers terminated with silanol and / or alkoxysilyl groups undergo moisture curing in air in the presence of a moisture curing catalyst. They are widely used as in-sealants and adhesives. However, as reported in Polymer Degradation and Stability 94 (2009) 465–495, silicone polymers terminated with silanol or alkoxy groups are susceptible to degradation and depolymerization in oil at high temperatures through a “depolymerization” or “chain tail biting” mechanism. When silicone polymers terminated with silanol and / or alkoxysilyl groups are heated, their viscosity molecular weight first increases sharply, which is a typical phenomenon of intermolecular reactions occurring between polymer chain ends through silanol condensation reactions. Long-term high temperature conditions lead to reduced polymer molecular weight due to the “tail biting” of silanol functions to promote intramolecular redistribution reactions, and this generates low molecular weight cyclic siloxanes. The degradation process is usually exacerbated in the presence of acids or bases that are typically present in aged oils. Volatile cyclic trimers and tetramers are the most prominent products of this cleavage and depolymerization because they are kinetically and thermodynamically stable at the degradation temperature. Their evaporation adds an additional driving force to the degradation process. The reduction in molar mass was found to be linearly related to the degree of volatility, confirming the step-wise nature of the volatile species characteristic of the depolymerization reaction. Therefore, the depolymerization of PDMS is mainly controlled by molecular structure and kinetic considerations, rather than bond energies. The formation of intramolecular cyclic transition states is the rate-determining step. Although not being bound by a particular theory, it is assumed that the silicon d-orbitals are involved in the rearrangement of the siloxane bonds, resulting in the elimination of cyclic oligomers and chain shortening.

[0034] Linear carbon-carbon-carbon (CCC) spacers within the silicone polymer backbone can be easily achieved by hydrosilylation of vinyl or allyl functional groups from silicone or organic components with Si-H functional groups in the silicone component. Such CCC spacers within silicone polymers provide rigidity to the flexible silicone polymer backbone and thus prevent degradation of the silicone polymer via tail biting or chain shearing mechanisms. In addition, CC spacers affect the thermal stability of silicone polymers. Other useful rigid spacers in silicone polymers include cyclic or branched linking groups with divalent alkylene, arylene, oxyalkylene, oxyarylene, siloxane-alkylene, siloxane-arylene, esters, amines, diols, imides, amides, alcohols, carbonates, carbamates, ureas, sulfides, ethers, or derivatives or combinations thereof. A simple method for introducing such rigid spacers (such as cyclic alkyl) is by hydrosilylation of polyvinyl functional organic compounds (such as TVCH) with Si-H containing silicone polymers.

[0035] The silicone polymer having a 3-D network structure containing CCC bonds in the present invention is not only more resistant to degradation via chain tail biting or chain shearing mechanisms than linear silicone polymers, but also has excellent thermal stability. In particular, the polymer exhibits improved oil resistance at 150°C for more than 1000 hours. In addition, the network structure provides initial wet strength for the application of sealants and adhesives. Usually the wet curing process is a slow process and requires several hours to several days to achieve full adhesive strength. Therefore, the well-designed network silicone polymer provides good initial strength for various applications.

[0036] One aspect of the present invention relates to an organosilicon polymer prepared from:

[0037] (i) from about 10 to about 98% of a vinyl terminated polyorganosiloxane having a weight average molecular weight greater than about 1,000 g / mol, preferably greater than about 10,000 g / mol;

[0038] (ii) from about 1 to about 20% of a hydride terminated polyorganosiloxane having a weight average molecular weight of less than about 100,000 g / mol, preferably less than about 10,000 g / mol;

[0039] (iii) from about 0.001 to about 20% of a vinyl or hydride (SiH) multifunctional organic compound or organosilicon compound; and

[0040] (iv) from about 0.00001 to about 5% of a hydrosilylation catalyst;

[0041] wherein the molar ratio of vinyl functional groups to hydride functional groups is about 0.1 to 0.8;

[0042] The weight average molecular weight of the organosilicon polymer is about 10,000 to 3,000,000 g / mol, preferably about 100,000 to 500,000 g / mol.

[0043] The vinyl terminated polyorganosiloxane polymer has α,ω terminated vinyl groups. The polyorganosiloxane polymer has at least two or more (R'R"SiO) units, wherein R' and R" are independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl, vinyl or a combination thereof. Examples of polyorganosiloxane polymers are polydialkylsiloxanes, polydiarylsiloxanes, polyalkylarylsiloxanes. In a preferred embodiment, the polyorganosiloxane polymer is a polymer or copolymer of polydimethylsiloxane, polydiphenylsiloxane, polymethylphenylsiloxane, poly(3,3,3-trifluoropropylmethyl)siloxane or a mixture thereof. In a most preferred embodiment, the polyorganosiloxane polymer is vinyl terminated polydimethylsiloxane (PDMS). The weight average molecular weight (Mw) of the vinyl terminated polyorganosiloxane polymer is greater than about 1,000 g / mol, preferably greater than about 10,000 g / mol.

[0044] In one embodiment of the present invention, two unique and different vinyl terminated siloxane polymers are used to form the silicone polymer product. The first vinyl terminated siloxane polymer is a high molecular weight siloxane polymer with a weight average molecular weight (Mw) greater than 100,000 g / mol, preferably about 120,000 to about 1,000,000 g / mol. The high molecular weight siloxane polymer will provide cohesive strength, adhesion and elongation. The second vinyl terminated siloxane polymer is a low molecular weight polymer with a weight average molecular weight (Mw) less than 100,000 g / mol, preferably about 5,000 to about 70,000 g / mol. The second vinyl terminated siloxane polymer will provide adjustable crosslink density and viscosity of the adhesive. High and low molecular weight reactive siloxane polymers are used together to regulate the crosslink density, modulus and viscosity of the silicone polymer and composition.

[0045] The hydride terminated polyorganosiloxane polymer has α,ω terminated H groups. The polyorganosiloxane polymer has at least two or more (R'R"SiO) units, wherein R' and R" are independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl, vinyl or a combination thereof. Examples of polyorganosiloxane polymers are polydialkylsiloxanes, polydiarylsiloxanes, polyalkylarylsiloxanes. In a preferred embodiment, the polyorganosiloxane polymer is a polymer or copolymer of polydimethylsiloxane, polydiphenylsiloxane, polymethylphenylsiloxane, poly(3,3,3-trifluoropropylmethyl)siloxane or a mixture thereof. In the most preferred embodiment, the polyorganosiloxane polymer is H terminated polydimethylsiloxane (PDMS).

[0046] The hydride terminated siloxane polymer has a weight average molecular weight of less than about 100,000 g / mol, preferably less than about 50,000 g / mol, and more preferably less than 10,000 g / mol.

[0047] The vinyl or hydride (SiH) multifunctional organic compound or the silicone polymer used to prepare the network silicone polymer may be an organic compound containing a vinyl multifunctional organic compound, or an organic compound containing a formula (R3R4SiO) n Cyclic siloxanes wherein R3 is vinyl, allyl, H or a combination thereof; R4 is R3, alkyl, aryl, fluoroalkyl, trialkylsilyl, or triarylsilyl or a combination thereof; and n=3 to 20. Examples of organic compounds containing vinyl or allyl multifunctional organic compounds are 1,2,4-trivinylcyclohexane, triallyloxytriazine, triallyl benzene trimeate, tetravinylsilane trivinylmethylsilane, tetravinylsilane, trivinylethoxysilane, tris(trimethyl)silane. Cyclic or linear siloxanes containing multifunctional vinyl or SiH (containing the formula (R3R4SiO) n , wherein R3 is vinyl, allyl, H or a combination thereof; and R4 is R3) Examples are 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane, tetravinyldimethyldisiloxane, 1,3,5,-11,2,5,5; tris(vinyldimethylsiloxy)methylsilane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trimethylcyclotrisiloxane, 1,3,5-trivinyl-1,1,3,5,5-pentamethyltrisiloxane, vinylmethylsiloxane homopolymer, vinylmethylsiloxane-dimethylsiloxane copolymer, methylhydrogenosiloxane homopolymer, methylhydrogenosiloxane-dimethylsiloxane copolymer, vinyl Q resin, vinyl T resin, hydride Q resin, hydride T resin.

[0048] The molar ratio of vinyl functional groups to hydride functional groups is defined as:

[0049] (Free vinyl functional groups) = 0.1 to 0.8

[0050] (Free hydride functional group)

[0051] Therefore, there is an excess of hydride functional groups in the silicone polymer.

[0052] The organosilicon polymer is generally formed in neat conditions and in the presence of a suitable hydrosilylation catalyst. No organic solvent is required. In one embodiment, the organosilicon polymer is prepared by reacting all components at a reaction temperature of about 25 to 150° C. for about 1 to 24 hours.

[0053] The hydrosilylation catalyst in the present invention is a transition metal complex of Pt, Rh, Ru. The preferred catalyst is Speier's catalyst H2PtCl6, or Karstedt's catalyst, or any olefin-stabilized platinum (0). The use of non-transition metal catalysts including early main group metals, boranes and phosphonium salts and N-heterocyclic carbenes is also disclosed.

[0054] Other aspects of the present invention relate to a moisture-curable silicone polymer comprising (A) a silicone polymer having an excess of free hydride functional groups and (B) a capped vinyl functional silane CH2=CH-SiY n R 3-n The reaction product is prepared by

[0055] wherein Y is alkoxy, aryloxy, acetoxy, oxime, alkenyloxy, amino, α-hydroxycarboxylic acid amide (—OCR'2CONR"2), α-hydroxycarboxylic acid ester (—OCR'2COOR"), H, OH, halogen, or a combination thereof; n=1, 2, or 3; and R, R', and R" are each independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl, or a combination thereof; and

[0056] The ratio of the vinyl functional groups of the (B) capped vinyl functional silane to the hydride functional groups of the (A) organosilicon polymer is about 1 to 1.5.

[0057] The end-capped vinyl functional silane used to make moisture-curable silicone polymers has a CH2=CH-SiY n R 3-nThe structure of wherein R is independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl or a combination thereof; Y is alkoxy, aryloxy, acetoxy, oxime, alkenyloxy, amino, amide, lactate amide, lactate ester, ester, halogen, and n is 1 to 3. Vinyl-SiY n S i 3-n Examples of silanes are vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyldimethylmethoxysilane, vinyltriethoxysilane, and the like. n S i 3-n The amount of is generally 0.01-30 wt %, more preferably 0.1-20 wt %, of the organosilicon polymer.

[0058] The molar ratio of vinyl functional groups to hydride functional groups is defined as:

[0059] (The free vinyl functional groups in the blocked vinyl functional silane (B) =1.0 to 1.5

[0060] (Free hydride functional groups in the silicone polymer (A)

[0061] As is well known to those skilled in the art, useful moisture curing moieties in silicone polymers generally include silyl groups containing alkoxy, aryloxy, acetoxy, oxime, alkenyloxy, amino, lactamido, lactate, H or halogen substituent groups.

[0062] Moisture-curable silicone polymers are generally formed under clean conditions and do not require organic solvents. First, a network silicone polymer is prepared as described above. Add about 0.1% to about 10% of a vinyl functional silane CH2=CH-SiY n R 3-n and additionally about 0.00001% to about 5% of a hydrosilylation catalyst, and reacting at about 25 to 150° C. for additional 1 to 24 hours.

[0063] Another aspect of the present invention relates to a moisture curing composition comprising:

[0064] (1) from about 10 to about 90% of the above-mentioned moisture-curable silicone polymer;

[0065] (2) from about 0.00001 to about 5% of a moisture cure catalyst; and

[0066] (3) Optionally, from about 5 to about 90% of a finely divided inorganic filler or mixture of fillers.

[0067] The moisture curing catalyst used in the moisture curable silicone composition of the present invention includes those known to those skilled in the art that can be used to catalyze and promote moisture curing. The catalyst can be a metal and a non-metal catalyst. Examples of metal catalysts that can be used in the present invention include tin, titanium, zinc, zirconium, lead, iron cobalt, antimony, manganese and bismuth organometallic compounds. Examples of non-metal-based catalysts include amines, amidines and tetramethylguanidine.

[0068] In one embodiment, the moisture curing catalyst that can be used to promote the moisture curing of the silicone composition is selected from, but not limited to, dibutyltin dilaurate, dimethyltin dineodecanoate, dioctyltin didecylmercaptate, bis(neodecanoyloxy)dioctyltin alkane, dimethylbis(oleoyloxy)tin alkane, dibutyltin diacetate, dibutyltin dimethanol, tin octoate, isobutyltintriceroate, dibutyltin oxide, solubilized dibutyltin oxide, diisooctyl bisphthalate dibutyltin, dioctyl bistripoxysilyl tin, dibutyltin bisacetylacetonate, silylated dibutyltin dioxide, carbomethoxyphenyl tin trisuccinate, and dibutyltin trisuccinate. tin tris-uberate, isobutyltin trisucrate, dimethyltin dibutyrate, dimethyltin diceneodecanoate, triethyltin tartrate, dibutyltin dibenzoate, tin oleate, tin naphthenate, butyltin tri-2-ethylhexylhexanoate, tin butyrate, dioctyltin didecylmercaptide, bis(neodecanoyloxy)dioctyltin d-olite, or dimethylbis(oleoyloxy)stannane. In a preferred embodiment, the moisture curing catalyst is selected from dimethyltin dineodecanoate (available from MomentivePerformanceMaterials Inc. under the trade name FOMREZ UL-28), dioctyltin didecylmercaptate (available from MomentivePerformanceMaterials Inc. under the trade name FOMREZ UL-32), bis(neodecanoyloxy)dioctyltin alkane (available from MomentivePerformanceMaterials Inc. under the trade name FOMREZ UL-38), dimethylbis(oleoyloxy)stannane (available from MomentivePerformanceMaterials Inc. under the trade name FOMREZ UL-50) and combinations thereof. More preferably, the moisture curing catalyst is dimethyltin dineodecanoate. In the wet composition according to the present invention, the moisture curing catalyst is present in an amount of 0.1-5% by weight based on the total weight of the composition.

[0069] However, environmental regulatory agencies and directives have increased or are expected to increase restrictions on the use of organotin compounds in formulated products. For example, compositions with greater than 0.5% by weight of dibutyltin currently need to be labeled as having a reproductive IB classification of toxicity. It is proposed that compositions containing dibutyltin be completely phased out in consumer applications within the next three to five years. The use of alternative organotin compounds, such as dioctyltin compounds and dimethyltin compounds, can only be considered as a short-term remedial plan, as these organotin compounds may also be regulated in the future. It would be helpful to identify non-tin based compounds that can accelerate the condensation cure of moisture-curable silicone compositions. Examples of non-toxic alternatives to organotin catalysts include titanium isopropoxide, zirconium octanoate, iron octanoate, zinc octanoate, cobalt naphthenate, tetrapropyl titanate, tetrabutyl titanate, titanium di-n-butoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), and the like. Other non-toxic alternatives to organotin catalysts are based on amino acid compounds. Examples of amino acid catalysts, wherein the amino acid compound is an N-substituted amino acid, wherein the N-substituted amino acid comprises at least one group other than hydrogen attached to the N-terminus. In another embodiment, the present invention may include a curable composition employing an amino acid compound as a condensation accelerator, wherein the amino acid compound is an O-substituted amino acid comprising a group other than hydrogen attached to the O-terminus. Other suitable amine catalysts include, for example, amino-functional silanes. The non-toxic moisture cure catalyst is used in an amount sufficient to effect moisture cure, typically from about 0.05 wt % to about 5.00 wt %, and advantageously from about 0.5 wt % to about 2.5 wt %.

[0070] The filler that can be used in the present invention is a finely divided inorganic filler. By "finely divided" is meant that the average particle size of the filler is less than about 5 microns. Advantageously, the average particle diameter of the inorganic filler is from about 0.2 to about 2.0 microns. In particularly advantageous embodiments: i) at least about 90% of the inorganic filler has a diameter less than 2 microns; and ii) at least about 65% of the inorganic filler has a diameter less than 1 micron. The filler may be present in an amount of at least about 15% by weight of the total composition. Ideally, the filler is present in an amount of from about 25% by weight to about 80% by weight of the total composition, and more ideally from about 25% by weight to about 60% by weight.

[0071] The silicone composition of the present invention includes certain fillers to help impart oil resistance properties to the final cured composition. Fillers are alkaline in nature so that they can react with any acidic byproducts formed in the working environment in which the composition of the present invention is intended to be used. By such reaction, the filler neutralizes these acidic byproducts before such byproducts degrade the elastomer, thereby improving adhesion retention. These fillers include, for example: zinc white, zirconium silicate, diatomaceous earth, calcareous clay particles; hydroxides, such as those of calcium, aluminum, magnesium, iron, etc.; carbonates, such as sodium, potassium, calcium carbonates and magnesium carbonate; metal oxides, such as metal oxides of zinc, magnesium, chromium, zirconium, aluminum, titanium and ferric oxide; and mixtures thereof. The filler can be present in the curable composition in the form of a composition at any suitable concentration.

[0072] A preferred filler is calcium carbonate. A commercially available example of a calcium carbonate filler suitable for use in the present invention is available from Omya, Inc. under the trade name UF-FL sold products. Any commercially available precipitated calcium carbonate can be used in the present invention. The precipitated calcium carbonate should be present in an amount of, for example, about 5 to about 50% by weight of the total composition. Ideally, the calcium carbonate is present in an amount of about 5 to about 15% by weight.

[0073] Ideally, together with precipitated calcium carbonate, the composition of the present invention can also include magnesium oxide particles in the alkaline filler component. Ideally, the presence of magnesium oxide is about 5 to about 50% by weight of the total composition, such as, for example, about 10 to about 25% by weight. According to the present invention, any magnesium oxide that satisfies the above-mentioned physical properties can be used. Ideally, magnesium oxide of the present invention is MAGCHEM 50M and MAGCHEM 200-AD, which are commercially available from Martin Marietta Magnesia Specialties, Inc., Baltimore, MD. These commercially available fillers contain about 90% by weight or more of magnesium oxide particles and various other oxides, which include, for example, calcium oxide, silicon dioxide, iron oxide, aluminum oxide and sulfur trioxide.

[0074] Another ideal filler is reinforcing silica. The silica can be fumed silica, which can be untreated or treated with an auxiliary agent to make it hydrophobic. In order to obtain any substantial reinforcing effect, the presence level of fumed silica should be at least about 5% by weight of the composition. Although the optimal silica content level varies depending on the characteristics of the specific silica, it is generally observed that before reaching the maximum reinforcing effect, the thixotropic effect of silica produces a composition with an unrealistically high viscosity. Hydrophobic silica tends to show a lower thixotropic effect, and therefore a larger amount can be included in a composition with a desired consistency. Therefore, when selecting the silica content level, it is necessary to balance the desired enhancement and actual viscosity. Fumed silica treated with hexamethyldisilazane is particularly desirable (HDK2000 of Wacker-Chemie Burghausen, Germany). Commercially available examples of fumed silica suitable for the present invention are sold by Degussa under the trade name AEROSIL R 8200.

[0075] In order to change the distribution characteristics of the composition by viscosity regulation, a thixotropic agent may be desirable. The amount of the thixotropic agent ranges from about 0.05 to about 25 weight percent of the total amount of the composition. As mentioned above, common examples of such thixotropic agents include fumed silica, and can be untreated or treated to change the chemical properties of its surface. In fact, any enhanced fumed silica can be used. Examples of such treated fumed silica include silica treated with polydimethylsiloxane and silica treated with hexamethyldisilazane. Such treated silica is commercially available, such as commercially available from Cabot Corporation with trade name CABSIL ND-TS, and commercially available from Evonik with trade name AEROSIL (such as AEROSIL R805). In untreated silica, amorphous silica and hydrated silica can be used. For example, commercially available amorphous silica includes: AEROSIL 300, which has an average primary particle size of about 7 nm; AEROSIL 200, which has an average primary particle size of about 12 nm; AEROSIL 130, which has an average primary particle size of about 16 nm; and commercially available hydrated silica includes: NIPSIL E150, which has an average particle size of 4.5 nm; NIPSIL E200A, which has an average particle size of 2.0 nm; and NIPSIL E220A, which has an average particle size of 1.0 nm (manufactured by Japan Silica Kogya Inc.). Other desirable fillers for use as thixotropic agents include those consisting of or containing alumina, silicon nitride, aluminum nitride, and silicon dioxide-coated aluminum nitride. Hydroxy-functional alcohols are also very suitable as thixotropic agents, such as tris[copoly(propylene oxide)(propylene oxide)] ether of trimethylolpropane and the polyalkylene glycol commercially available from BASF under the trade name PLURACOL V-10.

[0076] Other conventional fillers may also be incorporated into the compositions of the present invention provided that they impart alkalinity to the composition and do not adversely affect the oil-resistant curing mechanism and the adhesive properties of the final product obtained therefrom. Generally, any suitable mineral, carbonaceous, glass or ceramic filler may be used, including but not limited to: precipitated silica; clay; metal sulfate salts; chalk, lime powder; precipitated and / or pyrolyzed silicic acid; phosphates; carbon black; quartz; zirconium silicate; gypsum; silicon nitride; boron nitride; zeolite; glass; plastic powder; graphite; synthetic fibers and mixtures thereof. The amount of filler used ranges from about 5 to about 70% by weight of the total composition. Commercially available examples of precipitated silica fillers suitable for use in the present invention are sold by JM Huber under the trade name ZEOTHIX 95.

[0077] Organic fillers can also be used, in particular silicone resins, wood fibers, wood flour, sawdust, cellulose, cotton, pulp, cotton, wood chips, chopped straw and husks. In addition, short fibers such as glass fibers, glass filaments, polyacrylonitrile, carbon fibers, Kevlar fibers or polyethylene fibers can also be added.

[0078] The silicone composition may further include an optional silane adhesion promoter, a functional polymer and / or an oligomer adhesion promoter. The adhesion promoter may act to enhance the adhesion properties of the curable silicone composition to a specific substrate (i.e., metal, glass, plastic, ceramic and their blends). Depending on the specific substrate element used in a given application, any suitable adhesion promoter may be used for this purpose. Examples of available silane adhesion promoters include, but are not limited to, C3-C24 alkyltrialkoxysilanes, (meth)acryloxypropyltrialkoxysilanes, chloropropylmethoxysilanes, vinyltrimethoxysilanes, vinyltriethoxysilanes, vinylbenzylpropyltrimethoxysilanes, aminopropyltrimethoxysilanes, vinyltriacetoxysilanes, glycidyloxypropyltrimethoxysilanes, 1,2-di ... Trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, mercaptopropylmethoxysilane, 3-aminopropyltriethoxysilane, aminomethyltrimethoxysilane, aminomethyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, (N-2-aminoethyl)-3-aminopropyltrimethoxysilane, (N-2-aminoethyl)-3-aminopropyltriethoxysilane, diethylenetriaminopropyltrimethoxysilane, phenylaminomethyltrimethoxysilane, (N-2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-(N-phenylamino) Propyltrimethoxysilane, 3-piperazinylpropylmethyldimethoxysilane, 3-(N,N-dimethylaminopropyl)aminopropylmethyldimethoxysilane, tris[(3-triethoxysilyl)propyl]amine, tris[(3-trimethoxysilyl)propyl]amine, 3-(N,N-dimethylamino)propyltrimethoxysilane, 3-(N,N-dimethylamino)-propyltriethoxysilane, (N,N-dimethylamino)methyltrimethoxysilane, (N,N-dimethylamino)methyltriethoxysilane, bis(3-trimethoxysilyl)propylamine, Bis(3-triethoxysilyl)propylamine and mixtures thereof, particularly preferably 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, aminomethyltrimethoxysilane, aminomethyltriethoxysilane, 3-(N,N-dimethylamino)propyltrimethoxysilane, 3-(N,N-dimethylamino)propyltriethoxysilane, (N,N-dimethylamino)methyltrimethoxysilane, (N,N-dimethylamino)methyltriethoxysilane, bis(3-trimethoxysilyl)propylamine, bis(3-triethoxysilyl)propylamine and mixtures thereof.

[0079] Examples of useful functional polymeric and / or oligomeric adhesion promoters include, but are not limited to, hydrolyzable PDMS polymers or oligomers, for example, PDMS end-capped with trialkoxysilyl (meth)acrylate, dialkoxysilyl (meth)acrylate, or methacrylate groups.

[0080] The adhesion promoter is generally used in an amount of 0.2 to 40 wt %, more preferably 1 to 20 wt %, of the total curable silicone composition.

[0081] The silicone composition optionally includes a desiccant or moisture scavenger. Examples of suitable desiccants are: vinyl silanes, such as 3-vinylpropyltriethoxysilane; oxime silanes, such as methyl-O,O',O"-butan-2-onetrioximinosilane or O,O',O",O"'-butan-2-one-tetraoximinosilane; or benzamidosilanes, such as bis(N-methylbenzamido)methylethoxysilane; or carbamatosilanes, such as carbamatomethyltrimethoxysilane. However, methyl-, ethyl- or vinyl-trimethoxysilane, tetramethyl- or tetraethyl-ethoxysilane may also be used. Vinyltrimethoxysilane and tetraethoxysilane are particularly preferred in terms of cost and efficiency. The composition typically contains from about 0 to about 6 weight percent of a desiccant or moisture scavenger.

[0082] In the present composition, an effective amount of plasticizer may be added to ensure the desired processability of the uncured composition and the properties of the final cured composition.Both silicone and organic plasticizers can be used in the present invention.

[0083] Suitable plasticizers include, for example, trimethyl terminated polyorganosiloxanes, petroleum derived organic oils, polybutenes, alkyl phosphates, polyalkylene glycols, poly(propylene oxide), hydroxyethylated alkylphenols, dialkyl dithiophosphonates, poly(isobutylene), poly(α-olefins), and mixtures thereof. The plasticizer component can provide further oil resistance to the cured elastomer. Thus, from about 1 to about 50 weight percent, preferably from about 10 to about 35 weight percent, of a selected plasticizer can be incorporated into the composition of the present invention.

[0084] The present silicone composition may also include one or more crosslinking agents. The crosslinking agent may be a hexafunctional silane, but other crosslinking agents may also be used. Examples of such crosslinking agents include, for example, methyltrimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, methyltriacetoxysilane, vinyltriacetoxysilane, methyltri(N-methylbenzamido)silane, methyltri(isopropenyloxy)silane, methyltri(cyclohexylamino)silane, methyltri(methylethylketoxime)silane, vinyltri(methylethylketoxime)silane, methyltri(methylisobutylketoxime)silane, vinyltri(methylisobutylketoxime)silane, The invention also includes the following: tetra(methyl ethyl ketoximino) silane, tetra(methyl isobutyl ketoximino) silane, tetra(methyl amyl ketoximino) silane, dimethylbis(methyl ethyl ketoximino) silane, methylvinylbis(methyl ethyl ketoximino) silane, methylvinylbis(methyl isobutyl ketoximino) silane, methylvinylbis(methyl amyl ketoximino) silane, tetrafunctional alkoxyketoximino silane, tetrafunctional alkoxy-ketoximino silane, tri- or tetraenyloxy silane, tri- or tetralactamido silane and tri- or tetralactate silane.

[0085] Typically, the crosslinking agent used in the present composition is present in an amount of about 1 to about 10% by weight of the total composition. However, the exact concentration of the crosslinking agent can vary depending on the specific agent, the desired cure rate, and the molecular weight of the silicone polymer used in the composition.

[0086] The present organosilicon composition may also contain other additives as long as they do not inhibit the curing mechanism or the intended use, for example, conventional additives such as pigments, inhibitors, odor masking agents, etc. may be included.

[0087] The cross-linking reaction is a condensation reaction and generates a cross-linked network product through Si-O-Si covalent bonds between moisture-reactive components.

[0088] The reaction products of the present silicone polymers and compositions can be used as adhesives or sealants for bonding, sealing, encapsulating metal surfaces that are exposed to oil during their intended use. The silicone compositions of the present invention can also be formed into many different configurations and then addition cured. Articles formed in this manner can be used in various industries where oil-resistant silicone-based elastomeric articles are needed. In the vehicle assembly industry, for example, O-rings, hoses, seals and gaskets can be formed from the present compositions. Other conventional uses that require good sealing properties as well as oil resistance are also contemplated for the compositions of the present invention.

[0089] The CCC bonds impart oil resistance to the cured composition at elevated temperatures. The network silicone polymers and compositions cure by a condensation mechanism in the presence of moisture and a catalyst. The partially cross-linked structure in the network polymer exhibits a shorter skin over time and, therefore, better wet strength. The silicone polymers and compositions are particularly useful as sealants and gaskets in automotive powertrains.

[0090] The curable silicone composition can be applied to surfaces exposed to oil within its intended use. The surface to which the present composition is to be applied can be any surface exposed to oil, such as the working surface of a conventional internal combustion engine. This method includes applying the composition of the present invention to the working surface. The working surface can be composed of a variety of materials, such as most metals, glass, and daily necessities or engineering plastics. In another aspect of the present invention, a method for using an oil-resistant mechanical seal is provided, which remains sealed after exposure to oil. This method includes applying a seal-forming amount of the composition as previously described to the surface of a mechanical part. A seal is then formed between at least two mechanical surfaces by addition curing under exposure to elevated temperature conditions (e.g., 150°C), after which the seal is still competent even when exposed to oil under extreme temperature conditions for a long time (e.g., greater than 500 hours).

[0091] In yet another aspect of the present invention, a method of using an oil-resistant seal is provided, wherein the oil-resistant seal remains adhesive after contact with oil and / or immersion in oil. This method comprises forming a seal between two or more surfaces by applying an oil-resistant seal formed from a composition according to the present invention between the two or more surfaces. This method comprises the following steps: (a) providing a silicone sealant; (b) incorporating at least about 5 weight percent of a composition into the sealant, the composition comprising magnesium oxide particles having an average particle size of about 0.5 μM to about 1.5 tM and an average surface area of ​​about 50 M2 / g to about 175 M2 / g; and (c) cross-linking the silicone sealant to form an oil-resistant elastomeric article. Ideally, the sealant composition includes about 10 to about 90 weight percent of an organosilicon polymer, about 1 to about 20 weight percent of fumed silica, about 5 to about 50 weight percent of precipitated calcium carbonate and / or magnesium oxide, about 1 to about 10 weight percent of a crosslinking agent, and about 0.05 to about 5 weight percent of a moisture curing catalyst, each based on the total weight of the composition. The sealant composition may also include other optional components, including, for example, plasticizers, adhesion promoters, pigments, and the like.

[0092] The preparation of the moisture-curable composition can be carried out by mixing the moisture-curable network silicone polymer, moisture-curing catalyst, filler and other optional ingredients in the present invention. This mixing process can be carried out in a suitable dispersing unit, such as a high-speed mixer, a planetary mixer and a Brabender mixer. In all cases, care should be taken not to allow the mixture to come into contact with moisture, which would lead to undesirable curing. Suitable measures are well known in the art: mixing in an inert atmosphere under a protective gas and drying / heating the individual components before addition.

[0093] Example

[0094] Vinyl terminated PDMS, hydride terminated PDMS, 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, Karstedt's catalyst Pt(0), tetramethyldisiloxane, vinyltrimethoxysilane, methylhydrogensiloxane-dimethylsiloxane copolymer (MeHSiO 6-7 mol %) can be obtained from Gelest Inc.

[0095] 1,2,4-Trivinylcyclohexane and dibutyltin dilaurate were obtained from Sigma-Aldrich.

[0096] Fumed silica is available from Evonik.

[0097] SF105F engine oil is available from the Test Monitoring Center.

[0098] Tack-free time measurement : Determine the tack-free time under standard climatic conditions (25 + / - 2°C, relative humidity 50 + / - 5%). Mix the moisture-curable silicone polymer and 0.01 wt.% dibutyltin dilaurate composition in a plastic jar to form a composition. Immediately start a stopwatch. Lightly touch the surface with a fingertip until the composition no longer adheres to the fingertip. Record the tack-free time in hours.

[0099] Shore OO hardness : The procedure followed ASTM D2240-OO and fully cured moisture-curable silicone polymers were tested using a Shore durometer in the presence of 0.01 wt % dibutyltin dilaurate composition.

[0100] Mechanical properties (tensile test): The tensile test is used to determine the elongation at break and the tensile stress value (E modulus) according to DIN 53504. Sample dumbbell-shaped specimens with the following dimensions are used as test pieces: thickness: 2+ / -0.2mm; gauge width: 10+ / -0.5mm; gauge length: about 45mm; total length: 9cm. The test is carried out after 7 days of curing. A two-millimeter thick film is pulled out of the material. The film is stored under standard climatic conditions for 7 days and then a dumbbell shape is punched out. Three dumbbell-shaped specimens are made for each test. The test is carried out under standard climatic conditions. Before measuring, the specimen is adapted to the test temperature (i.e., stored) for at least 20 minutes. Before measuring, the thickness of the test specimen is measured at three positions at room temperature using a vernier caliper; i.e., for dumbbell-shaped specimens, measurements are made at both ends and in the middle within the initial gauge length. The average value is entered into the measurement program. The test specimen is clamped in a tensile tester so that the longitudinal axis is consistent with the mechanical axis of the tensile tester and the largest possible surface of the clamp is gripped without clamping the narrow part. At a test speed of 50 mm / min, the dumbbell-shaped specimen was tensioned to a preload of <0.1 MPa.

[0101] Example 1. Preparation of a network silicone polymer

[0102] A mixture of vinyl terminated polydimethylsiloxane (Mw 55000 g / mol) (600 g, 14 mmol), 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane (1.2 g, 3.48 mmol), hydride terminated polydimethylsiloxane (Mw 1000 g / mol) (45 g, 48 mmol) and Pt (0) (150 PPM) was stirred at room temperature for 30 minutes. The mixture was heated to 65-70 ° C and continued to mix for 3 hours. The product was collected in a quantitative yield as a colorless viscous liquid.

[0103] Comparative Example 2. Preparation of moisture-curable linear silicone polymer

[0104] A mixture of vinyl terminated polydimethylsiloxane (Mw 140000 g / mol) (180.0 g, 1.5 mmol), vinyl terminated polydimethylsiloxane (Mw 55000 g / mol) (45.0 g, 1.0 mmol) and Pt (0) (200 PPM) was stirred at room temperature for 30 minutes. Tetramethyl disiloxane (5.0 g, 37 mmol) was added and mixed for 30 minutes. The mixture was heated to 60 ° C and continued to mix for 3 hours. Excess tetramethyl disiloxane was removed under 60 ° C vacuum. Vinyl trimethoxy silane (10.0 g, 13 mmol) was added, and the mixture was stirred for 4 hours at 60 ° C. The product was collected in a quantitative yield, and it was a colorless viscous liquid.

[0105] Example 3. Preparation of moisture-curable network silicone polymer

[0106] A mixture of vinyl terminated polydimethylsiloxane (Mw 140000 g / mol) (520.0 g, 4.4 mmol), vinyl terminated polydimethylsiloxane (Mw 55000 g / mol) (130.0 g, 3.0 mmol), 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane (0.3 g, 0.87 mmol) and Pt (0) (150 PPM) was stirred at room temperature for 30 minutes. Tetramethyldisiloxane (10.4 g, 77.4 mmol) was added and mixed for 30 minutes. The mixture was heated to 60 ° C and continued to mix for 3 hours. Excess tetramethyldisiloxane was removed under 60 ° C vacuum. Vinyltrimethoxysilane (3.0 g, 20.2 mmol) was added and the mixture was stirred at 60 ° C for 4 hours. The product was collected in a quantitative yield as a colorless viscous liquid.

[0107] Example 4. Preparation of moisture-curable network silicone polymer

[0108] A mixture of vinyl terminated polydimethylsiloxane (Mw 140000 g / mol) (520.0 g, 4.4 mmol), vinyl terminated polydimethylsiloxane (Mw 55000 g / mol) (130.0 g, 3.0 mmol), methylhydrogensiloxane-dimethylsiloxane copolymer (MeHSiO 6-7 mol%, Mn 2000 g / mol) (0.2 g, 0.1 mmol) and Pt (0) (150 PPM) was stirred at room temperature for 30 minutes. Tetramethyldisiloxane (10.4 g, 77.4 mmol) was added and mixed for 30 minutes. The mixture was heated to 60 ° C and continued to mix for 3 hours. Excess tetramethyldisiloxane was removed under 60 ° C vacuum. Vinyltrimethoxysilane (3.5 g, 23.6 mmol) was added and the mixture was stirred at 60 ° C for 4 hours. The product was collected in a quantitative yield as a colorless viscous liquid.

[0109] Example 5. Preparation of moisture-curable network silicone polymer

[0110] A mixture of vinyl terminated polydimethylsiloxane (Mw 140000 g / mol) (520.0 g, 4.4 mmol), vinyl terminated polydimethylsiloxane (Mw 55000 g / mol) (130.0 g, 3.0 mmol), 1,2,4-trivinylcyclohexane (0.3 g, 1.8 mmol) and Pt (0) (150 PPM) was stirred at room temperature for 30 minutes. Tetramethyldisiloxane (10.4 g, 77.4 mmol) was added and mixed for 30 minutes. The mixture was heated to 60 ° C and continued to mix for 3 hours. Excess tetramethyldisiloxane was removed under 60 ° C vacuum. Vinyltrimethoxysilane (3.5 g, 23.6 mmol) was added and the mixture was stirred at 60 ° C for 4 hours. The product was collected in a quantitative yield, which was a colorless viscous liquid.

[0111] Example 6. Preparation of moisture-curable network silicone polymer

[0112] A mixture of vinyl terminated polydimethylsiloxane (Mw 55000 g / mol) (600 g, 14 mmol), 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane (1.2 g, 3.48 mmol), hydride terminated polydimethylsiloxane (Mw 1000) (45 g, 48 mmol) and Pt (0) (150 PPM) was stirred at room temperature for 30 minutes. The mixture was heated to 65-70 ° C and continued to mix for 3 hours. Vinyl trimethoxysilane (12 g, 81 mmol) was added, and the mixture was stirred at 65-70 ° C for 3 hours. The product was collected in a quantitative yield, and it was a colorless viscous liquid.

[0113] Example 7. Properties of Moisture Curable Silicone Polymers

[0114] Table 1. Properties of moisture-curable silicone polymers

[0115] Example 2(C) 3 4 5 6 Mw,g / mol 123,000 187,000 170,000 177,000 159,000 PDI 2.0 2.8 2.6 2.8 2.6 Viscosity, 25C, Pa-s 56 90 71 86 54 <![CDATA[Surface drying time * , h]]> 2.0 1.0 1.0 1.0 1.0 Fully cured film hardness, Shore OO 67 70 70 65 73

[0116] * The sample contained 0.01 wt% dibutyltin dilaurate.

[0117] Table 2. Properties of moisture-curable silicone polymers

[0118] <![CDATA[Example * > 2(C) 6 Initial modulus, psi 44 66 Initial elongation, % 479 264 <![CDATA[Ageing modulus ** ,in engine oil for 1000 hours, psi]]> 8 16 <![CDATA[Elongation at break after aging ** , 1000 hours in engine oil, %]]> 721 134

[0119] * The sample contained 0.01 wt% dibutyltin dilaurate and 7 wt% fumed silica; ** The cured samples were immersed in SF105F engine oil at 150°C for 1000 hours.

[0120] As shown in Table 1 above, under similar viscosity, the network polymer Examples 3-6 generally have higher weight average molecular weight (Mw) and wider molecular weight distribution (PDI) than the linear polymer (Comparative Example 2 (C)). In the presence of 0.1% dibutyltin dilaurate, the network polymer exhibits a faster surface curing speed (tack-free time) than the linear polymer. Figure 1 As shown, the viscosity of the network silicone polymer Example 6 (square dots) decreases at a faster rate than the linear silicone polymer of Example 2 (C) (triangle dots).

[0121] Reticulated silicone polymer Examples 3, 4, and 6 have higher Shore OO hardness than the linear polymers. Reticulated silicone polymer Example 5 has a similar Shore OO hardness value as the linear silicone polymer, and this may be due to incomplete curing of the non-silicone compound trivinylcyclohexane, resulting in a more rigid network structure.

[0122] also, Figure 2 GPC values ​​of Examples 2(C) and 6 are shown. Both have similar peak average molecular weights (Mp) of about 115,599, but Example 6 (dashed line) has a broader PDI, which indicates more low molecular weight fractions and more high molecular weight fractions in the polymer of Example 6. However, compared to Example 2(C) (straight line), Example 6 has only slightly higher viscosity, but provides a network structure.

[0123] Comparative Example 2 (C) shows that the linear polymer has a higher elongation than the network polymer (Example 6). The network silicone polymer has a higher initial modulus and aged modulus than the linear polymer. For both the initial sample and the aged sample in SF105F oil at 150°C for 100 hours, the fully cured network silicone polymer sample shows a lower elongation and higher modulus than the linear polymer.

[0124] As will be apparent to those skilled in the art, many modifications and variations may be made to the present invention without departing from the spirit and scope of the present invention. The specific embodiments described herein are provided by way of example only, and the present invention is limited only by the terms of the appended claims and the full scope of equivalents to which such claims are entitled.

Claims

1. A network silicone polymer, the polymer being prepared by: (i) 10 to 98 weight percent of a vinyl terminated polyorganosiloxane having a weight average molecular weight greater than 1,000 g / mol; (ii) 1 to 20 wt % of a SiH-terminated polyorganosiloxane having a weight average molecular weight of less than 100,000 g / mol; (iii) 0.001 to 20 wt% of a vinyl multifunctional organic compound selected from the group consisting of 1,2,4-trivinylcyclohexane, triallyloxytriazine, triallyl benzenetricarboxylate, tetravinylsilane, trivinylmethylsilane, trivinylethoxysilane, 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane, tetravinyldimethyldisiloxane, tris(vinyldimethylsiloxy)methylsilane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trimethylcyclotrisiloxane, and 1,3,5-trivinyl-1,1,3,5,5-pentamethyltrisiloxane; and (iv) 0.00001 wt % to 5 wt % of a hydrosilylation catalyst; wherein the molar ratio of vinyl functional groups to SiH functional groups is 0.1 to 0.8; wherein the weight average molecular weight of the network silicone polymer is from 10,000 g / mol to 3,000,000 g / mol; and The weight percentages of (i) to (iv) add up to 100 weight %.

2. The network silicone polymer according to claim 1, wherein the (i) vinyl terminated polyorganosiloxane has the following formula: monomer (R1R2SiO) unit, wherein R1 and R2 are independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl or a combination thereof.

3. The network organosilicon polymer according to claim 1, wherein the (ii) SiH-terminated polyorganosiloxane has the following formula: monomer (R1R2SiO) unit, wherein R1 and R2 are independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl or a combination thereof.

4. The network silicone polymer according to any one of claims 1 to 3, wherein the weight average molecular weight of the vinyl terminated polyorganosiloxane is greater than 10,000 g / mol.

5. The network organosilicon polymer according to any one of claims 1 to 3, wherein the weight average molecular weight of the SiH-terminated polyorganosiloxane is less than 10,000 g / mol.

6. A moisture-curable network silicone polymer prepared from a reaction product comprising: (A) A network silicone polymer prepared from: (i) 10 to 98 weight percent of a vinyl terminated polyorganosiloxane having a weight average molecular weight greater than 1,000 g / mol; (ii) 1 to 20 wt % of a SiH-terminated polyorganosiloxane having a weight average molecular weight of less than 100,000 g / mol; (iii) 0.001 to 20 wt% of a vinyl multifunctional organic compound selected from the group consisting of 1,2,4-trivinylcyclohexane, triallyloxytriazine, triallyl benzenetricarboxylate, tetravinylsilane, trivinylmethylsilane, trivinylethoxysilane, 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane, tetravinyldimethyldisiloxane, tris(vinyldimethylsiloxy)methylsilane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trimethylcyclotrisiloxane, and 1,3,5-trivinyl-1,1,3,5,5-pentamethyltrisiloxane; and (iv) 0.00001 wt % to 5 wt % of a hydrosilylation catalyst; wherein the molar ratio of vinyl functional groups to SiH functional groups is 0.1 to 0.8; wherein the weight average molecular weight of the network silicone polymer is 10,000 g / mol to 3,000,000 g / mol, and The weight percentages of (i) to (iv) add up to 100 weight %, and (B) End-capped vinyl functional silane CH2=CH-SiY n R 3-n , wherein Y is alkoxy, aryloxy, acetoxy, oxime, alkenyloxy, amino, α-hydroxycarboxylic acid amide (—OCR'2CONR"2), α-hydroxycarboxylic acid ester (—OCR'2COOR"), H, OH, halogen, or a combination thereof; n=1, 2, or 3; and R, R', and R" are each independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl, or a combination thereof; and The ratio of the vinyl functional groups in the (B) blocked vinyl functional silane to the free SiH functional groups in the (A) organosilicon polymer is 1 to 1.

5.

7. The network silicone polymer of claim 6, wherein the weight average molecular weight of the vinyl terminated polyorganosiloxane is greater than 10,000 g / mol.

8. The network organosilicon polymer of claim 6, wherein the SiH-terminated polyorganosiloxane has a weight average molecular weight of less than 10,000 g / mol.

9. A moisture-curable composition comprising: (1) 10% to 90% of a moisture-curable silicone polymer prepared from the reaction product comprising: (A) A network silicone polymer prepared from: (i) 10 to 98 weight percent of a vinyl terminated polyorganosiloxane having a weight average molecular weight greater than 1,000 g / mol; (ii) 1 to 20 wt % of a SiH-terminated polyorganosiloxane having a weight average molecular weight of less than 100,000 g / mol; (iii) 0.001 to 20 wt% of a vinyl multifunctional organic compound selected from the group consisting of 1,2,4-trivinylcyclohexane, triallyloxytriazine, triallyl benzenetricarboxylate, tetravinylsilane, trivinylmethylsilane, trivinylethoxysilane, 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane, tetravinyldimethyldisiloxane, tris(vinyldimethylsiloxy)methylsilane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trimethylcyclotrisiloxane, and 1,3,5-trivinyl-1,1,3,5,5-pentamethyltrisiloxane; and (iv) 0.00001 wt % to 5 wt % of a hydrosilylation catalyst; wherein the molar ratio of vinyl functional groups to SiH functional groups is 0.1 to 0.8; wherein the weight average molecular weight of the network silicone polymer is 10,000 g / mol to 3,000,000 g / mol, and The weight percentages of (i) to (iv) add up to 100 weight %; and (B) End-capped vinyl functional silane CH2=CH-SiY n R 3-n , wherein Y is alkoxy, aryloxy, acetoxy, oxime, alkenyloxy, amino, α-hydroxycarboxylic acid amide (—OCR'2CONR"2), α-hydroxycarboxylic acid ester (—OCR'2COOR"), H, OH, halogen, or a combination thereof; n=1, 2, or 3; and R, R', and R" are each independently alkyl, aryl, fluoroalkyl, trialkylsilyl, triarylsilyl, or a combination thereof; and wherein the ratio of the vinyl functional groups in the (B) blocked vinyl functional silane to the free SiH functional groups in the (A) organosilicon polymer is 1 to 1.5; (2) 0.00001% to 5% of a moisture curing catalyst; and (3) Optionally, 5 to 90% of a finely divided inorganic filler or a mixture of fillers.

10. The moisture-curable composition of claim 9, wherein the filler is selected from the group consisting of silicone resins, organic fillers, plastic powders, and combinations thereof.

11. The moisture-curable composition of claim 9, further comprising a reactive silane.

12. The moisture-curable composition of claim 9 which is an adhesive or a sealant.

13. The moisture-curable composition of claim 9, wherein the vinyl terminated polyorganosiloxane has a weight average molecular weight greater than 10,000 g / mol.

14. The moisture-curable composition of claim 9, wherein the SiH-terminated polyorganosiloxane has a weight average molecular weight of less than 10,000 g / mol.

15. The moisture-curable composition of claim 12, wherein the adhesive or sealant is an automotive gasket.

Citation Information

Patent Citations

  • Silicone elastomer compositions

    EP0572148A2

  • High modulus silicone rubber

    US4052357A

  • Oil resistant low modulus silicone sealant composition

    US4514529A

  • Auto-adhering one-component RTV silicone sealant composition utilizing glycidoxyalkyl substituted alkoxy-oxime silane as an adhesion promoter

    US4673750A

  • Auto-adhering one-component RTV silicone sealant composition utilizing an adhesion promoter

    US4735979A