Long-lasting mildew-proof adhesive and preparation method thereof
The long-term effect of the cross-linking agent compounded with methyl tributyl ketone oxime silane, propyl tributyl ketone oxime silane and tetrabutyl ketone oxime silane and the aminopropyl triethoxysilane curing agent is used in the kitchen and bathroom. Anti-mold glue solves the problem of existing anti-mold glues becoming moldy in humid environments and achieves long-term anti-mold effects with high mechanical properties and low cost.
Patent Information
- Application Number
- CN202110468715.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-04-28
AI Technical Summary
The existing anti-mold glue in kitchens and bathrooms is prone to mold in a long-term humid environment, resulting in a decrease in strength and adhesion. The production cost is high and complex, making it difficult to achieve long-term anti-mold effects.
The cross-linking agent is prepared from methyltributylketoneoximesilane, propyltributylketoneoximesilane and tetrabutylketoneoximesilane, combined with aminopropyltriethoxysilane or (aminoethyl)aminopropyl Trimethoxysilane is used as a curing agent to prepare a long-lasting anti-mold glue with high cross-linking density and strong compactness, and an anti-mold agent is added to prevent mold invasion.
The hardness, tensile strength and adhesion of the prepared colloid are better than those of ordinary home decoration glue, and the cost is low. It can resist mildew for a long time in a high-humidity environment. The mildew-proof grade reaches level 0, and the mechanical properties are significantly improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer sealing materials for buildings, and in particular to a long-acting mildew-proof adhesive, in particular to a novel long-acting mildew-proof adhesive used in kitchens and bathrooms and a preparation method thereof. Background Art
[0002] In the home decoration industry, sealants are usually used for bonding, sealing, joints, and waterproofing. However, in kitchens and bathrooms, since water is often used, the air in the kitchens and bathrooms is generally very humid. Even if mildew-proof silicone sealants are used, the silicone sealants will become moldy under the action of humid water vapor for a long time, causing a decrease in strength and adhesion, thereby affecting the appearance of the kitchen and bathroom and even causing safety problems.
[0003] At present, the mildew-proof glues on the market mainly include ordinary silicone sealants, silane-modified polyether sealants, etc. Among them, ordinary silicone sealants are mainly organic raw materials and are very easy to breed mildew. The mildew-proof principle of most mildew-proof glues comes from the auxiliary mildew-proof agent. The amount of mildew-proof agent added to silicone glue is a certain proportion and is very limited. Once mildew is bred, the mildew-proof agent added in the system will be consumed, but when the mildew-proof agent is exhausted, it will not play a mildew-proof role; Silane-modified polyether sealants use alkoxysilane-terminated polyether polymers as the base material, but if a silane-terminated polyether is used alone, it is difficult to achieve long-term mildew-proof effect due to the insufficient density of the colloidal structure and the poor mechanical properties. Generally, multiple silane-terminated polyethers are required to be compounded in a strict proportion to obtain a long-lasting mildew-proof glue, which significantly increases the production cost and the difficulty of preparation.
[0004] Therefore, there is an urgent need for a long-lasting mildew-proof adhesive that has a more convenient preparation process, is low-cost, and can be applied to kitchens and bathrooms. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a long-lasting mildew-proof glue, which is mainly prepared by compounding a cross-linking agent of methyl tributylidene silane, propyl tributylidene silane and tetrabutyl tributylidene silane, and matching a specific curing agent formula, so as to prepare a long-lasting mildew-proof glue with high cross-linking density, very dense colloid, and mold cannot enter, and the hardness, tensile strength and adhesion of the colloid itself are higher, which are better than the mechanical properties of ordinary home improvement glue, and the cost is lower and the preparation is simple, and it is particularly suitable for long-lasting mildew-proof glue in kitchens, bathrooms and other occasions.
[0006] On the one hand, the present invention provides a long-lasting mildew-proof glue, comprising a base glue, a crosslinking agent and a curing agent; the crosslinking agent is composed of methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane.
[0007] The inventors have found through extensive research that the cross-linking density of the colloid prepared by compounding methyltributylacetoximosilane, propyltributylacetoximosilane and tetrabutylketoneximosilane is very high, making the colloid very dense and mold unable to enter.
[0008] Furthermore, the mass ratio of the methyl tributylacetoximate silane, the propyl tributylacetoximate silane and the tetrabutyl ketone oxime silane is 6 to 9:3 to 5:1.
[0009] The appropriate mass ratio among methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl tributylacetoximosilane can further enhance the cross-linking effect, thereby increasing the density of the colloid and preventing mold from entering.
[0010] Furthermore, the mass ratio of the methyl tributylacetoximate silane, the propyl tributylacetoximate silane and the tetrabutyl ketone oxime silane is 7:4:1.
[0011] Furthermore, the curing agent is at least one of aminopropyltriethoxysilane or (aminoethyl)aminopropyltrimethoxysilane.
[0012] On the basis of the cross-linking agent compounded with methyltributylacetoximine silane, propyltributylacetoximine silane and tetrabutylketoneximine silane, with the addition of a suitable curing agent, the mechanical properties of the colloid can be further improved, thereby making the hardness, tensile strength and adhesion of the prepared colloid higher, which is better than the mechanical properties of ordinary home improvement glue.
[0013] Furthermore, the curing agent is (aminoethyl)aminopropyltrimethoxysilane, and the mass ratio of the cross-linking agent to the curing agent is 10 to 15:1.
[0014] Experiments have shown that when (aminoethyl)aminopropyltrimethoxysilane is used as a curing agent, the mechanical properties of the obtained colloid are even better.
[0015] Furthermore, it also includes a mildew preventer, which is BCO-2 mildew preventer produced by Guangdong Dimei; and the base glue is 107 glue.
[0016] Appropriate mildew inhibitors are sealed in colloids to serve as the last line of defense against the entry of mildew. However, mildew inhibitors are usually left unused for long periods of time because mildew cannot enter.
[0017] Furthermore, it also includes a plasticizer, a catalyst and a filler, and the plasticizer is dimethyl silicone oil.
[0018] Furthermore, the catalyst is dibutyltin dilaurate, and the filler is fumed white carbon black.
[0019] Furthermore, calculated by mass, the long-lasting mildew-proof glue includes 100 parts of 107 glue, 12 parts of a cross-linking agent, 0.2 parts of a mildew-proof agent, 1 part of a curing agent, 40 parts of a plasticizer, 0.2 parts of a catalyst, and 16 parts of a filler.
[0020] In another aspect, the present invention provides a method for preparing the environmentally friendly long-lasting mildew-proof adhesive as described above, comprising the following steps:
[0021] (1) First add 107 glue, crosslinking agent, plasticizer and mildewproof agent, and stir in vacuum for 30-40 minutes; (2) Then add fumed silica, stir evenly, and stir in vacuum at high speed for 30-40 minutes; (3) Finally, add curing agent and catalyst and stir in vacuum for 20-30 minutes. The reaction temperature must be controlled below 50°C during the whole process.
[0022] The beneficial effects of the present invention are:
[0023] 1. The cross-linking density of the prepared colloid is high, the colloid is very dense, and mold cannot enter, which can achieve long-term mildew prevention;
[0024] 2. High hardness, good toughness, high tensile strength and high adhesion;
[0025] 3. It can be widely used in home decoration, kitchen and bathroom and other construction sites. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with the examples. It should be noted that the examples described below are intended to facilitate the understanding of the present invention and do not have any limiting effect on it. The reagents used in this example are all known products and were obtained by purchasing commercially available products.
[0027] Example 1 Crosslinking agent: methyl tributylidene oxime silane; curing agent: aminopropyl triethoxy silane
[0028] The colloid provided in this embodiment uses methyl tributylidene silane as a cross-linking agent, and the main preparation process is: (1) first add 100 parts of 107 glue, 12 parts of methyl tributylidene silane, 40 parts of dimethyl silicone oil, and 0.2 parts of BCO-2 mildew inhibitor from Guangdong Dimei, and stir in vacuum for 30-40 minutes at a stirring speed of 300-400 rpm; (2) then add 16 parts of fumed silica and stir evenly, and stir in vacuum at high speed for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally add 1 part of aminopropyl triethoxysilane and 0.2 parts of dibutyltin dilaurate, and stir in vacuum for 20-30 minutes. The reaction temperature needs to be controlled below 50°C throughout the process.
[0029] Example 2 Crosslinking agent: tetrabutyl ketone oxime silane; curing agent: aminopropyl triethoxy silane
[0030] The colloid provided in this embodiment uses tetrabutyl ketone oxime silane as a cross-linking agent, and the main preparation process is: (1) first add 100 parts of 107 glue, 12 parts of tetrabutyl ketone oxime silane, 40 parts of dimethyl silicone oil, and 0.2 parts of Guangdong Dimei's BCO-2 mildew inhibitor, and stir in vacuum for 30-40 minutes at a stirring speed of 300-400 rpm; (2) then add 16 parts of fumed silica and stir evenly, and stir in vacuum at high speed for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally add 1 part of aminopropyl triethoxysilane and 0.2 parts of dibutyltin dilaurate, and stir in vacuum for 20-30 minutes. The reaction temperature needs to be controlled below 50°C throughout the process.
[0031] Example 3 Crosslinking agent: propyl tributylidene oxime silane; curing agent: aminopropyl triethoxy silane
[0032] The colloid provided in this embodiment uses propyl trisbutyl ketoxime silane as a cross-linking agent, and the main preparation process is: (1) first add 100 parts of 107 glue, 12 parts of propyl trisbutyl ketoxime silane, 40 parts of dimethyl silicone oil, and 0.2 parts of BCO-2 mildew inhibitor from Guangdong Dimei, and stir in vacuum for 30-40 minutes at a stirring speed of 300-400 rpm; (2) then add 16 parts of fumed silica and stir evenly, and stir in vacuum at high speed for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally add 1 part of aminopropyl triethoxysilane and 0.2 parts of dibutyltin dilaurate, and stir in vacuum for 20-30 minutes. The reaction temperature needs to be controlled below 50°C throughout the process.
[0033] Example 4 Crosslinking agent: methyl tributylacetoximate silane + tetrabutyl ketone oxime silane; curing agent: aminopropyl triethoxysilane
[0034] The colloid provided in this embodiment uses a compound of methyl tributylacetoximate silane and tetrabutyl ketone oxime silane as a crosslinking agent, wherein the mass ratio of methyl tributylacetoximate silane to tetrabutyl ketone oxime silane is 3:1. The main preparation process is: (1) first add 100 parts of 107 glue, 12 parts of methyl tributylacetoximate silane and tetrabutyl ketone oxime silane (mass ratio is 3:1), 40 parts of dimethyl silicone oil, and 0.2 parts of Guangdong Dimei's BCO-2 mildew inhibitor; , vacuum stirring for 30-40 minutes at a stirring speed of 300-400 rpm; (2) adding 16 parts of fumed silica and stirring evenly, vacuum stirring at high speed for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally adding 1 part of aminopropyltriethoxysilane and 0.2 parts of dibutyltin dilaurate, vacuum stirring for 20-30 minutes, and the reaction temperature needs to be controlled below 50°C throughout the process.
[0035] Example 5 Crosslinking agent: methyl tributylacetonate oxime silane + propyl tributylacetonate oxime silane + tetrabutyl ketone oxime silane; curing agent: aminopropyl triethoxysilane
[0036] The colloid provided in this embodiment uses methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane as a crosslinking agent, wherein the mass ratio of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane is 7:4:1. The main preparation process is as follows: (1) first add 100 parts of 107 glue, 12 parts of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane (mass ratio is 7:4:1), 40 parts of dimethyl silicone oil, (1) add 0.2 parts of BCO-2 mildew inhibitor produced by Guangdong Dimei, stir under vacuum for 30-40 minutes at a stirring speed of 300-400 rpm; (2) add 16 parts of fumed silica and stir evenly, stir at high speed under vacuum for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally add 1 part of aminopropyl triethoxysilane and 0.2 parts of dibutyltin dilaurate, stir under vacuum for 20-30 minutes, and the reaction temperature must be controlled below 50°C throughout the process.
[0037] Example 6 Crosslinking agent: methyl tributylacetoximate silane + propyl tributylacetoximate silane + tetrabutyl ketone oxime silane; curing agent: (aminoethyl) aminopropyl trimethoxysilane
[0038] The colloid provided in this embodiment uses methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane as a crosslinking agent, wherein the mass ratio of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane is 7:4:1. The main preparation process is as follows: (1) first add 100 parts of 107 glue, 12 parts of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane (mass ratio is 7:4:1), 40 parts of dimethyl silicone oil, Guangdong Di (1) add 0.2 parts of Midea BCO-2 mildew inhibitor, stir under vacuum for 30-40 minutes at a stirring speed of 300-400 rpm; (2) add 16 parts of fumed silica and stir evenly, stir at high speed under vacuum for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally add 1 part of (aminoethyl)aminopropyltrimethoxysilane and 0.2 parts of dibutyltin dilaurate, stir under vacuum for 20-30 minutes, and the reaction temperature must be controlled below 50°C throughout the process.
[0039] Example 7 Crosslinking agent: methyl tributylacetoximate silane + phenyl tributylacetoximate silane + tetrabutyl ketone oxime silane; curing agent: (aminoethyl) aminopropyl trimethoxysilane
[0040] The colloid provided in this embodiment uses methyl tributylacetoximosilane, phenyl tributylacetoximosilane and tetrabutyl ketone oxime silane as a crosslinking agent, wherein the mass ratio of methyl tributylacetoximosilane, phenyl tributylacetoximosilane and tetrabutyl ketone oxime silane is 7:4:1. The main preparation process is as follows: (1) first add 100 parts of 107 glue, 12 parts of methyl tributylacetoximosilane, phenyl tributylacetoximosilane and tetrabutyl ketone oxime silane (mass ratio is 7:4:1), 40 parts of dimethyl silicone oil, Guangdong Di (1) add 0.2 parts of Midea BCO-2 mildew inhibitor, stir under vacuum for 30-40 minutes at a stirring speed of 300-400 rpm; (2) add 16 parts of fumed silica and stir evenly, stir at high speed under vacuum for 30-40 minutes at a stirring speed of 900-1000 rpm; (3) finally add 1 part of (aminoethyl)aminopropyltrimethoxysilane and 0.2 parts of dibutyltin dilaurate, stir under vacuum for 20-30 minutes, and the reaction temperature must be controlled below 50°C throughout the process.
[0041] Example 8 Detection and Analysis
[0042] The properties of the mildew-proof adhesives prepared in Examples 1 to 7 were investigated respectively, wherein the crosslinking density was calculated according to the ratio of unit mass to volume; the surface dryness was tested according to GB / T 13477.5-2002; the bonding strength was tested according to GB / T 13477.18-2002; the elongation at break was tested according to GB / T 528-2009; the tensile strength was tested according to GB / T 528-2009; the hardness was tested according to GB / T 531.1-2008 for sample preparation and testing; the mildew resistance level was entrusted to Guangdong Microbiological Analysis and Testing Center for testing, where level 0 - no obvious mildew growth under about 50 times magnification, level 1 - mildew growth is not visible to the naked eye, level 2 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is 10% to 30%, level 3 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is 30% to 60%, and level 4 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is greater than 60%. The test sample is an environment with a humidity of 80%, and the sample is 3 months after the glue is applied. The test results are shown in Table 1.
[0043] Table 1. Comparison of the performance of mildew-proof adhesives
[0044]
[0045]
[0046] As can be seen from Table 1, according to Example 1, Example 2, Example 3, Example 4, and Example 5, when aminopropyl triethoxysilane is used as a curing agent, when a methyl tributylanoxime silane (Example 1), or tetrabutyl ketoxime silane (Example 2), or propyl tributylanoxime silane (Example 3) is used alone as a cross-linking agent, the obtained colloid mildew-proof effect is significantly poor, and mildew can be clearly seen after three months, while when methyl tributylanoxime silane and tetrabutyl ketoxime silane are compounded as a cross-linking agent (Example 4), the mildew-proof effect of the obtained colloid is significantly poor. The cross-linking density reaches 2.56 g / ml, the mildew resistance level is significantly improved to level 1, and the colloid mechanical properties are also more excellent, and the bonding strength, elongation at break, tensile strength and hardness are improved to a certain extent; when methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane are compounded (Example 5), the mildew resistance level is further increased to level 0, the cross-linking density reaches 3.05 g / ml, the elongation at break reaches 890%, and the colloid mechanical properties are further improved.
[0047] Comparing Example 5 and Example 6, it can be seen that when (aminoethyl)aminopropyltrimethoxysilane is used as the curing agent (Example 6), the colloid bonding performance is further improved, so (aminoethyl)aminopropyltrimethoxysilane is better used in combination with a cross-linking agent prepared by mixing methyltributylacetonatoximosilane, propyltributylacetonatoximosilane and tetrabutylketoximesilane, and a dense colloid with higher cross-linking density can be obtained, so that the cross-linking density reaches 3.21g / ml, the elongation at break reaches 920%, and the mildew resistance grade reaches the highest grade 0.
[0048] In addition, by comparing Example 6 with Example 7, when phenyltributylacetonate oxime silane, methyltributylacetonate oxime silane and tetrabutylketone oxime silane are used as the crosslinking agent (Example 7), the crosslinking effect is not ideal, the mildew resistance level is not high, and the colloid mechanical properties are not significantly improved.
[0049] In summary, when methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane are used as cross-linking agents, and (aminoethyl) aminopropyl trimethoxysilane or aminopropyl triethoxysilane is used as a curing agent, a long-lasting mildew-proof adhesive with significantly improved mechanical properties, very high density and mildew-proof grade of more than level 1 can be obtained. Especially when (aminoethyl) aminopropyl trimethoxysilane is used as the curing agent, the mildew-proof grade can reach level 0, and the mechanical properties are very excellent.
[0050] Example 9 Effect of different ratios of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl ketone oxime silane
[0051] In this embodiment, the method provided in Example 6 is used to prepare the mildew-proof glue, wherein the ratio of methyl tributylanoxime silane, propyl tributylanoxime silane and tetrabutyl tributylanoxime silane is 5:2:1, 6:3:1, 7:4:1, 8:5:1, 9:5:1 and 10:5:1 respectively. The properties of the mildew-proof glue are investigated respectively, wherein the crosslinking density is calculated according to the ratio of unit mass to volume; the surface dryness is tested according to GB / T 13477.5-2002; the bonding strength is tested according to GB / T 13477.18-2002; the elongation at break is tested according to GB / T 528-2009; the tensile strength is tested according to GB / T 528-2009; the hardness is tested according to GB / T 531.1-2008 for sample preparation and testing; the mildew resistance level was entrusted to the Guangdong Microbiological Analysis and Testing Center for testing, where level 0 - no obvious mildew growth under about 50 times magnification, level 1 - mildew growth is not visible to the naked eye, level 2 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is 10% to 30%, level 3 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is 30% to 60%, and level 4 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is greater than 60%. The test sample is an environment with a humidity of 80%, and the sample is 3 months after the glue is applied. The test results are shown in Table 2.
[0052] Table 2. Effect of different ratios of methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl ketone oxime silane
[0053]
[0054] As can be seen from Table 2, different ratios of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl tributylacetoximosilane have a great influence on the performance of the obtained mildew-proof glue. When the ratio range is within the range of 6-9:3-5:1, the obtained mildew-proof glue has a higher crosslinking density, and the bonding strength, tensile strength and hardness are significantly better. The elongation at break is also maintained within a relatively good range, and the mildew-proof grade reaches above grade 1, which meets the requirements of environmentally friendly long-lasting mildew-proof glue; among them, the ratio range of 7:4:1 is the best choice, and the obtained mildew-proof glue has the best bonding strength, tensile strength and hardness, the elongation at break is as high as 920%, and the mildew-proof grade reaches grade 0.
[0055] Example 10 Effect of different ratios of crosslinking agent and curing agent
[0056] In this embodiment, the method provided in Example 6 is used to prepare the mildew-proof adhesive, wherein the crosslinking agent is methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane (mass ratio is 7:4:1), the curing agent is (aminoethyl) aminopropyl trimethoxysilane, and the ratio of the crosslinking agent to the curing agent is 5:1, 10:1, 12:1, 15:1, 17:1 and 20:1, respectively. The properties of the mildew-proof adhesive prepared are investigated respectively, wherein the crosslinking density is calculated according to the ratio of unit mass to volume; the surface dryness is tested according to GB / T13477.5-2002; the bonding strength is tested according to GB / T 13477.18-2002; the elongation at break is tested according to GB / T 528-2009; the tensile strength is tested according to GB / T 528-2009; the hardness is tested according to GB / T 531.1-2008 for sample preparation and testing; the mildew resistance level was entrusted to the Guangdong Microbiological Analysis and Testing Center for testing, where level 0 - no obvious mildew growth under about 50 times magnification, level 1 - mildew growth is not visible to the naked eye, level 2 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is 10% to 30%, level 3 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is 30% to 60%, and level 4 - mildew growth is obviously visible to the naked eye, and the sample surface coverage area is greater than 60%. The test sample is an environment with a humidity of 80%, and the sample is 3 months after the glue is applied. The test results are shown in Table 2.
[0057] Table 3. Effect of different ratios of crosslinking agent and curing agent
[0058] Crosslinking agent: curing agent 5:1 10:1 12:1 15:1 17:1 20:1 Surface dry(min) 19 18 15 17 18 18 Crosslinking density (g / ml) 2.59 2.87 3.21 2.91 2.67 2.18 Bonding (glass to aluminum block) OK OK OK OK OK OK Bond strength(Mpa) 0.8 1.4 1.63 1.32 1.1 0.92 24H curing depth (mm) 2.2 2.5 2.5 2.5 2.4 2.0 Elongation at break (%) 570 730 920 770 550 520 Tensile strength(Mpa) 0.7 1.2 1.6 1.32 0.9 0.93 Hardness (Shore A) 24 31 39 33 25 25 Mildew resistance level Level 2 Level 1 Level 0 Level 1 Level 2 Level 2
[0059] As can be seen from Table 3, the different ratios of the cross-linking agent composed of methyl tributylacetoximosilane, propyl tributylacetoximosilane and tetrabutyl tributylacetoximosilane and the curing agent (aminoethyl) aminopropyl trimethoxysilane have a great influence on the performance of the obtained mildew-proof adhesive. When the ratio range is within the range of 10:1 to 15:1, the obtained mildew-proof adhesive has a higher cross-linking density, and the bonding strength, tensile strength and hardness are significantly better. The elongation at break is also maintained within a relatively good range, and the mildew-proof grade reaches above grade 1, which meets the requirements of environmentally friendly long-term mildew-proof adhesive. Among them, the ratio range of 12:1 is the best choice, and the obtained mildew-proof adhesive has the best bonding strength, tensile strength and hardness, the elongation at break is as high as 920%, and the mildew-proof grade reaches grade 0.
[0060] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A combination of a crosslinking agent and a curing agent for preparing a long-lasting mildew-proof adhesive for improving the crosslinking density and bonding strength of the colloid, characterized in that: The cross-linking agent is composed of methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane, and the mass ratio of the methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane is 7:4:1; the curing agent is (aminoethyl) aminopropyl trimethoxysilane; the mass ratio of the cross-linking agent to the curing agent is 12:1; the long-lasting mildew-proof glue is composed of 100 parts of 107 glue, 12 parts of cross-linking agent, 0.2 parts of mildew-proof agent, 1 part of curing agent, 40 parts of plasticizer, 0.2 parts of catalyst and 16 parts of filler; the plasticizer is dimethyl silicone oil; the catalyst is dibutyl tin dilaurate, and the filler is fumed white carbon black.
2. The use according to claim 1, characterized in that The mildew preventer is BCO-2 mildew preventer produced by Guangdong Dimei.
3. A long-lasting mildew-proof adhesive for use as claimed in claim 1 or 2, characterized in that: The long-acting mildew-proof glue is composed of 100 parts of 107 glue, 12 parts of cross-linking agent, 0.2 parts of mildew-proof agent, 1 part of curing agent, 40 parts of plasticizer, 0.2 parts of catalyst and 16 parts of filler; the cross-linking agent is composed of methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane, and the mass ratio of methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane is 7:4:1; the curing agent is (aminoethyl)aminopropyltrimethoxysilane; the mass ratio of the cross-linking agent to the curing agent is 12:
1.
4. A method for preparing the long-lasting mildew-proof adhesive for use as claimed in claim 1 or 2, characterized in that: (1) First add 107 glue, crosslinking agent, plasticizer and mildewproof agent, and stir in vacuum for 30-40 minutes; (2) Then add fumed silica and stir evenly, and stir in vacuum at high speed for 30-40 minutes; (3) Finally, add curing agent and catalyst and stir in vacuum for 20-30 minutes. The reaction temperature should be controlled below 50°C during the whole process; The cross-linking agent is composed of methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane, and the mass ratio of the methyl tributylacetoximate silane, propyl tributylacetoximate silane and tetrabutyl tributylacetoximate silane is 7:4:1; the curing agent is (aminoethyl) aminopropyl trimethoxysilane; the mass ratio of the cross-linking agent to the curing agent is 12:1.
Citation Information
Patent Citations
Ketonic oxime type silicone sealant and preparation method thereof
CN108192561A