A low-cost denitration catalyst slurry and its preparation method and application
By sand or ball milling using raw materials such as tungsten, vanadium, molybdenum, etc., a low-cost denitrification catalyst slurry with high dispersion and suspension is prepared, which solves the problems of complex processes and high costs in the existing technology, and realizes the Efficient application of integrated dust removal and denitrification materials.
Patent Information
- Application Number
- CN202210811649.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-07-11
AI Technical Summary
The preparation process of existing porous ceramic materials supported denitrification catalysts is complex, with long cycles and high cost, resulting in poor dispersion, suspension and wetting of the slurry of denitrification catalysts, limiting the promotion and application of integrated dust removal and denitrification materials.
Using tungsten, vanadium, molybdenum, titanium, silicon sol, ammonia, organic surfactants and inorganic colloids as raw materials, low-cost denitrification catalyst slurry is prepared through sand or ball milling processes, increasing particle dispersion and suspension , suitable for porous materials with pore sizes of more than 2 μm.
The preparation process is simplified, the cost is reduced, the high dispersion, suspension and wetting are achieved, and the channel is avoided. It is suitable for the application of large-scale production and integrated dust removal and denitrification materials.
Smart Images

Figure CN115254199B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flue gas purification, and in particular to a low-cost denitration catalyst slurry and a preparation method and application thereof. Background Art
[0002] The integrated dust removal and denitrification material is a functional material formed by the efficient composite of porous ceramic materials and nano-denitrification catalysts. It combines the filtration principle of porous ceramic materials with the selective catalyst reduction denitrification mechanism, and can achieve dust removal and denitrification functions at the same time. It can be widely used in high-temperature flue gas purification, which is conducive to the simplification of industrial flue gas treatment equipment and the intensification of corporate processes.
[0003] At present, the main methods for loading denitration catalysts on porous ceramic materials include sol-gel method, coprecipitation method, impregnation method, etc. After loading the denitration catalyst inside or on the surface of the porous ceramic material, the integrated dust removal and denitration material is obtained by heat treatment. However, compared with the impregnation method, the sol-gel method and the coprecipitation method have problems such as complex preparation process, long production cycle, and high cost. The impregnation method has become the mainstream preparation process. The impregnation method usually adopts the method of coating the denitration catalyst slurry on the inside or surface of the porous ceramic material pores to achieve the loading of the denitration catalyst inside or on the surface of the porous ceramic material pores. However, the denitration catalyst slurry used for the impregnation method is not mature at present, and generally has problems such as poor dispersibility, poor suspension, and poor wettability, which greatly restricts the promotion and application of integrated dust removal and denitration materials; in addition, in the preparation process of the denitration catalyst slurry, it is necessary to prepare the catalyst precursor by spray drying or kneading, and then heat treatment and ball milling in sequence, and then grind the catalyst slurry after mixing a variety of additives. The preparation process is complicated, the cycle is long, and the batch production cost is high. Summary of the invention
[0004] To solve the above problems, the present invention provides a low-cost denitration catalyst slurry and a preparation method and application thereof. The preparation method has a simple process, a short cycle, safe operation, low cost, and can be scalably produced. The prepared denitration catalyst slurry has small particles, high dispersibility, suspension and wettability, and is suitable for coating porous materials with a pore size of 2μm or more, and is not easy to clog the pores of the porous materials during coating.
[0005] On the one hand, the present invention provides a method for preparing a low-cost denitration catalyst slurry, comprising the following steps: preparing a denitration catalyst precursor, wherein the denitration catalyst precursor is a mixture of a tungsten source, a vanadium source, a molybdenum source, a titanium source, a silica sol, an ammonia solution, an organic surfactant, an inorganic colloid, and water; and sand milling or ball milling the denitration catalyst precursor to obtain the low-cost denitration catalyst slurry.
[0006] In some embodiments of the present invention, the denitration catalyst precursor is mixed by weight: 6-12 parts of tungsten source, 10-15 parts of vanadium source, 6-12 parts of molybdenum source, 60-85 parts of titanium source, 3-6 parts of silica sol, 15-20 parts of ammonia water, 5-10 parts of organic surfactant, 0.5-1 part of inorganic colloid, and 60-90 parts of water.
[0007] In some embodiments of the present invention, the tungsten source is ammonium metatungstate, the vanadium source is ammonium metavanadate, the molybdenum source is ammonium molybdate, and the titanium source is metatitanic acid and / or titanium dioxide. The purity of the ammonium metatungstate, ammonium metavanadate, ammonium molybdate, metatitanic acid, and titanium dioxide is preferably above 98%.
[0008] In some embodiments of the present invention, the silica sol is alkaline silica sol, and the silicon content in the silica sol is 30-40 wt %.
[0009] In some embodiments of the present invention, the organic surfactant is diethylamine or acetylene glycol or polyacrylamine.
[0010] In some embodiments of the present invention, the inorganic colloid is bentonite or magnesium aluminum silicate.
[0011] In some embodiments of the present invention, when the denitration catalyst precursor is sand-milled, the sand-milling time is 30-60 minutes; when the denitration catalyst precursor is ball-milled, the ball-milling time is 6-10 hours.
[0012] In some embodiments of the present invention, after the denitration catalyst precursor is sand-milled or ball-milled, 5-10 parts by weight of an organic surfactant is added, and the mixture is stirred evenly to obtain the low-cost denitration catalyst slurry.
[0013] On the other hand, the present invention further provides a low-cost denitration catalyst slurry, which is prepared according to any of the preparation methods described above.
[0014] On the other hand, the present invention also provides an application of the low-cost denitration catalyst slurry, wherein the low-cost denitration catalyst slurry is coated inside the pores of a porous material with a pore size of 2 μm or more to obtain an integrated dust removal and denitration material.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The preparation method of the present invention uses tungsten source, vanadium source, molybdenum source, titanium source, silica sol, ammonia water, organic surfactant, inorganic colloid and water as raw materials, and adopts sand milling or ball milling process to prepare denitration catalyst slurry. Compared with the traditional method of "spray drying or kneading followed by heat treatment and ball milling, mixing with multiple additives and then grinding to obtain catalyst slurry", the present invention only adopts sand milling or ball milling process, and the preparation process is simple, the cycle is short, the operation is safe, the cost is low, and large-scale production can be achieved; in the preparation process of the denitration catalyst slurry, the present invention adopts silica sol to increase thermal stability, ammonia water to provide an alkaline environment, and an organic surfactant and an inorganic colloid (slurry stabilizer) system. Under the joint action of these two types of substances, the solid particles in the catalyst slurry are well dispersed, and the catalyst slurry has good suspension at a lower viscosity and is not easy to precipitate. The solid particles in the prepared denitration catalyst slurry have small grains, high dispersibility, suspension and wettability, and can be suitable for coating porous materials with a pore size of 2μm or more, and are not easy to block the pores of the porous materials during coating.
[0017] (2) The preparation method of the present invention limits the formula of the denitration catalyst precursor to a mixture of 6-12 parts of tungsten source, 10-15 parts of vanadium source, 6-12 parts of molybdenum source, 60-85 parts of titanium source, 3-6 parts of silica sol, 15-20 parts of ammonia water, 5-10 parts of organic surfactant, 0.5-1 part of inorganic colloid, and 60-90 parts of water. The denitration catalyst precursor prepared by this formula is more conducive to subsequent sand milling or ball milling, and can ensure good dispersibility while ensuring particle refinement; in addition, the present invention preferably prepares the denitration catalyst precursor 5-10 parts of organic surfactant are added at the same time, and 5-10 parts by weight of organic surfactant are added after sand milling or ball milling. The organic surfactant is added twice. A small amount of organic surfactant is added during sand milling or ball milling, and the organic surfactant will not become ineffective due to heat while ensuring dispersion. The second addition of organic surfactant after sand milling or ball milling is further conducive to dispersion, avoiding the problem of a large amount of organic surfactant being added at one time, causing the organic surfactant to become ineffective due to heat during sand milling or ball milling, and agglomeration and inability to disperse in the later period.
[0018] (3) The organic surfactant selected in the present invention is diethylamine or acetylene glycol or polyacrylamide, and the inorganic colloid is bentonite or magnesium aluminum silicate. Diethylamine or acetylene glycol or polyacrylamide is a small molecule surfactant. These small molecules will form a double electron layer on the surface of the solid particles in the denitration catalyst slurry. Under the action of the charge, the particles can be better separated, giving the denitration catalyst slurry better dispersibility; bentonite or magnesium aluminum silicate has a lamellar structure, which can be combined with water to expand into a suspended and stable colloid, will not be eroded by microorganisms, will not deteriorate or mold after long-term storage, and the viscosity does not change with temperature; the surfactant selected in the present invention can be quickly and evenly dispersed in the entire system, will not migrate on the surface, and the smaller molecular weight will not be broken up or destroyed during the rapid dispersion process, and the surface tension is lower in static and dynamic conditions. With the cooperation of the organic surfactant and the inorganic colloid of the present invention, the viscosity of the denitration catalyst slurry can be regulated, that is, the dispersibility of the denitration catalyst slurry can be ensured, and the suspension of the denitration catalyst slurry can be improved, and the viscosity can be reduced, so that the prepared denitration catalyst slurry is more stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required to be used in the embodiments of the present invention will be described below.
[0020] Figure 1 A particle size distribution diagram of particles in a low-cost denitration catalyst slurry prepared by a preparation method according to an embodiment of the present invention;
[0021] Figure 2 A particle size distribution diagram of particles in a low-cost denitration catalyst slurry prepared by a preparation method according to another embodiment of the present invention;
[0022] Figure 3 This is a particle size distribution diagram of particles in a low-cost denitration catalyst slurry prepared by a preparation method according to another embodiment of the present invention. DETAILED DESCRIPTION
[0023] In order to make the objectives, technical solutions and advantages of the present invention more clear, various aspects of the present invention will be described in detail below in conjunction with specific embodiments. However, these specific embodiments are only used to illustrate the present invention and do not constitute any limitation on the scope of protection and essential content of the present invention.
[0024] The present invention provides a method for preparing a low-cost denitration catalyst slurry, comprising the following steps: preparing a denitration catalyst precursor, wherein the denitration catalyst precursor is prepared by mixing a tungsten source, a vanadium source, a molybdenum source, a titanium source, a silica sol, an ammonia solution, an organic surfactant, an inorganic colloid, and water; and sand milling or ball milling the denitration catalyst precursor to obtain a low-cost denitration catalyst slurry.
[0025] In the present invention, the denitration catalyst precursor is prepared by mixing 6-12 parts of tungsten source, 10-15 parts of vanadium source, 6-12 parts of molybdenum source, 60-85 parts of titanium source, 3-6 parts of silica sol, 15-20 parts of ammonia water, 5-10 parts of organic surfactant, 0.5-1 part of inorganic colloid and 60-90 parts of water by weight.
[0026] In the present invention, the tungsten source is ammonium metatungstate, the vanadium source is ammonium metavanadate, the molybdenum source is ammonium molybdate, and the titanium source is metatitanic acid and / or titanium dioxide. Preferably, the purity of ammonium metatungstate, ammonium metavanadate, ammonium molybdate, metatitanic acid, and titanium dioxide is above 98%.
[0027] In the present invention, the silica sol is alkaline silica sol, and the silicon content in the silica sol is 30-40wt%.
[0028] In the present invention, the organic surfactant is diethylamine, acetylene glycol or polyacrylamide, and the inorganic colloid is bentonite or magnesium aluminum silicate.
[0029] In the present invention, when the denitration catalyst precursor is sand-milled, the sand-milling time is 30-60 minutes; when the denitration catalyst precursor is ball-milled, the ball-milling time is 6-10 hours.
[0030] In the present invention, after sand milling or ball milling the denitration catalyst precursor, 5-10 parts by weight of an organic surfactant is added, and the mixture is stirred evenly to obtain a low-cost denitration catalyst slurry.
[0031] The present invention also provides a low-cost denitration catalyst slurry, which is prepared according to the preparation method of the present invention.
[0032] The present invention also provides an application of the low-cost denitration catalyst slurry prepared by the present invention, and the low-cost denitration catalyst slurry prepared by the present invention is coated inside the pores of a porous ceramic material with a pore diameter of more than 2 μm to obtain an integrated dust removal and denitration material.
[0033] Embodiment 1:
[0034] This embodiment provides a method for preparing a low-cost denitration catalyst slurry, comprising the following steps:
[0035] Weigh 6 parts of tungsten source, 10 parts of vanadium source, 6 parts of molybdenum source, 60 parts of titanium source, 3 parts of silica sol, 15 parts of ammonia water, 5 parts of organic surfactant, 0.5 parts of inorganic colloid, and 60 parts of water by weight, pour them into a stirring bucket for mixing, and stir them evenly to obtain a denitration catalyst precursor;
[0036] The denitration catalyst precursor is sand-milled for 30-60 minutes (preferably, 30 minutes) by a sand mill, the ground slurry is poured into a stirring barrel, and then 5 parts by weight of an organic surfactant is added, and stirred thoroughly (preferably, stirred for 10 minutes) to obtain a low-cost denitration catalyst slurry.
[0037] In this embodiment, the tungsten source is ammonium metatungstate, the vanadium source is ammonium metavanadate, the molybdenum source is ammonium molybdate, and the titanium source is metatitanic acid. Preferably, the purity of ammonium metatungstate, ammonium metavanadate, ammonium molybdate, and metatitanic acid is above 98%.
[0038] In this embodiment, the silica sol is alkaline silica sol, and the silicon content in the silica sol is 30-40wt%.
[0039] In this embodiment, the organic surfactant is diethylamine, and the inorganic colloid is bentonite.
[0040] This embodiment also provides a low-cost denitration catalyst slurry, which is prepared according to the preparation method of this embodiment. Figure 1 As shown, the particle size distribution in the low-cost denitration catalyst slurry prepared by the preparation method of this embodiment is shown. It can be seen from the figure that the particle size in the low-cost denitration catalyst slurry prepared by the preparation method of this embodiment is less than 1 μm, D50=0.067 μm.
[0041] This embodiment also provides an application of a low-cost denitration catalyst slurry prepared by the preparation method of this embodiment, and the low-cost denitration catalyst slurry prepared by this embodiment is coated on the inside of the pores of a porous ceramic material with a pore size of 2 μm or more to obtain a dust removal and denitration integrated material. The low-cost denitration catalyst slurry prepared by this embodiment has small grains, and D50 is only 0.067 μm, and the prepared low-cost denitration catalyst slurry has high dispersibility, suspension and wettability, and can be successfully coated on a porous material with a pore size of 2 μm or more, and it is not easy to block the pores of the porous material during coating, and can be used to prepare a dust removal and denitration integrated material.
[0042] Embodiment 2:
[0043] This embodiment provides a method for preparing a low-cost denitration catalyst slurry, comprising the following steps:
[0044] Weigh 8 parts of tungsten source, 12 parts of vanadium source, 8 parts of molybdenum source, 70 parts of titanium source, 5 parts of silica sol, 17 parts of ammonia water, 7 parts of organic surfactant, 0.7 parts of inorganic colloid, and 80 parts of water by weight, and mix them to obtain a denitration catalyst precursor;
[0045] The denitration catalyst precursor is poured into a horizontal ball mill and ball-milled for 6-10 hours (preferably, 8 hours), the ground slurry is poured into a stirring barrel, and then 7 parts by weight of an organic surfactant is added, and stirred thoroughly (preferably, stirred for 10 minutes) to obtain a low-cost denitration catalyst slurry.
[0046] In this embodiment, the tungsten source is ammonium metatungstate, the vanadium source is ammonium metavanadate, the molybdenum source is ammonium molybdate, and the titanium source is titanium dioxide. Preferably, the purity of ammonium metatungstate, ammonium metavanadate, ammonium molybdate, and titanium dioxide is above 98%.
[0047] In this embodiment, the silica sol is alkaline silica sol, and the silicon content in the silica sol is 30-40wt%.
[0048] In this embodiment, the organic surfactant is acetylene glycol, and the inorganic colloid is magnesium aluminum silicate.
[0049] This embodiment also provides a low-cost denitration catalyst slurry, which is prepared according to the preparation method of this embodiment. Figure 2 As shown, the particle size distribution in the low-cost denitration catalyst slurry prepared by the preparation method of this embodiment is shown. It can be seen from the figure that the particle size in the low-cost denitration catalyst slurry prepared by the preparation method of this embodiment is less than 1 μm, D50=0.063 μm.
[0050] This embodiment also provides an application of a low-cost denitration catalyst slurry prepared by the preparation method of this embodiment, and the low-cost denitration catalyst slurry prepared by this embodiment is coated on the inside of the pores of a porous ceramic material with a pore size of 2 μm or more to obtain a dust removal and denitration integrated material. The low-cost denitration catalyst slurry prepared by this embodiment has small grains, and D50 is only 0.063 μm, and the prepared low-cost denitration catalyst slurry has high dispersibility, suspension and wettability, and can be successfully coated on a porous material with a pore size of 2 μm or more, and it is not easy to block the pores of the porous material during coating, and can be used to prepare a dust removal and denitration integrated material.
[0051] Embodiment 3:
[0052] This embodiment provides a method for preparing a low-cost denitration catalyst slurry, comprising the following steps:
[0053] Weigh 12 parts of tungsten source, 15 parts of vanadium source, 12 parts of molybdenum source, 85 parts of titanium source, 6 parts of silica sol, 20 parts of ammonia water, 10 parts of organic surfactant, 1 part of inorganic colloid, and 90 parts of water by weight, pour them into a stirring bucket for mixing, and stir evenly to obtain a denitration catalyst precursor;
[0054] The denitration catalyst precursor is sand-milled for 30-60 minutes (preferably, 60 minutes) by a sand mill, the ground slurry is poured into a stirring barrel, and then 10 parts by weight of an organic surfactant is added, and stirred thoroughly (preferably, stirred for 10 minutes) to obtain a low-cost denitration catalyst slurry.
[0055] In this embodiment, the tungsten source is ammonium metatungstate, the vanadium source is ammonium metavanadate, the molybdenum source is ammonium molybdate, and the titanium source is metatitanic acid and titanium dioxide. Preferably, the purity of ammonium metatungstate, ammonium metavanadate, ammonium molybdate, metatitanic acid, and titanium dioxide is above 98%.
[0056] In this embodiment, the silica sol is alkaline silica sol, and the silicon content in the silica sol is 30-40wt%.
[0057] In this embodiment, the organic surfactant is polyacrylamide and the inorganic colloid is bentonite.
[0058] This embodiment also provides a low-cost denitration catalyst slurry, which is prepared according to the preparation method of this embodiment. Figure 3 As shown, the particle size distribution in the low-cost denitration catalyst slurry prepared by the preparation method of this embodiment is shown. It can be seen from the figure that the particle size in the low-cost denitration catalyst slurry prepared by the preparation method of this embodiment is less than 1 μm, D50=0.061 μm.
[0059] This embodiment also provides an application of a low-cost denitration catalyst slurry prepared by the preparation method of this embodiment, and the low-cost denitration catalyst slurry prepared by this embodiment is coated on the inside of the pores of a porous ceramic material with a pore size of 2 μm or more to obtain a dust removal and denitration integrated material. The low-cost denitration catalyst slurry prepared by this embodiment has small grains, and D50 is only 0.061 μm, and the prepared low-cost denitration catalyst slurry has high dispersibility, suspension and wettability, and can be successfully coated on a porous material with a pore size of 2 μm or more, and it is not easy to block the pores of the porous material during coating, and can be used to prepare a dust removal and denitration integrated material.
[0060] The present invention has been described above in conjunction with specific embodiments. These specific embodiments are merely exemplary and cannot be used to limit the scope of protection of the present invention. Those skilled in the art may make various modifications, changes or substitutions without departing from the essence of the present invention. Therefore, various equivalent changes made according to the present invention still fall within the scope covered by the present invention.
Claims
1. A method for preparing a low-cost denitration catalyst slurry, characterized in that: The following steps are involved: Preparing a denitration catalyst precursor, wherein the denitration catalyst precursor is prepared by mixing a tungsten source, a vanadium source, a molybdenum source, a titanium source, a silica sol, an ammonia solution, an organic surfactant, an inorganic colloid, and water; Sand milling or ball milling the denitration catalyst precursor to obtain the low-cost denitration catalyst slurry; The denitration catalyst precursor is prepared by mixing 6-12 parts of tungsten source, 10-15 parts of vanadium source, 6-12 parts of molybdenum source, 60-85 parts of titanium source, 3-6 parts of silica sol, 15-20 parts of ammonia water, 5-10 parts of organic surfactant, 0.5-1 part of inorganic colloid, and 60-90 parts of water; the silica sol is alkaline silica sol, and the silicon content in the silica sol is 30-40wt%; the organic surfactant is diethylamine or acetylene glycol; The inorganic colloid is bentonite or magnesium aluminum silicate.
2. The preparation method according to claim 1, characterized in that The tungsten source is ammonium metatungstate, the vanadium source is ammonium metavanadate, the molybdenum source is ammonium molybdate, and the titanium source is metatitanic acid and / or titanium dioxide.
3. The preparation method according to claim 1, characterized in that: When the denitration catalyst precursor is sand-milled, the sand-milling time is 30-60 minutes; when the denitration catalyst precursor is ball-milled, the ball-milling time is 6-10 hours.
4. The preparation method according to claim 1, characterized in that: After sand milling or ball milling the denitration catalyst precursor, 5-10 parts by weight of an organic surfactant is added, and the mixture is stirred evenly to obtain the low-cost denitration catalyst slurry.
5. A low-cost denitration catalyst slurry, characterized in that: The low-cost denitration catalyst slurry is prepared according to the preparation method according to any one of claims 1 to 4.
6. The use of the low-cost denitration catalyst slurry according to claim 5, characterized in that: The low-cost denitration catalyst slurry is coated inside the pores of a porous material with a pore diameter of 2 μm or more to obtain a dust removal and denitration integrated material.