A method for quickly estimating the plasticity index of mineral powder for asphalt mixture
By combining the water-saturation-drying method with image processing, the detection process of the plasticity index of mineral powder is simplified, enabling rapid and accurate evaluation of mineral powder quality and solving the problems of cumbersome detection and low efficiency in existing technologies.
Patent Information
- Application Number
- CN202210950653.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-08-09
AI Technical Summary
Existing methods for detecting the plasticity index of mineral powder are cumbersome, inefficient, and yield inaccurate results, failing to meet the need for rapid screening of mineral powder quality.
The water-saturated-drying method is adopted, and the shrinkage cracking degree of mineral powder is calculated through image processing, which simplifies the operation process and quickly predicts the plasticity index of mineral powder.
A simple and rapid method for detecting the plasticity index of mineral powder is provided, which can obtain accurate test results within 24 hours, reducing workload and improving testing efficiency.
Smart Images

Figure CN115266484B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering material performance detection, and in particular relates to a method for quickly estimating the plasticity index of mineral powder for asphalt mixture. Background Art
[0002] Mineral powder is crucial to improving the performance of asphalt mixtures. Therefore, the industry standard "Technical Specifications for Highway Asphalt Pavement Construction" (JTG F40-2004) gives clear technical requirements for mineral powder. The corresponding technical indicators are shown in Table 1. The test methods for various indicators are given in the "Test Procedures for Highway Engineering Aggregates" (JTG E42-2005).
[0003] Table 1 Technical requirements for mineral powder used in asphalt mixture
[0004]
[0005] In the mineral powder index system in Table 1, the plasticity index is the most critical and is the core index for controlling the quality of mineral powder. The test method for this index is T0118 in the "Highway Geotechnical Test Code" (JTG E40-2007), which adopts the combined determination method of liquid limit and plastic limit.
[0006] (1) Deficiencies in the combined determination method of liquid limit and plastic limit (T0118-2007).
[0007] The main purpose of the T0118-2007 method is to determine the liquid limit and plastic limit of soil, which is used to classify soil, calculate natural consistency and plasticity index, and is used for highway engineering design and construction. The defects in the process of determining the plasticity index of mineral powder are as follows:
[0008] ①The test operation is cumbersome and complicated, and specimens with different water contents need to be prepared;
[0009] ② It is unclear what type of soil the mineral powder belongs to, so the determination of the liquid limit is not accurate, and thus the IP index is inaccurate;
[0010] ③The test time is long and the test results cannot be reflected immediately.
[0011] In project-level asphalt pavement construction projects, it is necessary to conduct a preliminary screening of the quality of mineral powders from different mineral powder manufacturers. If the T0118-2007 method is used to test the plasticity index, it will inevitably cause a huge waste of manpower and material resources. If a simple and visual method can be used to preliminarily judge the plasticity index of the mineral powder, and typical mineral powders are selected for liquid limit and plasticity testing, the testing workload will be greatly reduced, achieving twice the result with half the effort. Summary of the invention
[0012] The purpose of the present invention is to solve the problems of cumbersome operation and low efficiency of existing methods for testing the plasticity index of mineral powder, and to provide a method for quickly estimating the plasticity index of mineral powder for asphalt mixture. The method preliminarily determines the plasticity index of the mineral powder through the saturation-drying method, provides a simple and intuitive method for selecting mineral powder for asphalt mixture, reduces the frequency of plasticity index testing of mineral powder, and reduces laboratory workload.
[0013] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0014] A method for quickly estimating the plasticity index of mineral powder for asphalt mixture, the method specifically comprises:
[0015] Take 300±0.5g of mineral powder, saturate it with water in a shallow dish, let it be evenly distributed with equal thickness, then put it into an oven at 105℃±5℃ to dry it, let the mineral powder shrink freely, wait for the water to evaporate and the mineral powder to dry, take out the shallow dish, take pictures of the shrinkage state of the mineral powder and process the image, use image processing software to calculate the perimeter L of the mineral powder edge and the total length l of the shrinkage cracks in the edge, and use formula 1 to calculate the shrinkage crack degree S of the mineral powder saturation-drying method k ;
[0016]
[0017] Where: S k -mineral powder shrinkage crack degree, %; L-mineral powder edge circumference; l-total length of shrinkage cracks within the edge.
[0018] The larger the plasticity index of the mineral powder, the more shrinkage cracks there will be after saturation and drying. k Therefore, the size of the plasticity index can be determined by the shrinkage cracking degree of the mineral powder saturation-drying method.
[0019] Furthermore, the method steps are:
[0020] (1) Weigh 300g of mineral powder and put it into a circular ceramic or metal shallow dish with a height of 10-20mm and an inner diameter of Φ=20cm. The structure and dimensions of the shallow dish are as follows: Figure 1 As shown, the edge of the shallow dish should be at right angles to the bottom of the dish;
[0021] (2) Weigh 500g of water and mix it evenly with the mineral powder in the container using a glass rod to make the mineral powder fully saturated with water. The water must cover all the mineral powder;
[0022] (3) Place the container on a horizontal platform and allow the mixture of mineral powder and water to settle for 30 minutes. Then place the container in an oven at 105°C for at least 12 hours to ensure that the water in the container is completely evaporated. After the container is taken out and cooled, observe the crack state on the surface of the mineral powder. The denser the cracks and the wider the cracks, the larger the plasticity index, and vice versa.
[0023] (4) After the container is taken out and cooled, a mobile phone is used to vertically photograph the shrinkage state of the mineral powder in the container, and the image is processed;
[0024] (5) Using image processing software, calculate the perimeter L of the mineral powder edge and the total length l of the shrinkage cracks within the edge. Figure 2 This is the state of cracks after the image processing of the mineral powder saturated with water and dried;
[0025] (6) Calculate the shrinkage cracking degree S of the mineral powder saturated water-drying method using formula 1 k ;
[0026]
[0027] Where: S k - Mineral powder shrinkage cracking degree, %; L-mineral powder edge circumference; the inner circumference of the test container can be taken as L = πR 2 , R = Φ / 2; l-total length of shrinkage cracks in the edge;
[0028] (7) Each mineral powder is tested three times and the average value is taken. The error of three parallel test pieces cannot be greater than 10%;
[0029] (8) Through the mineral powder plasticity index IP and shrinkage cracking degree S k The relationship between the plasticity index and the S that meets the technical requirements can be determined. k The value is used as the technical standard for the shrinkage cracking degree of mineral powder using the saturated-dried method.
[0030] The beneficial effects of the present invention relative to the prior art are:
[0031] (1) To provide a simple quality evaluation method for the selection of mineral powder for asphalt mixture;
[0032] (2) The use of relative quantitative indicators makes the quality evaluation of mineral powder more objective and accurate.
[0033] (3) This method is simple and convenient, does not require complex instruments and tedious operations, and can quickly determine the test results within 24 hours.
[0034] (4) It can form a unified standard to provide guidance for the preliminary selection of mineral powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1This is the structural dimension drawing of the test vessel;
[0036] Figure 2 It is a schematic diagram of mineral powder;
[0037] Figure 3 This is a picture of the mineral powder saturation test process;
[0038] Figure 4 This is a picture of the surface crack state of 200 mesh mineral powder after saturation and drying;
[0039] Figure 5 This is a picture of the surface crack state of 400 mesh mineral powder after saturation and drying;
[0040] Figure 6 This is a picture of the surface crack state of 600 mesh mineral powder after saturation and drying;
[0041] Figure 7 This is a picture of the surface crack state of 800 mesh mineral powder after saturated water and drying;
[0042] Figure 8 This is a picture of the surface crack state of 1250 mesh mineral powder after saturated water and drying;
[0043] Fig. 9 These are the crack state diagrams before and after the mineral powder crack image processing. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and implementation cases, but is not limited thereto. Any modification or equivalent substitution of the technical solution of the present invention that does not depart from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0045] Embodiment 1:
[0046] 1. Mineral powder saturation test
[0047] Weigh 300g of dry mineral powder, put it into the specified container, add 500g of pure water, stir it thoroughly with a glass rod, place the container on a horizontal platform, and let the mixture of mineral powder and water settle for 30 minutes. The mineral powder after precipitation should be kept with uniform thickness. Figure 2 and 3 This is a picture of the mineral powder saturation test process.
[0048] 2. Mineral powder drying test
[0049] Preheat the oven to 105℃, carefully place the container containing the mineral powder in the oven, and keep the container in a horizontal state in the oven bracket. Dry for 12 hours to allow the mineral powder to shrink freely during the dehydration process. After drying, take out the container and place it in a room temperature environment to cool to room temperature.
[0050] 3. Data collection
[0051] Place the cooled container horizontally and take a photo of the surface of the mineral powder with a mobile phone. When taking photos, try to keep the image height the same and the phone level. Figures 4 to 8 Take pictures of mineral powders of different finenesses with your mobile phone.
[0052] 4. Data processing
[0053] Import the crack distribution picture of the saturated and dried mineral powder into the computer, use the corresponding software to process the image, and calculate the edge perimeter L of the mineral powder and the total crack length l. Fig. 9 The crack images of mineral powder before and after treatment are shown in Figure 1. The shrinkage crack degree S of mineral powder is calculated using formula 1. k .
[0054]
[0055] Where: S k - Mineral powder shrinkage cracking degree, %; L-mineral powder edge circumference. The inner circumference of the test container can be taken as L = πR 2 , R = Φ / 2; l-total length of shrinkage cracks within the edge.
[0056] 5. Plasticity index estimation
[0057] The shrinkage cracking degree S of the mineral powder calculated by formula 1 k , substitute the regression formula 2 of plasticity index IP and shrinkage cracking degree to estimate the plasticity index of the tested mineral powder.
[0058] IP=1.5668S k +6.5431 (2)
[0059] Where: S k -mineral powder shrinkage cracking degree, %; IP-mineral powder plasticity index, %;
[0060] For example, the measured shrinkage cracking degree S of a certain mineral powder k =2.2, S k Substituting =2.2 into equation 2, it is calculated that the IP of the mineral powder is 9.99%, while the plasticity index determined by the T0118-2007 method is IP=9.2%, with an error of 8.6%.
Claims
1. A method for quickly estimating the plasticity index of mineral powder for asphalt mixture, Features: The method is specifically as follows: Take 300±0.5g of mineral powder, saturate it with water in a shallow dish, let it be evenly distributed with equal thickness, then put it into an oven at 105℃±5℃ to dry it, let the mineral powder shrink freely, wait for the water to evaporate and the mineral powder to dry, take out the shallow dish, take pictures of the shrinkage state of the mineral powder and process the image, use image processing software to calculate the perimeter L of the mineral powder edge and the total length l of the shrinkage cracks in the edge, and use formula 1 to calculate the shrinkage crack degree S of the mineral powder saturation-drying method k ; Where: S k -mineral powder shrinkage crack degree, %; L-mineral powder edge circumference; l-total length of shrinkage cracks within the edge.
2. A method for quickly estimating the plasticity index of mineral powder for asphalt mixture according to claim 1, Features: The method steps are: (1) Weigh 300g of mineral powder and put it into a circular ceramic or metal shallow dish with a height of 10-20mm and an inner diameter of Φ=20cm. The edge of the shallow dish should be at right angles to the bottom of the dish; (2) Weigh 500g of water and mix it evenly with the mineral powder in the container using a glass rod to make the mineral powder fully saturated with water. The water must cover all the mineral powder; (3) Place the container on a horizontal platform and allow the mixture of mineral powder and water to settle for 30 minutes. Then place the container in an oven at 105°C for at least 12 hours to ensure that the water in the container is completely evaporated. (4) After the container is taken out and cooled, the shrinkage state of the mineral powder in the container is photographed vertically and the image is processed; (5) Using image processing software, calculate the perimeter L of the mineral powder edge and the total length l of the shrinkage cracks within the edge; (6) Calculate the shrinkage cracking degree S of the mineral powder saturated water-drying method using formula 1 k ; Where: S k -mineral powder shrinkage crack degree, %; L-mineral powder edge perimeter; l-total length of shrinkage cracks in the edge; (7) Each mineral powder is tested three times and the average value is taken. The error of three parallel test pieces cannot be greater than 10%; (8) Through the mineral powder plasticity index IP and shrinkage cracking degree S k The relationship between the plasticity index and the S that meets the technical requirements is determined. k The value of .