Graphene device and preparation method thereof, photoelectric detector
By using a metal layer catalyst to grow graphene at a preset temperature in the preparation of graphene photodetectors, the transfer process of graphene is avoided, the problem of graphene damage is solved, and a high-performance graphene photodetector is achieved.
Patent Information
- Application Number
- CN202210694742.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-17
AI Technical Summary
The existing graphene photodetector preparation method is easily damaged during the transfer process of graphene, which reduces the detection performance.
Using a metal layer as a catalyst, graphene is grown on the device pattern at a preset temperature, causing the tip of the metal catalytic layer to fuse to form a graphene device, avoiding the transfer process of graphene, thus improving the performance of the device.
The graphene device prepared by this method shows good purple light absorption at the tip fuse, which improves the performance of the photodetector and is suitable for the field of photodetectors.
Smart Images

Figure CN115274889B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of photoelectric detectors, and in particular to a graphene device and a preparation method thereof, and a photoelectric detector. Background Art
[0002] Graphene can easily form Schottky junctions with other semiconductors. The carriers generated by light absorption in the semiconductor can be transferred to the graphene layer, changing its conductive properties, making it possible to prepare graphene-based photodetectors. In addition, graphene also has the characteristics of zero band gap and high carrier mobility, and can absorb light in a fairly wide spectral wavelength range. Therefore, it is an ideal photoelectric device material and can be used to prepare photodetectors with high responsiveness, wide absorption spectrum, and high sensitivity. Graphene-like carbon films are similar to graphene structures, both of which are sp 2 The structure not only has the excellent properties of graphene, but also has a loose and porous structure with a large specific surface area, and has great potential in the application field of sensor devices.
[0003] However, in the existing method of preparing graphene photodetectors, graphene or graphene-like carbon films are usually grown in advance, and then the graphene or graphene-like carbon films are transferred to form photodetectors. During the graphene transfer process, the graphene may be damaged, thereby reducing the detection performance of the graphene photodetector. Summary of the invention
[0004] In view of the above technical problems, the present disclosure provides, on the one hand, a method for preparing a graphene device, comprising: performing photolithography on a substrate to form a device pattern, wherein the device pattern comprises a first portion pattern and a second portion pattern, and a connection between the first portion pattern and the second portion pattern is a tip shape; preparing a metal catalyst layer on the device pattern, wherein a shape of the metal catalyst layer is the same as a shape of the device pattern; under preset temperature conditions, growing graphene on the surface of the metal catalyst layer and fusing the tip of the metal catalyst layer to obtain a graphene device.
[0005] According to an embodiment of the present disclosure, a metal catalyst layer is prepared on a device pattern, specifically comprising: sputtering an aluminum metal layer, a copper metal layer, a gold metal layer, a nickel metal layer, a germanium metal layer, or a titanium metal layer on the device pattern to form a metal catalyst layer.
[0006] According to an embodiment of the present disclosure, when the metal catalyst layer is an aluminum metal layer, a plasma enhanced chemical vapor deposition method is used to grow graphene on the aluminum metal layer.
[0007] According to an embodiment of the present disclosure, when the metal catalyst layer is a copper metal layer, graphene is grown on the copper metal layer using a chemical vapor deposition method.
[0008] According to an embodiment of the present disclosure, an aluminum metal layer with a thickness of 50 nm is sputtered on the device pattern, or a copper metal layer with a thickness of 80 nm is sputtered on the device pattern.
[0009] According to an embodiment of the present disclosure, when the metal catalyst layer is an aluminum metal layer, graphene is grown on the surface of the metal catalyst layer at 625°C.
[0010] According to an embodiment of the present disclosure, when the metal catalyst layer is a copper metal layer, graphene is grown on the surface of the metal catalyst layer at 850°C.
[0011] According to an embodiment of the present disclosure, the substrate is a sapphire substrate or a silicon-based substrate.
[0012] According to an embodiment of the present disclosure, the substrate is a sapphire substrate. Before photolithography is performed on the substrate, the preparation method further includes: performing hydrophilic treatment on the sapphire substrate to enhance the wettability of the sapphire substrate with the metal catalyst layer.
[0013] According to an embodiment of the present disclosure, hydrophilic treatment of the sapphire substrate includes: hydrophilic treatment of the sapphire substrate by oxygen plasma bombardment, or hydrophilic treatment of the sapphire substrate by immersing the sapphire substrate in a mixed solution of sulfuric acid and hydrogen peroxide and heating and boiling, or hydrophilic treatment of the sapphire substrate by immersing the sapphire substrate in a hydrofluoric acid solution.
[0014] According to an embodiment of the present disclosure, a negative photoresist is used to perform photolithography on a substrate, and the negative photoresist is removed by soaking in acetone.
[0015] On the other hand, the present disclosure provides a graphene device, which is prepared by the preparation method as described above, including: a substrate; a metal catalyst layer formed on the substrate, the metal catalyst layer is broken at the middle tip; and graphene is formed on the metal catalyst layer.
[0016] Yet another aspect of the present disclosure provides a photodetector, comprising the graphene device as described above. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:
[0018] Figure 1 A flow chart of a method for preparing a graphene device according to the present disclosure is schematically shown.
[0019] Figure 2 The flowchart of the method for preparing a graphene device according to the first embodiment of the present disclosure is schematically shown.
[0020] Figure 3The device cross-sectional structure diagram corresponding to each operation of the graphene device preparation method according to the first embodiment of the present disclosure is schematically shown.
[0021] Figure 4 The structure diagram of a device pattern according to an embodiment of the present disclosure is schematically shown.
[0022] Figure 5 A flow chart of a method for preparing a graphene device according to a second embodiment of the present disclosure is schematically shown.
[0023] Figure 6 A flow chart of a method for preparing a graphene device according to a third embodiment of the present disclosure is schematically shown.
[0024] Figure 7 The structure of a graphene device according to an embodiment of the present disclosure is schematically shown.
[0025] Figure 8 The diagram schematically shows a current-versus-time (IT) curve after the growth of an aluminum device on a sapphire substrate according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.
[0027] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0028] In the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.
[0029] In the description of the present disclosure, it is necessary to understand that the terms "longitudinal", "length", "circumferential", "front", "rear", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the subsystem or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present disclosure.
[0030] Throughout the drawings, the same elements are represented by the same or similar reference numerals. Conventional structures or configurations will be omitted when they may cause confusion in the understanding of the present disclosure. The shapes, sizes, and positional relationships of the components in the drawings do not reflect the actual size, proportion, and actual positional relationship. In addition, in the present disclosure, any reference symbol between brackets should not be constructed as a limitation to the present disclosure.
[0031] Similarly, in order to simplify the present disclosure and help understand one or more of the various disclosed aspects, in the above description of the exemplary embodiments of the present disclosure, the various features of the present disclosure are sometimes grouped together into a single embodiment, figure, or description thereof. The description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" and the like means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0032] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the feature. In the description of the present disclosure, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0033] In view of the shortcomings of the prior art, the embodiments of the present disclosure provide a method for preparing a type of heating self-fusing graphene device with a special tip structure by using a metal layer as a catalyst, which forms a simple violet light detector after growing at a certain temperature. The graphene device prepared by the preparation method exhibits good violet light absorption at the tip fuse port and can be applied to the field of photoelectric detectors.
[0034] Figure 1 A flow chart of a method for preparing a graphene device according to the present disclosure is schematically shown.
[0035] like Figure 1 As shown, the method for preparing the graphene device may include, for example, operations S101 to S103.
[0036] In operation S101 , photolithography is performed on a substrate to form a device pattern, wherein the device pattern includes a first portion pattern and a second portion pattern, and a connection between the first portion pattern and the second portion pattern is in a tip shape.
[0037] In operation S102, a metal catalyst layer is formed on the device pattern, wherein a shape of the metal catalyst layer is the same as a shape of the device pattern.
[0038] In the embodiment of the present disclosure, the metal catalyst layer may include an aluminum metal layer, a copper metal layer, a gold metal layer, a nickel metal layer, a germanium metal layer, a titanium metal layer, or an alloy consisting of at least two of aluminum, copper, gold, nickel, germanium, and titanium.
[0039] In operation S103, graphene is grown on the surface of the metal catalyst layer under a preset temperature condition, and the tip of the metal catalyst layer is melted to obtain a graphene device.
[0040] According to the preparation method provided by the embodiment of the present disclosure, a device pattern with a pointed shape is photoetched on a substrate, and a metal catalyst layer with the same shape is sputtered according to the device pattern, so that after graphene is grown at a preset temperature, the tip of the metal catalyst layer breaks at the preset temperature to form an electrode of the device. Graphene and the electrode are obtained simultaneously in a one-step method, and then a graphene device is obtained. There is no need for a graphene transfer process, which ensures the quality of the graphene carbon film and improves the performance of the graphene device.
[0041] The following is combined with other figures Figure 1 The preparation method shown is further described.
[0042] Figure 2 The flowchart of the method for preparing a graphene device according to the first embodiment of the present disclosure is schematically shown. Figure 3 The device cross-sectional structure diagram corresponding to each operation of the graphene device preparation method according to the first embodiment of the present disclosure is schematically shown.
[0043] like Figure 2 and Figure 3 As shown, the preparation method may include, for example, operations S201 to S205.
[0044] In operation S201 , a sapphire substrate is subjected to a hydrophilic treatment.
[0045] In this embodiment, since the wettability of the sapphire substrate (mainly composed of Al2O3) with metal is poor, the sapphire substrate needs to be hydrophilized before photolithography. The sapphire substrate can be hydrophilized by oxygen plasma bombardment, or by soaking the sapphire substrate in a mixed solution of sulfuric acid and hydrogen peroxide and heating and boiling it, or by soaking the sapphire substrate in a hydrofluoric acid solution. The structure of the device obtained in operation S201 is as follows: Figure 3 shown.
[0046] For example, the surface of the sapphire substrate is treated to be hydrophilic by immersing and heating in a mixed solution of sulfuric acid (H2SO4) and hydrogen peroxide (H2O2). Specifically, the sapphire substrate is placed in a mixture of hydrogen peroxide and sulfuric acid, heated and boiled at high temperature (~200°C) for about 2 hours, then cooled naturally, the wafer is taken out and cleaned, and a sapphire substrate with good hydrophilicity is obtained after acid treatment, which is conducive to the adhesion of metals.
[0047] In operation S202 , photolithography is performed on the hydrophilic treated sapphire substrate to form a device pattern.
[0048] In this embodiment, a negative photoresist can be used to perform photolithography on the substrate. For example, the model of the negative photoresist can be AR-N 4340, and the rotation speed during coating can be 4000 r. The thickness of the photoresist formed at this rotation speed is about 1.68 um. Then, the substrate can be pre-baked at 110°C for 120 s, the exposure time can be 15 s, and the exposure power can be 8.2 mW / cm 2 ; Then post-bake, the post-bake temperature can be 100 ℃, and the time can be 80 s. Finally, develop, the developer is AR300-475 (ratio is KMPPD238-II: water = 5:2), and the development time is about 90 s. When using the mask in photolithography, pay attention to distinguishing its front and back sides, and pay attention to light shielding during the removal and use of the photoresist. After the photolithography is completed, the photoresist is removed by soaking in acetone and using the principle of mutual solubility of organic solvents and organic matter, and finally a patterned device on a sapphire substrate is obtained.
[0049] Figure 4 The structure diagram of a device pattern according to an embodiment of the present disclosure is schematically shown.
[0050] like Figure 4As shown, the first part pattern and the second part pattern of the device pattern can be symmetrical structures. For example, each part pattern can be composed of a rectangular pattern and a triangular pattern, and the triangular patterns of the two parts of the pattern are relatively connected to form a tip shape, and the rectangular pattern is located on the outside. For another example, each part pattern can be composed of a triangular pattern, and the triangular patterns of the two parts of the pattern are relatively connected to form a tip shape. The specific pattern can be determined according to the actual application, and the present disclosure does not limit it. It only needs to ensure that the connection between the first part pattern and the second part pattern of the device pattern is a tip structure. In general, the size of the tip shape does not exceed 3 nm.
[0051] In operation S203, an aluminum metal layer is prepared on the device pattern to form a metal catalyst layer, wherein the shape of the metal catalyst layer is the same as that of the device pattern.
[0052] In this embodiment, the thickness of the sputtered aluminum metal layer can be, for example, 50 nm. The shape of the aluminum metal layer can be the same as the device pattern, which can be composed of a rectangular pattern and a triangular pattern, the triangular patterns of the two parts of the pattern are relatively connected to form a tip shape, and the rectangular pattern is located on the outside. It can also be composed of a triangular pattern, the triangular patterns of the two parts of the pattern are relatively connected to form a tip shape. The structure of the device obtained in operation S203 is as follows Figure 3 shown.
[0053] In operation S204 , graphene is grown on the surface of the aluminum metal layer at a preset temperature.
[0054] In this embodiment, since aluminum metal has no catalytic effect on the growth of graphene, and the melting point of metal aluminum is about 660°C, indicating that the temperature at which the tip fuses is less than or equal to 660°C, a plasma enhanced chemical vapor deposition (PECVD) method can be used to grow graphene on the aluminum metal layer. For example, graphene can be grown on the surface of the metal catalyst layer at 625°C. The structure of the device obtained in operation S204 is as follows: Figure 3 shown.
[0055] In operation S205 , the preset temperature is maintained to fuse the tip of the aluminum metal layer to obtain a graphene device.
[0056] In this embodiment, the structure of the device obtained in operation S205 is as follows: Figure 3 shown.
[0057] Figure 5 A flow chart of a method for preparing a graphene device according to a second embodiment of the present disclosure is schematically shown.
[0058] like Figure 5 As shown, the preparation method is Figure 2The preparation method shown differs in that: Figure 5 The metal catalyst layer used in the preparation method shown is a copper metal catalyst layer, and for example, the method may include operations S501 to S505.
[0059] In operation S501, a sapphire substrate is subjected to a hydrophilic treatment.
[0060] In operation S502 , photolithography is performed on the hydrophilic treated sapphire substrate to form a device pattern.
[0061] In operation S503 , a copper metal layer is prepared on the device pattern to form a metal catalyst layer, wherein the shape of the metal catalyst layer is the same as that of the device pattern.
[0062] In operation S504 , graphene is grown on the surface of the copper metal layer at a preset temperature.
[0063] In this embodiment, since copper is catalytic for the growth of graphene, the melting point of metal copper is 1083°C, which means that the temperature at which the tip melts is less than or equal to 1083°C. Therefore, graphene can be grown on the copper metal layer by chemical vapor deposition (CVD). For example, graphene can be grown on the surface of the copper metal layer at 850°C.
[0064] In operation S505 , the preset temperature is maintained to fuse the tip of the copper metal layer, thereby obtaining a graphene device.
[0065] It should be noted that Figure 5 The implementation details of operations S501 to S503 and S505 in the preparation method shown in FIG. Figure 2 Similar, for details not shown, see Figure 2 The example part of the preparation method shown will not be repeated here.
[0066] Figure 6 A flow chart of a method for preparing a graphene device according to a third embodiment of the present disclosure is schematically shown.
[0067] like Figure 6 As shown, Figure 6 The preparation method shown is Figure 2 or Figure 5 The preparation method shown differs in that: Figure 6 The manufacturing method shown uses a silicon-based substrate and may include, for example, operations S601 to S604.
[0068] In operation S601 , photolithography is performed on a silicon-based substrate to form a device pattern.
[0069] In this embodiment, since the silicon-based substrate has good adhesion to the metal layer, hydrophilic treatment is usually not required. Therefore, the silicon-based substrate can be directly photolithographically processed to obtain a device pattern.
[0070] In operation S602 , a metal catalyst layer is formed on the device pattern, wherein a shape of the metal catalyst layer is the same as a shape of the device pattern.
[0071] In this embodiment, the metal catalyst layer may be, for example, a copper metal layer or an aluminum metal layer.
[0072] In operation S603 , graphene is grown on the surface of the metal catalyst layer at a preset temperature.
[0073] In operation S604, the preset temperature is maintained to cause the tip of the metal catalyst layer to fuse, thereby obtaining a graphene device.
[0074] It should be noted that Figure 6 The implementation details of operations S601 to S604 in the preparation method shown are similar to those of Figure 2 or Figure 5 The corresponding parts are similar, please refer to the Figure 2 or Figure 5 The example part of the preparation method shown will not be repeated here.
[0075] Based on the same inventive concept, an embodiment of the present disclosure also provides a graphene device prepared based on the above preparation method.
[0076] Figure 7 The structure of a graphene device according to an embodiment of the present disclosure is schematically shown.
[0077] like Figure 7 As shown, it includes: a substrate; a metal catalyst layer formed on the substrate, the metal catalyst layer is broken at the middle tip; and graphene is formed on the metal catalyst layer.
[0078] Based on the same inventive concept, an embodiment of the present disclosure also provides a photodetector, including the graphene device as described above.
[0079] It should be noted that the specific implementation details of the graphene device and photodetector provided in the embodiments of the present disclosure are similar to those in the preparation method section. Please refer to the preparation method embodiment section for details, and no further details will be given here.
[0080] In order to verify the advantages of the graphene device and its preparation method, and the photodetector provided by the embodiments of the present disclosure, the ultraviolet light conductivity of the prepared graphene device was tested in the embodiments of the present disclosure.
[0081] Firstly, the ultraviolet light conductivity of the graphene device obtained by growing graphene by PECVD method at 625 °C on a 50 nm aluminum metal layer with sapphire as substrate was tested.
[0082] Figure 8 The diagram schematically shows a current-versus-time (IT) curve after the growth of an aluminum device on a sapphire substrate according to an embodiment of the present disclosure.
[0083] like Figure 8 As shown, in this embodiment, 405 nm purple light is applied to the graphene device, and the IT curve is tested at a fixed voltage of 5 V. The test results show that the current of the graphene device is about 5 nA in the initial state. When 405 nm purple light is applied, the device current increases by about 2 nA, indicating that after the PECVD growth at 625 ° C, graphene material is generated on the metal layer. After the material absorbs the purple light, the current increases, and the device has a weak photoelectric effect.
[0084] Then, the ultraviolet light conductivity of the graphene device obtained by growing graphene by CVD method at 850°C on a 80 nm copper metal layer with sapphire as the substrate was tested.
[0085] In this embodiment, 405 nm purple light is applied to the graphene device, and the IT curve is tested at a fixed voltage of 5 V. The test results show that it can be seen from the IT curve that the grown graphene has a certain absorption of 405 nm purple light, the initial state current is 0.75 uA, and the current increases by about 0.5 uA after applying 405 nm purple light. Compared with the aluminum device, the copper device absorbs the same intensity of purple light and the current increase is more obvious, indicating that the graphene grown at the tip of the copper device is of better quality and has a stronger current gain effect after absorbing purple light. This is also related to the catalytic property of copper. Obviously, catalytic metals are more conducive to the growth of graphene materials. And from the IV curve of the device, it can be seen that the current changes nonlinearly with the increase of voltage, that is, the device composed of the grown graphene material and copper metal exhibits semiconductor characteristics.
[0086] Finally, the ultraviolet light conductivity of the graphene device obtained by growing graphene by CVD method at 850 °C on a 80 nm copper metal layer with a silicon substrate was tested.
[0087] Based on the current-voltage (IV) curve of the copper device grown on the silicon-based substrate of the embodiment of the present disclosure, it can be seen that the current shows a nonlinear change with the increase of voltage, that is, the device composed of the graphene-like carbon film material and copper metal after growth shows semiconductor characteristics. In addition, the tip of the copper device was not melted after growth at 850°C on the silicon-based substrate. Testing its IV curve shows that its current increases linearly with the increase of voltage, showing conductor characteristics.
[0088] Based on the above experimental tests, it can also be seen that by designing a device pattern with an extreme structure and completing the preparation method of electrodes and graphene in one step based on the device pattern, the device exhibits good ultraviolet light absorption after the tip is fused, that is, the preparation method can obtain a graphene device with excellent photoelectric properties.
[0089] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.
Claims
1. A method for preparing a graphene device, characterized in that: include: Performing photolithography on the substrate to form a device pattern, wherein the device pattern includes a first portion pattern and a second portion pattern, and a connection between the first portion pattern and the second portion pattern is in a pointed shape; Preparing a metal catalyst layer on the device pattern, wherein the shape of the metal catalyst layer is the same as the shape of the device pattern; Under a preset temperature condition, graphene is grown on the surface of the metal catalyst layer, and the tip of the metal catalyst layer is melted to obtain a graphene device; The step of preparing a metal catalyst layer on the device pattern specifically comprises: sputtering an aluminum metal layer, a copper metal layer, a gold metal layer, a nickel metal layer, or a titanium metal layer on the device pattern to form the metal catalyst layer; When the metal catalyst layer is the aluminum metal layer, the graphene is grown on the aluminum metal layer using plasma enhanced chemical vapor deposition; when the metal catalyst layer is the copper metal layer, the graphene is grown on the copper metal layer using chemical vapor deposition.
2. The preparation method according to claim 1, characterized in that: An aluminum metal layer with a thickness of 50 nm is sputtered on the device pattern, or a copper metal layer with a thickness of 80 nm is sputtered on the device pattern.
3. The preparation method according to claim 1, characterized in that: When the metal catalyst layer is the aluminum metal layer, growing graphene on the surface of the metal catalyst layer at 625° C.; When the metal catalyst layer is the copper metal layer, graphene is grown on the surface of the metal catalyst layer at 850°C.
4. The preparation method according to claim 1, characterized in that: The substrate is a sapphire substrate or a silicon-based substrate. Before photolithography is performed on the substrate, the preparation method further comprises: The sapphire substrate is subjected to a hydrophilic treatment to enhance the wettability of the sapphire substrate and the metal catalyst layer.
5. The preparation method according to claim 4, characterized in that: The hydrophilic treatment of the sapphire substrate comprises: The sapphire substrate is subjected to hydrophilic treatment by oxygen plasma bombardment, or the sapphire substrate is subjected to hydrophilic treatment by soaking in a mixed solution of sulfuric acid and hydrogen peroxide and heating and boiling, or the sapphire substrate is subjected to hydrophilic treatment by soaking in a hydrofluoric acid solution.
6. The preparation method according to claim 1, characterized in that: The substrate is photolithographically processed by using a photoresist negative resist, and the photoresist negative resist is removed by soaking in acetone.
7. A graphene device, characterized in that: The method according to any one of claims 1 to 6 is used for preparation, comprising: substrate; A metal catalyst layer is formed on the substrate, and the metal catalyst layer is broken at the middle tip; Graphene is formed on the metal catalyst layer.
8. A photoelectric detector, characterized in that: Comprising the graphene device as claimed in claim 7.