Silicone-free thermal interface materials with reactive diluents
The silicone-free thermal interface material is formed through a two-component reactive diluent system, which solves the problem of the hardness and brittleness of thermal interface materials changing with time in the existing technology, and realizes a silicone-free thermal interface material with low hardness, high thermal conductivity and stable performance. Thermal interface materials.
Patent Information
- Application Number
- CN202080088149.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-17
AI Technical Summary
Existing thermal interface materials increase in hardness and brittleness over time after curing, and diluent migration causes changes in mechanical, electrical and thermal properties, making them difficult to dispense and maintain low viscosity through standard liquid dispensing systems.
A two-component reactive diluent system is used to deliver silicone-free thermal interface materials through liquid dispensing equipment. The reactive diluent does not participate in cross-linking after curing, forming a thermally conductive coating with low hardness and high thermal conductivity that remains stable for a long time. Internally stable hardness.
It achieves low hardness and high thermal conductivity of silicone-free thermal interface materials, maintains good physical conformability and stable hardness, and avoids performance changes caused by diluent migration.
Smart Images

Figure CN115279825B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates generally to thermal interface materials and, more particularly, to a silicone-free, two-component liquid dispensable system that cures in situ to a thermally conductive coating that is physically flexible over an extended period of time. Background Art
[0002] Thermally conductive materials are widely used as interfaces between, for example, heat-generating electronic components and heat sinks to allow excess thermal energy to be transferred from the electronic components to the thermally coupled heat sink. A variety of designs and materials for such thermal interfaces have been implemented, with the highest performance being achieved when gaps between the thermal interface and the corresponding heat transfer surface are substantially avoided to promote conductive heat transfer from the electronic component to the heat sink. Therefore, the thermal interface material preferably mechanically conforms to the slightly uneven heat transfer surface of the corresponding component. Therefore, an important physical property of a high-performance thermal interface material is flexibility and relatively low hardness.
[0003] Some exemplary conformable thermal interface materials include silicone polymers that form a matrix filled with thermally conductive particles such as aluminum oxide and boron nitride. Regardless of room temperature and / or elevated temperature, the material is generally flexible enough to conform to the irregularities of the interface surface. However, silicone-based materials may be incompatible in certain applications, such as when the outgassing of silicone-based materials may not be permitted. Alternative non-silicone polymer systems have the disadvantage of limiting their use in thermal interface applications. Some conventional non-silicone systems that exhibit acceptable hardness values also exhibit relatively high pre-curing viscosities, which present challenges to distribution and assembly. Other non-silicone systems may have suitable pre-curing viscosities for distribution and assembly and acceptable post-curing hardness, but generally require reactive diluents that may interfere with the cross-linking reaction of the polymer, or tend to migrate out of non-reactive diluents of the thermal interface material, which causes the hardness and brittleness of the thermal interface material to increase over time.
[0004] A diluent is typically a substance used as a diluent agent. For purposes of the present invention, a diluent is a material used as a viscosity and hardness modifier, particularly as a viscosity and hardness reducer. As described above, many non-silicone polymer systems that can be used for thermally conductive interfaces exhibit too high a pre-curing viscosity to be easily dispensed by a standard liquid dispensing system. Including one or more diluents in a pre-cured polymer system can help reduce the viscosity to a point that can be delivered by conventional liquid dispensing equipment. The presence of a diluent in a cross-linked polymer network can also advantageously reduce the cure hardness parameter to obtain the desired flexibility.
[0005] Conventional use of diluents to reduce the viscosity and hardness of thermally conductive cross-linked networks suffers from the migration of the diluent out of the network after cross-linking. This migration can cause problems with nearby components and also cause changes in the mechanical, electrical and thermal properties of the interface material. These problems are magnified in thermally conductive materials due to the high proportion of particulate fillers in the polymer matrix.
[0006] It is therefore an object of the present invention to provide a silicone-free thermal interface formed from a relatively low viscosity liquid dispensable composition and cured to a relatively stable durometer hardness over time. The composition may preferably include a two-component reactive diluent system that reacts to increase molecular weight but does not significantly react with the crosslinkable polymer system.
[0007] It is another object of the present invention to provide a silicone-free thermal interface formed from a two-component reactant composition that can be delivered by a liquid dispensing device and that can be cured into a relatively low durometer body whose durometer hardness remains substantially unchanged over an extended period of time.
[0008] Another object of the present invention is to provide a two-component reactive diluent that is compatible with the silicone-free polymer matrix and reacts with itself to increase the molecular weight without participating in the curing of the polymer. Summary of the invention
[0009] By the present invention, a low hardness, high thermal conductivity silicone-free thermal interface can be formed from a composition that exhibits a viscosity suitable for dispensing in the form of a liquid coating by conventional liquid dispensing equipment. The thermal interface of the present invention preferably exhibits a relatively stable post-curing durometer hardness over a long period of time. The relatively low durometer hardness promotes good physical conformity of the thermal interface to the coated substrate. In some embodiments, the coated substrate may include one or more batteries from a battery system.
[0010] The composition generally includes three main components: a non-silicone cross-linkable polymer, a thermally conductive particulate filler, and a reactive diluent. The pre-cured material exhibits a liquid dispensable viscosity and is curable to form a soft solid with high thermal conductivity. The reactive diluent allows the material to be dispensable and maintain a low viscosity, but is reactive to increase the molecular weight, thereby limiting its migration out of the cured material.
[0011] In one embodiment, the thermal interface is formed from a two-component composition comprising a first component having a first reactant with a reactive functionality of 1 or 2, wherein the first component is -1 The composition further comprises a second component having a second reactant, wherein the second reactant:
[0012] (i) having a reactive functionality of 1 or 2 in the case where the first reactant functionality is 1 or 2; and
[0013] (ii) having a reactive functionality of 3 or greater only if the first reactant has a functionality of 1.
[0014] The second component of the composition is preferably -1 The composition further comprises a non-silicone cross-linkable polymer and a thermally conductive filler. The first and second reactants can react with each other to form a thermally conductive filler having a viscosity of less than 500,000 cP at a shear rate and 20°C. -1 A product having a viscosity of at least 1,000,000 cP at a shear rate, and wherein the thermal interface exhibits a thermal conductivity of at least 1 W / m*K.
[0015] In some embodiments, each of the polymer and the thermally conductive filler is included in one or more of the first component and the second component. The first and second reactants of the first and second components can be selected from the following reactive groups: epoxy resins, amines, acrylates, thiols, polyols and isocyanates. The composition can be cured to a hardness of less than 80 Shore 00, more preferably 20-70 Shore 00.
[0016] The method for forming a thermal interface on a surface comprises providing a first component having a first reactive diluent with a viscosity less than 100 cP, a second component having a second reactive diluent with a viscosity less than 100 cP, wherein the first and second diluents react with each other to form a non-crosslinked product having a viscosity greater than 1000 centipoise. The method further comprises providing a non-silicone curable resin and a thermally conductive filler. The first and second components and the resin and the filler can be dispensed onto the surface through at least one orifice to react the first diluent with the second diluent. The method further comprises curing the resin, preferably to a hardness less than 80 Shore 00. The thermal interface may preferably exhibit a thermal conductivity of at least 1.0 W / m*K. Each of the resin and the thermally conductive filler may be included in one or more of the first and second components. The first component may be dispensed as a first liquid through the first orifice, and the second component may be dispensed as a second liquid through the second orifice.
[0017] The surface may be connected to a battery or a portion of a battery such that the battery system includes a battery and a thermal interface thermally coupled to the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a schematic diagram of a system for forming a thermal interface on a surface.
[0019] Figure 2 is a schematic diagram of a system for forming a thermal interface on a surface. DETAILED DESCRIPTION
[0020] The above-listed objects and advantages as well as other objects, features and advancements represented by the present invention will now be presented in light of the detailed embodiments described with reference to the accompanying drawings. Other embodiments and aspects of the present invention are considered to be within the grasp of those of ordinary skill in the art.
[0021] The thermally conductive interface of the present invention can be formed as a coating on a surface or on a self-supporting body for placement along a heat dissipation path, typically for removing excess heat from heat generating electronic components. The thermal interface is preferably silicone-free and filled with thermally conductive particles to achieve the desired thermal conductivity, typically at least about 1 W / m*K. The thermal interface is preferably compliant with surface roughness by exhibiting a durometer hardness of less than about 80 Shore 00.
[0022] Typically, the thermally conductive interface is a curable material formed by a composition of a first component having a first reactant, a second component having a second reactant that can react with the first reactant, a non-silicone cross-linkable polymer, and a thermally conductive particle filler. The first reactant and the second reactant are preferably diluents, which themselves have a relatively low viscosity and are used to reduce the viscosity of the entire pre-cured composition so that the composition can be readable and dispensed by a liquid dispensing device. Therefore, the first and second reactive diluents can each exhibit a viscosity of less than 500cP. In another embodiment, the first and second reactive diluents can each exhibit a viscosity of less than 100cP. In an exemplary embodiment, the first and second reactive diluents each exhibit a viscosity of about 20cP. The quantitative viscosity values described herein are considered to be at room temperature (20°C) and 1s -1 The shear rate was obtained on a parallel plate rheometer.
[0023] The first and second diluents preferably react with each other to form a non-crosslinked product with a viscosity greater than 1000 cP. In some embodiments, the first and second diluent reactants may react with each other to form a product with a viscosity of at least 10,000 cP. By reacting with each other, the first and second reactive diluents may react to form a diluent product with an increased molecular weight, which is less likely to migrate from the thermal interface than conventional diluent materials. As a result, the diluent product formed by the reaction of the first and second reactive diluents can continue to act as a hardness modifier for the thermal interface over a long period of time. However, this increase in molecular weight occurs only when the first and second reactive diluents react, and the reaction between the first and second reactive diluents can occur when the first and second components of the composition forming the thermal interface are mixed after the liquid is distributed.
[0024] One aspect of the present invention is that the reactive diluent does not participate in the polymer cross-linking reaction. In addition, the diluent reaction itself is not cross-linked, whereby the molecular weight of the diluent product is limited to the extent that the diluent product maintains hardness reduction properties for the entire thermal interface. Therefore, the first and second reactive diluents are selected to react with each other, but do not undergo a cross-linking reaction. Therefore, the first and second reactive diluents can be selected to form only non-cross-linked products. For the purposes of this article, the term "non-cross-linked" refers to no reactant molecule connected to more than two other reactant molecules, unless the other reactant molecules are only connected to a single reactant molecule. Exemplary non-cross-linked diluent products are as follows:
[0025] (1)y–x–y
[0026] (2)–(–x–y–x–y–x–)–
[0027] (3)
[0028] in:
[0029] x = first reactive diluent,
[0030] y = second reactive diluent.
[0031] In order to control the reactivity of the first and second reactive diluents, the "functionality" of the reactive diluents should be considered. The term functionality refers to the number of polymerizable groups in the reactants, which affects the formation and degree of crosslinking of the polymer. Monofunctional molecules have a functionality (f) = 1, difunctional molecules have a functionality (f) = 2, and trifunctional molecules have a functionality (f) = 3. In the case of functionality (f = 2), linear reaction products can be formed. Reactants with a functionality (f ≥ 3) can produce branching points and crosslinked products. Monofunctional reactants (f = 1) result in chain termination. The following are exemplary diluent reaction products of diluent reactants having the stated functionalities:
[0032] x 1 –y 1
[0033] x 1 –y 2 –x 2 –y 2 –x 2 –y 1
[0034]
[0035] in:
[0036] x = first reactive diluent,
[0037] y = second reactive diluent,
[0038] x 1 For f = 1,
[0039] x 2 f = 2,
[0040] x 3 f=3.
[0041] In some embodiments, the first reactant has a reactive functionality of 1 or 2, and the second reactant:
[0042] (i) having a reactive functionality of 1 or 2 in the case where the first reactant functionality is 1 or 2; and
[0043] (ii) having a reactive functionality of 3 or greater only if the first reactant has a functionality of 1.
[0044] Under this functionality restriction, the first and second reactants are reactive to form only non-crosslinked products. By preventing crosslinking of the first and second reactants, the diluent reaction product is able to soften the thermal interface material despite having a larger molecular weight.
[0045] The first and second reactive diluents can be added to the composition in an amount suitable for appropriately adjusting viscosity to obtain pre-curing dispensability and post-curing flexibility. In some embodiments, the reactive diluent can account for about 5-50% by weight of the composition. The exemplary reactive diluent system representing the first and second reactive diluents includes epoxy resin / amine, amine / acrylate, acrylate / acrylate plus catalyst, mercaptan / acrylate, polyol / isocyanate, and amine / isocyanate. It is expected that those of ordinary skill in the art can select the reactive group of suitable diluent from one or more of epoxy resin, amine, acrylate, mercaptan, polyol and isocyanate.
[0046] The composition for forming the thermal interface of the present invention preferably includes a non-silicone curable resin, which forms the bulk matrix of the thermal interface. In some embodiments, the composition may include a non-silicone crosslinkable polymer. In a preferred embodiment, the thermal interface is silicone-free, wherein no more than trace amounts of silicone are included in the thermal interface. It is expected that a variety of non-silicone crosslinkable polymers can be used in the composition of the present invention to achieve the desired physical properties. Exemplary crosslinked polymer systems include silyl-modified polymers (SMP), epoxy resins / amines, epoxy resins / anhydrides, acrylates and polyurethanes. Preferably, the crosslinked polymer is any non-silicone polymer that forms a crosslinked network without reacting with a diluent. The applicant has found that SMP materials, such as those described in U.S. Patent No. 3,632,557 and U.S. Patent Application Publication No. 2004 / 0127631 (the contents of which are incorporated herein as a whole), can be particularly used to prepare the thermally conductive interface of the present invention. It should be understood that various combinations of crosslinked polymers and reactive diluent systems can be selected for specific properties. Examples of combinations of crosslinked polymers and reactive diluents are listed in Table 1 below:
[0047] Table 1
[0048] Cross-linkable polymers Reactive diluent system Silyl-modified polymer (SMP) Epoxy resin / amine Silyl-modified polymer (SMP) Amine / Acrylate Silyl-modified polymer (SMP) Acrylate Silyl-modified polymer (SMP) Thiol / Acrylate Epoxy resin / anhydride Acrylate Epoxy resin / anhydride Polyol / isocyanate
[0049] Systems using epoxy / amine, acrylate, polyurethane or thiol / ene polymer crosslinking systems can potentially co-react with some of the diluents listed in Table 1 above, but specific combinations of molecules with appropriate catalysts and / or inhibitors are possible.
[0050] In order to improve the thermal conductivity of the thermally conductive interface, the composition of the present invention may include thermally conductive particles dispersed therein. The particles can be both thermally conductive and electrically conductive. Alternatively, the particles can be thermally conductive and electrically insulating. Exemplary thermally conductive particles include aluminum oxide, silicon oxide, aluminum trihydrate, zinc oxide, graphite, magnesium oxide, aluminum nitride, boron nitride, metal particles, and combinations thereof. The thermally conductive particles can have various shapes and sizes, and it is expected that a particle size distribution can be used to fit the parameters of any particular application. In some embodiments, the thermally conductive particles can have an average particle size of about 0.1-100 microns, and can be present in the thermally conductive material at a concentration of about 20-95% by weight.
[0051] The thermally conductive particles may be dispersed in at least one of the first and second components at a loading concentration of about 20-95% by weight. It is desirable to provide sufficient thermally conductive particles so that the thermally conductive interface formed by the component mixture exhibits a thermal conductivity of at least 1 W / m*K. In some embodiments, each of the cross-linkable polymer and the thermally conductive filler may be included in one or more of the first component and the second component.
[0052] The composition used to form the thermal interface of the present invention is preferably selected to be curable to a hardness of less than 80 Shore 00, more preferably to a hardness of 20-70 Shore 00. This durometer hardness of the cured thermal interface is driven by the combination of reactive diluent, non-silicone cross-linkable polymer and thermally conductive filler selected and the reactive concentration of each component.
[0053] Various additional components may be included in the compositions of the present invention to achieve the desired reaction rate and physical properties of the reactants and the final thermal interface. Exemplary additives include crosslinking catalysts, non-reactive diluents, solvents, antioxidants, surfactants, reaction accelerators, reaction inhibitors, stabilizers, fillers, and combinations thereof.
[0054] Figure 1 and Figure 2 A system and method for forming a thermal interface of the present invention on a surface is schematically illustrated. The system 10, 110 includes a supply 12, 112 of a first component having a first reactive diluent, and a supply 14, 114 of a second component having a second reactive diluent that reacts with the first reactive diluent. In the illustrated embodiment, a non-silicone curable resin and a thermally conductive filler are provided in one or more of the first and second component supplies 12, 112 and 14, 114. The first and second components are dispensed onto a surface 22, 122 through at least one orifice to react the first reactive diluent with the second reactive diluent. Figure 1 In the illustrated system 10, the first and second components are dispensed through a common orifice 16. Figure 2 In the illustrated system 110, the first and second components are dispensed through separate orifices 116A, 116B. The surface 22 may be the surface of the battery 20 or thermally coupled to the battery 20. After the first and second components are dispensed onto the surface 22, 122, the coating may be cured by a curing device 30, 130. Exemplary curing devices may include a heating oven, an ultraviolet (UV) radiation lamp, a photoinitiator, etc. In some embodiments, the curable resin may be cured at a temperature exceeding 25°C. Figure 1 and 2 The schematic diagram of FIG. 1 shows a conveyor 40, 140 for moving the coated battery 20, 120 to a curing station where it is exposed to a curing device 30, 130. In a preferred embodiment, the first and second components may be dispensed through at least one orifice 16, 116 in liquid form.
[0055] Example
[0056] The first embodiment thermal interface is formed from the following two-component composition:
[0057]
[0058] The first component exhibited a viscosity of 100,000 cP and the second component exhibited a viscosity of 200,000 cP, the viscosity being measured on a parallel plate rheometer at 1 s. -1 The shear rate is measured.
[0059] After mixing the first and second components, a cured solid having a durometer hardness of 50 Shore 00 and a thermal conductivity of 3.0 W / m*K was produced after 24 hours at 25°C.
[0060] A second embodiment thermal interface having the following composition was prepared:
[0061]
[0062] Upon mixing the first and second components, a cured solid having a hardness of 55 Shore 00 was obtained.
[0063] The present invention has been described in considerable detail herein in order to comply with patent law and to provide those skilled in the art with the information necessary to apply novel principles and to construct and use embodiments of the present invention as desired. However, it should be understood that various modifications may be implemented without departing from the scope of the invention itself.
Claims
1. A thermal interface formed by a two-component composition, the two-component composition comprising: A first component having a first reactant with a reactive functionality of 1 or 2, wherein the first component is -1 and exhibiting a viscosity of less than 500,000 cP at 20°C; A second component having a second reactant, wherein: (i) where the first reactant has a functionality of 1 or 2, the second reactant has a reactive functionality of 1 or 2; as well as (ii) only in the case where the first reactant has a functionality of 1, the second reactant has a reactive functionality of 3 or greater, The second component is in 1s -1 and exhibiting a viscosity of less than 500,000 cP at 20°C; Non-silicone cross-linkable polymers; and Thermally conductive fillers; The first and second reactants can react with each other to form -1 and a product having a viscosity of at least 1,000,000 cP at 20° C., and wherein the thermal interface exhibits a thermal conductivity of at least 1 W / m*K, and neither of the first and second reactants reacts with the polymer.
2. The thermal interface of claim 1, wherein each of the polymer and the thermally conductive filler is contained in one or more of the first component and the second component.
3. The thermal interface of claim 2, wherein the composition is curable to a hardness of less than 80 Shore 00.
4. The thermal interface of claim 3, wherein the composition is curable to a hardness of 20-70 Shore 00.
5. The thermal interface of claim 1 wherein the polymer cures at a temperature in excess of 25°C.
6. The thermal interface of claim 1 wherein the polymer comprises a silyl-modified polymer.
7. The thermal interface of claim 1, wherein the thermally conductive filler is selected from the group consisting of aluminum oxide, aluminum nitride, silicon oxide, zinc oxide, and boron nitride.
8. The thermal interface of claim 1, wherein the first reactant and the second reactant are selected from the following reactive group: epoxies, amines, acrylates, thiols, polyols, and isocyanates.
9. The thermal interface of claim 1 which is free of silicone.
10. A battery system comprising: Battery; and A thermal interface as claimed in claim 1 thermally coupled to the battery.
11. The battery system of claim 10, wherein the thermal interface is coated on the battery.
12. A method of forming a thermal interface on a surface, the method comprising: (a) Provide: (i) a first component of a first reactive diluent having a viscosity less than 100 cP; (ii) a second component having a second reactive diluent having a viscosity less than 100 cP, the first and second diluents reacting with each other to form a non-crosslinked product having a viscosity greater than 1000 cP; (iii) non-silicone curable resins; and (iv) a thermally conductive filler, wherein both the first and second diluents are non-reactive with the resin; (b) dispensing the first component and the second component and the resin and the filler onto the surface through at least one orifice to react the first diluent with the second diluent; and (c) curing the resin.
13. The method of claim 12, wherein the thermal interface exhibits a thermal conductivity of at least 1.0 W / m*K.
14. The method of claim 12, wherein each of the resin and the thermally conductive filler is contained in one or more of the first component and the second component.
15. The method of claim 14, comprising dispensing the first component as a first liquid through a first orifice and dispensing the second component as a second liquid through a second liquid orifice.
16. The method of claim 15, wherein the surface is connected to or is part of a battery.
17. The method of claim 12, wherein the thermal interface exhibits a hardness of less than 80 Shore 00.
18. The method of claim 12, comprising curing the resin at a temperature exceeding 25°C.
Citation Information
Patent Citations
Curable composition
US20040127631A1
Vulcanizable silicon terminated polyurethane polymers
US3632557A
Thermally conductive material
CN101121878A
Dispensable cured resin
CN101351755A
Thermally conductive composition
CN101815772A