A method for controlling the Fe2O3 content and adhesion in the oxide scale of high carbon steel wire rod

By adjusting the chemical composition and process parameters of high-carbon steel strips, the Fe2O3 content in the iron oxide sheet is improved, and the problem of poor adhesion of the iron oxide sheet after rolling is solved, and good adhesion of the iron oxide sheet of high-carbon steel strips is achieved. and coverage.

CN115283435BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210812553.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-12
Publication Date
2024-12-03
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the adhesion of the iron oxide sheet of the plate strip on the steel grades that are quickly cooled after rolling, and cannot meet the requirements of the adhesion of the iron oxide sheet of the plate strip after rolling.

Method used

By adjusting the chemical composition and process of high-carbon steel strips, including parameters such as pretreatment of liquid steel, converter smelting, continuous casting process, rolling temperature and cooling speed, the Fe2O3 content in the iron oxide strips is increased, and the iron oxide strips is promoted. Adhesion.

Benefits of technology

It effectively improves the adhesion of the iron oxide sheet of high-carbon steel coil strips, so that the coverage rate of the iron oxide sheet is no less than 90%, and meets the adhesion requirements of the fast-cooling strips after rolling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003741070140000061
    Figure BDA0003741070140000061
  • Figure BDA0003741070140000071
    Figure BDA0003741070140000071
  • Figure BDA0003741070140000081
    Figure BDA0003741070140000081
Patent Text Reader

Abstract

The present invention relates to a method for preparing a high carbon steel wire rod having an iron oxide scale containing Fe 2 O 3 The invention discloses a method for controlling the content and adhesion of the wire rod, wherein the chemical composition of the wire rod is: [C] 0.60% to 0.85%, [Si] 0.15% to 0.30%, [Mn] 0.40% to 0.55%, [S] 0.0050% to 0.015%, [P] 0.0050% to 0.020%, [Cr] 0.04% to 0.09%, [Ti] 0.0002% to 0.0015%, Als 0.0005% to 0.0020%, and the rest is Fe and impurities. The invention improves the Fe content in the wire rod oxide scale by designing the chemical composition of the wire rod and controlling the process. 2 O 3 The content effectively improves the adhesion of the oxide scale of high carbon steel wire rod.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wire rod production, and in particular to a method for controlling the Fe2O3 content and adhesion of iron oxide scale in a high-carbon steel wire rod. Background Art

[0002] High carbon steel wire rod is generally used as raw material for users to manufacture deep-processed products. It is necessary to ensure that the surface of the wire rod is completely covered with iron oxide scale after production to prevent surface rust caused by the falling of iron oxide scale. In order to ensure the integrity of the iron oxide scale on the surface of the wire rod, the thickness of the iron oxide scale needs to be controlled. In general, the thickness of the iron oxide scale is larger, and the adhesion of the iron oxide scale on the surface of the wire rod is relatively good.

[0003] The Chinese patent application with application (patent) number CN200810000916.1 discloses "a control technology for the iron scale on the surface of hot-rolled wire rods", which uses a mechanical peeling method or a mechanical peeling plus pickling and descaling method to control the iron scale on the surface of high-carbon steel hot-rolled wire rods for wire making, and controls the thickness and structure of the iron scale on the surface of the hot-rolled wire rods by controlling the Stelmor cooling process. Specific measures include closing the water tank after the final rolling and adjusting the water volume of the water tank after the final rolling to increase the spinning temperature; increasing the high-temperature oxidation time after spinning to move the phase change zone backward; increasing the air volume of the fan after the phase change of the Stelmor air cooling line to speed up the cooling speed, etc. By controlling the Stelmor cooling process, the thickness of the iron scale on the surface of the hot-rolled wire rod is effectively increased, the proportion of FeO in the iron scale is increased, and the structure of the iron scale is improved, which is convenient for the treatment of the iron scale on the surface of high-carbon steel hot-rolled wire rods for wire making that are descaled by mechanical peeling or mechanical peeling plus pickling.

[0004] However, the process of high temperature wire drawing + slow cooling after rolling + rapid cooling after phase change adopted in the above technical solution is not suitable for the control of iron scale of steel grades that require rapid cooling after rolling. In order to meet the requirements of the adhesion of surface iron scale of the wire rod after rapid cooling after rolling, a new rolling process needs to be developed to improve the adhesion of the iron scale of the wire rod. Summary of the invention

[0005] The present invention provides a method for controlling the Fe2O3 content in the oxide scale of a high carbon steel wire rod and its adhesion. The Fe2O3 content in the oxide scale of the wire rod is increased through the chemical composition design of the wire rod and the process control, and the adhesion of the oxide scale of the high carbon steel wire rod is effectively improved.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for controlling the Fe2O3 content and adhesion in the oxide scale of a high-carbon steel wire rod, wherein the chemical composition of the high-carbon steel wire rod is as follows by mass percentage: [C] 0.60% to 0.85%, [Si] 0.15% to 0.30%, [Mn] 0.40% to 0.55%, [S] 0.0050% to 0.015%, [P] 0.0050% to 0.020%, [Cr] 0.04% to 0.09%, [Ti] 0.0002% to 0.0015%, Als 0.0005% to 0.0020%, and the remainder is Fe and unavoidable impurities; the control method comprises the following steps:

[0008] 1) The molten steel undergoes a process of molten iron pretreatment, converter smelting, LF refining production, and continuous casting to obtain a continuous casting billet;

[0009] 2) The total heating time of the continuous casting billet during continuous rolling is 3.5-4.5h, the soaking section temperature is controlled at 1250-1290℃, and the soaking section time is controlled at 50-60min; the continuous casting billet is heated and rolled into a continuous rolling billet, the final rolling temperature is 930-950℃, and the thickness of the decarburized layer on the surface of the continuous rolling billet is controlled at 0.6-1.1mm; the continuous rolling billet is partially ground before rolling the wire rod, and the ratio of defect length to depth after grinding is ≥3;

[0010] 3) The total time in the furnace for continuous rolling billet heating is 2.5 to 3 hours, the soaking section temperature is 1100 to 1160°C, and the soaking time is 30 to 40 minutes;

[0011] 4) After the continuous rolling billet leaves the heating furnace, high-pressure water descaling is performed;

[0012] 5) The rolling temperature of the rolled piece when it leaves the rolling mill is 840-860°C, the rolling speed is 3-4 m / s, the area reduction rate is 15%-20%, and the deformation rate is 6-9s -1 ;

[0013] 6) The rolling temperature of the rolled piece when it leaves the pre-finishing rolling mill is 940-980°C, the rolling speed is 10-12 m / s, the area reduction rate is 17%-20%, and the deformation rate is 60-65s -1 ; The rolled pieces after leaving the pre-finishing mill are water-cooled, and the cooling water pressure is 2.0~4.0bar;

[0014] 7) The rolling temperature of the rolled piece when it leaves the finishing mill is 950-980°C, the rolling speed is 100-110 m / s, the area reduction rate is 17%-22%, and the deformation rate is 750-800s -1 ; The rolled piece after finishing rolling is water cooled, and the cooling water pressure is 3.0~4.0bar;

[0015] 8) The rolling temperature of the rolled piece when it leaves the double module rolling mill is 890-930°C, the rolling speed is 100-110 m / s, the area reduction rate is 3%-6%, and the deformation rate is 580-620s -1 ; The rolled pieces after exiting the double module are water cooled, and the cooling water pressure is 3.0-4.0 bar;

[0016] 9) The wire rod spinning temperature is 900-940°C. After the wire rod is spun, it is cooled on an air-cooled roller. The cooling rate is controlled at 20-28°C / s. The wire rod coiling temperature is controlled at 510-540°C.

[0017] The specifications of the continuous casting billet are 250-300mm×350-400mm; the wire rod is rolled from the continuous rolling billet of 150-170mm×150-170mm.

[0018] The descaling pressure during the high-pressure water descaling is ≥14MPa.

[0019] The specification of the wire rod is 5.0-6.0 mm.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The primary iron oxide scale of the steel billet is removed by heating and descaling the steel billet. The surface oxidation of the rolled piece is promoted by controlling the chemical composition of the wire rod and the process parameters of the rolling process, so that the Fe2O3 content in the iron oxide scale of the high carbon steel wire rod is increased from the conventional 3% to more than 10%, and the adhesion of the iron oxide scale of the high carbon steel wire rod is improved, so that the iron oxide scale coverage rate of the wire rod (the ratio of the iron oxide scale covering the wire rod surface) is not less than 90%. DETAILED DESCRIPTION

[0022] The invention discloses a method for controlling the Fe2O3 content and the adhesion of the Fe2O3 content in the oxide scale of a high carbon steel wire rod. The chemical composition of the high carbon steel wire rod is as follows by mass percentage: [C] 0.60% to 0.85%, [Si] 0.15% to 0.30%, [Mn] 0.40% to 0.55%, [S] 0.0050% to 0.015%, [P] 0.0050% to 0.020%, [Cr] 0.04% to 0.09%, [Ti] 0.0002% to 0.0015%, Als 0.0005% to 0.0020%, and the rest is Fe and unavoidable impurities. The control method comprises the following steps:

[0023] 1) The molten steel undergoes a process of molten iron pretreatment, converter smelting, LF refining production, and continuous casting to obtain a continuous casting billet;

[0024] 2) The total heating time of the continuous casting billet during continuous rolling is 3.5-4.5h, the soaking section temperature is controlled at 1250-1290℃, and the soaking section time is controlled at 50-60min; the continuous casting billet is heated and rolled into a continuous rolling billet, the final rolling temperature is 930-950℃, and the thickness of the decarburized layer on the surface of the continuous rolling billet is controlled at 0.6-1.1mm; the continuous rolling billet is partially ground before rolling the wire rod, and the ratio of defect length to depth after grinding is ≥3;

[0025] 3) The total time in the furnace for continuous rolling billet heating is 2.5 to 3 hours, the soaking section temperature is 1100 to 1160°C, and the soaking time is 30 to 40 minutes;

[0026] 4) After the continuous rolling billet leaves the heating furnace, high-pressure water descaling is performed;

[0027] 5) The rolling temperature of the rolled piece when it leaves the rolling mill is 840-860°C, the rolling speed is 3-4 m / s, the area reduction rate is 15%-20%, and the deformation rate is 6-9s -1 ;

[0028] 6) The rolling temperature of the rolled piece when it leaves the pre-finishing rolling mill is 940-980°C, the rolling speed is 10-12 m / s, the area reduction rate is 17%-20%, and the deformation rate is 60-65s -1 ; The rolled pieces after leaving the pre-finishing mill are water-cooled, and the cooling water pressure is 2.0~4.0bar;

[0029] 7) The rolling temperature of the rolled piece when it leaves the finishing mill is 950-980°C, the rolling speed is 100-110 m / s, the area reduction rate is 17%-22%, and the deformation rate is 750-800s -1 ; The rolled piece after finishing rolling is water cooled, and the cooling water pressure is 3.0~4.0bar;

[0030] 8) The rolling temperature of the rolled piece when it leaves the double module rolling mill is 890-930°C, the rolling speed is 100-110 m / s, the area reduction rate is 3%-6%, and the deformation rate is 580-620s -1 ; The rolled pieces after exiting the double module are water cooled, and the cooling water pressure is 3.0-4.0 bar;

[0031] 9) The wire rod spinning temperature is 900-940°C. After the wire rod is spun, it is cooled on an air-cooled roller. The cooling rate is controlled at 20-28°C / s. The wire rod coiling temperature is controlled at 510-540°C.

[0032] The specifications of the continuous casting billet are 250-300mm×350-400mm; the wire rod is rolled from the continuous rolling billet of 150-170mm×150-170mm.

[0033] The descaling pressure during the high-pressure water descaling is ≥14MPa.

[0034] The specification of the wire rod is 5.0-6.0 mm.

[0035] The chemical composition design principle of the high carbon steel wire rod of the present invention is as follows:

[0036] Carbon is a chemical element that controls the strength of the wire rod. The higher the carbon content, the higher the strength of the wire rod. Too high a carbon content causes the wire rod to break during the drawing process. Therefore, the carbon content of the wire rod needs to be controlled within a certain range. The carbon content of the present invention is controlled within a range of 0.60% to 0.85%.

[0037] Silicon is the main deoxidizing element in steel and can improve the cleanliness of steel. Silicon is conducive to the formation of olivine and improves the adhesion of iron oxide scale. However, too high silicon content in steel will increase the transformation temperature of austenite to pearlite of the wire rod and reduce the drawing performance of the wire rod. Too high silicon content will also make the olivine content in the iron oxide scale of the wire rod too high, reducing the mechanical descaling performance of the iron oxide scale of the wire rod. Therefore, the silicon content of the present invention is controlled at 0.15%j~0.30%.

[0038] Manganese is also a chemical element that controls the strength of the wire rod. Manganese forms manganese olivine when the wire rod is oxidized, which can improve the adhesion of the wire rod iron oxide scale; however, if the manganese content in the wire rod is too high, the manganese olivine content in the iron oxide scale will increase, which will greatly reduce the mechanical descaling performance of the wire rod iron oxide scale. Therefore, the manganese element in the wire rod needs to be controlled at a low level while ensuring the strength requirements and adhesion. The present invention controls the manganese content to 0.40% to 0.55%.

[0039] FeS formed by sulfur and iron has a low melting point, which is conducive to accelerating the oxidation rate of the matrix on the surface of the wire rod. However, the sulfur content in the wire rod should not be too high, otherwise it will reduce the drawing and stranding performance of the wire rod. Therefore, the sulfur content in the present invention is controlled at 0.0050% to 0.015%.

[0040] The olivine is pinned on the surface of the wire rod, which will reduce the oxidation rate of the wire rod matrix. Phosphorus can reduce the melting point of olivine in the wire rod and improve the removal rate of olivine on the surface of the wire rod. However, if the phosphorus content in the steel is too high, it is easy to cause serious phosphorus segregation and reduce the drawing performance of the wire rod. Therefore, the phosphorus content in the present invention is controlled at 0.0050% to 0.020%.

[0041] Chromium improves the hardenability of wire rods, can refine the wire rod structure, and improve the drawing performance of wire rods. The oxides formed by chromium promote the probability of cracks in the oxide layer under the action of rolling force, increase the oxidation rate of the oxide layer, and increase the Fe2O3 content of the iron oxide scale. The oxides formed by chromium improve the adhesion of the iron oxide scale. However, if the chromium content is too high, the oxides formed by combining with oxygen elements adhere to the surface of the wire rod and are difficult to remove, and the content needs to be controlled; therefore, the present invention controls the chromium content to 0.04% to 0.09%.

[0042] Titanium forms fine compounds with nitrogen and oxygen in steel, which has the effect of reducing the propagation rate of micro cracks in wire rods. The oxide of titanium has the characteristic of increasing the uneven stress distribution of the oxide layer, making the oxide layer prone to cracks during the rolling process and promoting the oxidation of iron. However, too high a titanium content increases the size and number of titanium inclusions in the steel, reducing the drawing and stranding performance of the wire rod. Therefore, the titanium content of the present invention is controlled at 0.0002% to 0.0015%.

[0043] Aluminum controls the deformability of inclusions in steel and can improve the drawing and stranding properties of wire rods. Fine Al2O3 oxides in wire rods can increase the stress concentration of the oxide layer during deformation and promote the cracking of the oxide layer, thereby increasing the Fe2O3 content in the iron oxide scale. However, excessive aluminum content in steel causes large-sized Al2O3 inclusions to appear in the steel, reducing the drawing properties of the wire rod. Therefore, the aluminum content of the present invention is controlled at 0.0005% to 0.0020%.

[0044] The design principle of the method for controlling the Fe2O3 content in the oxide scale of a high carbon steel wire rod described in the present invention is as follows:

[0045] 1) The molten steel is produced by molten iron pretreatment, converter smelting, LF refining and continuous casting, and the specifications of the continuous casting billet are 250-300mm*350-400mm;

[0046] 2) The total heating time of the continuous casting billet during continuous rolling is 3.5-4.5h, the soaking section temperature is controlled at 1250-1290°C, and the soaking section time is controlled at 50-60min; the continuous casting billet is heated and rolled into a continuous rolling billet, the final rolling temperature is 930-950°C, and the thickness of the decarburization layer on the surface of the continuous rolling billet is controlled at 0.6-1.1mm, and the thicker decarburization layer is used to increase the Fe2O3 content of the iron oxide scale on the wire rod surface;

[0047] The continuous rolling billet is partially ground before rolling the wire rod. After grinding, the ratio of defect length to depth is ≥3. By controlling the length and depth ratio of the defect during billet grinding, the occurrence of wire rod surface defects can be prevented.

[0048] 3) The total furnace time for continuous rolling slab heating is 2.5-3h, the soaking section temperature is 1100-1160℃, and the soaking time is 30-40min; continuous rolling slab heating lays the foundation for wire rod rolling;

[0049] 4) After the continuous rolling billet comes out of the heating furnace, high-pressure water is used for descaling; high-pressure water descaling is used to remove the primary iron oxide scale on the surface of the continuous casting billet, laying the foundation for controlling the Fe2O3 content of the iron oxide scale on the surface of the wire rod.

[0050] 5) The rolling temperature of the rolled piece when it leaves the rolling mill is 840-860°C, the rolling speed is 3-4 m / s, the area reduction rate is 15%-20%, and the deformation rate is 6-9s -1 ;

[0051] 6) The rolling temperature of the rolled piece when it leaves the pre-finishing rolling mill is 940-980°C, the rolling speed is 10-12 m / s, the area reduction rate is 17%-20%, and the deformation rate is 60-65s -1 ; After pre-finishing rolling, the wire rod is water-cooled, and the cooling water pressure is 2.0~4.0bar.

[0052] 7) The rolling temperature of the rolled piece when it leaves the finishing mill is 950-980°C, the rolling speed is 100-110 m / s, the area reduction rate is 17%-22%, and the deformation rate is 750-800s -1 ; After finishing rolling, the wire rod is water-cooled, and the cooling water pressure is 3.0~4.0bar.

[0053] 8) The rolling temperature of the rolled piece when it leaves the double module rolling mill is 890-930°C, the rolling speed is 100-110 m / s, the area reduction rate is 3%-6%, and the deformation rate is 580-620s -1 ; After leaving the double module, the wire rod is water-cooled, and the cooling water pressure is 3.0~4.0bar.

[0054] The Fe2O3 content of the oxide scale on the surface of the wire rod finally depends on the rolling process parameters of the wire rod. The higher rolling speed and deformation rate of the wire rod are conducive to the crushing of the oxide scale on the surface of the wire rod, which intensifies the oxidation degree of the wire rod surface and promotes the increase of the Fe2O3 content in the oxide scale.

[0055] 9) The wire rod spinning temperature is 900-940°C. After the wire rod is spun, it is cooled on an air-cooled roller. The cooling rate is controlled at 10-25°C / s. The phase change wire rod coiling temperature is controlled at 510-540°C. By coiling the wire rod at a higher temperature, the Fe2O3 content of the iron oxide scale on the wire rod surface is increased.

[0056] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0057] [Example]

[0058] The specifications of the high carbon steel wire rods, production process parameters and the Fe2O3 content in the oxide scale of the high carbon steel wire rods in Examples 1-7 are shown in the following table.

[0059]

[0060]

[0061]

[0062] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for controlling the Fe2O3 content and adhesion in the oxide scale of high carbon steel wire rod, characterized in that: The chemical composition of the high carbon steel wire rod is calculated by mass percentage as follows: [C] 0.60% to 0.85%, [Si] 0.15% to 0.30%, [Mn] 0.40% to 0.55%, [S] 0.0050% to 0.015%, [P] 0.0050% to 0.020%, [Cr] 0.04% to 0.09%, [Ti] 0.0002% to 0.0015%, Als 0.0005% to 0.0020%, and the rest is Fe and unavoidable impurities; the control method comprises the following steps: 1) The molten steel undergoes a process of molten iron pretreatment, converter smelting, LF refining production, and continuous casting to obtain a continuous casting billet; 2) The total heating time of the continuous casting billet during continuous rolling is 3.5-4.5h, the soaking section temperature is controlled at 1250-1290℃, and the soaking section time is controlled at 50-60min; the continuous casting billet is heated and rolled into a continuous rolling billet, the final rolling temperature is 930-950℃, and the thickness of the decarburized layer on the surface of the continuous rolling billet is controlled at 0.6-1.1mm; the continuous rolling billet is partially ground before rolling the wire rod, and the ratio of defect length to depth after grinding is ≥3; 3) The total time in the furnace for continuous rolling billet heating is 2.5 to 3 hours, the soaking section temperature is 1100 to 1160°C, and the soaking time is 30 to 40 minutes; 4) After the continuous rolling billet leaves the heating furnace, high-pressure water descaling is carried out, and the descaling pressure is ≥14MPa; 5) The rolling temperature of the rolled piece when it leaves the rolling mill is 840-860°C, the rolling speed is 3-4m / s, the area reduction rate is 15%-20%, and the deformation rate is 6-9s -1 ; 6) The rolling temperature of the rolled piece when it leaves the pre-finishing rolling mill is 940-980°C, the rolling speed is 10-12m / s, the area reduction rate is 17%-20%, and the deformation rate is 60-65s -1 ; The rolled pieces after leaving the pre-finishing mill are water-cooled, and the cooling water pressure is 2.0~4.0bar; 7) The rolling temperature of the rolled piece when it leaves the finishing mill is 950-980°C, the rolling speed is 100-110 m / s, the area reduction rate is 17%-22%, and the deformation rate is 750-800s -1 ; The rolled pieces after finishing rolling are water cooled, and the cooling water pressure is 3.0~4.0 bar; 8) The rolling temperature of the rolled piece when it leaves the double module rolling mill is 890-930°C, the rolling speed is 100-110m / s, the area reduction rate is 3%-6%, and the deformation rate is 580-620s -1 ; The rolled pieces after exiting the double module are water cooled, and the cooling water pressure is 3.0-4.0 bar; 9) The wire rod extrusion temperature is 900-940°C. After the wire rod is extruded, it is cooled on an air-cooled roller. The cooling rate is controlled at 20-28°C / s. The wire rod coiling temperature is controlled at 510-540°C. The specification of the continuous casting billet is 250-300mm×350-400mm; the wire rod is rolled from the continuous rolling billet of 150-170mm×150-170mm; the specification of the wire rod is 5.0-6.0mm.